A layered MoTe2 / C nanoflower, preparation method and application thereof
By using 1,4-butanediol and deionized water to prepare a solution in the preparation of MoTe2 nanomaterials, and calcining and adding a tellurium source under argon hydrogen environment, the layered structure of MoTe2/C nanoflowers were successfully prepared, solving the existing technology The problem of large reaction energy consumption and single morphology has achieved low energy consumption and high electrochemical performance nanoflower materials, suitable for sodium ion battery negative electrode materials.
Patent Information
- Application Number
- CN202211105770.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-09-09
AI Technical Summary
The existing MoTe2 nanomaterials have large reaction energy consumption during the preparation process, and the product morphology is single and difficult to regulate, which limits its wide application in the chemical and electronic fields.
Molybdenum and carbon source solutions were prepared in 1,4-butanediol and deionized water, and after stirring and washing, calcining in an argon environment, then adding tellurium source under an argon hydrogen environment, controlling the calcination temperature and time, and preparing a layered layer Structure of MoTe2/C nanoflowers.
The preparation process is simplified, low energy consumption and morphological regulation. The prepared MoTe2/C nanoflowers have excellent electrochemical properties and are suitable for the negative electrode materials of sodium ion batteries, improving the embedding and removal efficiency of sodium ions.
Smart Images

Figure CN115872367B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of micro-nano materials, in particular to a layered structure MoTe2 / C nano flower, a preparation method and application thereof. Background Art
[0002] Molybdenum ditelluride (MoTe2) is an important molybdenum-based two-dimensional material. Due to its wide layered structure and excellent electronic conductivity, it has excellent catalytic properties, electrochemical properties and photothermal conversion properties. It is often used to prepare catalysts, photothermal conversion materials, electrode materials, etc. It is widely used in chemical, electronic and other fields.
[0003] At present, researchers have used vacuum evaporation, hydrothermal method and solid phase method to prepare a variety of MoTe2 materials with nanofilm, nanosheet, block and other forms. For example, Chinese patent CN201910598482.8 uses vacuum evaporation method to prepare a MoTe2 with heterojunction structure. 2-x O x / MoTe2 semiconductor material, in which MoTe2 appears in the form of a thin film. Chinese patent CN201910934298.6 uses a hydrothermal method to prepare a flaky semi-metallic MoTe2 and a flaky semi-metallic MoTe2 / RGO, and the preparation process is relatively simple. Chinese patent CN201911010608.1 uses a solid phase method to control the synthesis of three phases of MoTe2. The three phases of MoTe2 are metal / semiconductor 1T' / 2H isomorphous heterogeneous junction, metal phase 1T' and semiconductor phase 2H. The above-mentioned MoTe2 nanomaterials have high reaction energy consumption during the preparation process, the product morphology is single, and it is difficult to control. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a layered MoTe2 / C nanoflower, a preparation method and application thereof.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for preparing a layered MoTe2 / C nanoflower comprises the following steps:
[0007] 1) adding a molybdenum source to 1,4-butanediol to prepare a solution A, wherein the concentration of molybdenum ions in the solution A is 0.01 to 0.03 mol / L;
[0008] Add the carbon source into deionized water to prepare a solution B with a concentration of 0.008-0.02 mol / L;
[0009] 2) adding solution B to solution A at a volume ratio of 1:(0.3-0.8) to obtain a mixed solution, stirring the mixed solution at room temperature for 4-6 hours, and after the reaction is completed, washing and vacuum drying to obtain a precursor;
[0010] 3) Calcine the precursor at 400-500° C. for 2-3 hours in an argon environment, then add a tellurium source at a mass ratio of 1:(1-3) between the precursor and the tellurium source, and calcine in an argon-hydrogen environment to obtain a layered MoTe2 / C nanoflower.
[0011] Furthermore, in step 1), the molybdenum source is molybdenum acetylacetonate, potassium molybdate or molybdic acid.
[0012] Furthermore, in step 1), the carbon source is 2-hydroxyacetanilide, 2,4-dihydroxyphenethylamine or 4-(2-aminoethyl)-1,2-benzenediol.
[0013] Furthermore, in the step 2), washing is performed 3 to 4 times, the vacuum drying temperature is 50 to 70° C., and the drying time is 10 to 12 hours.
[0014] Furthermore, in the step 3), the tellurium source is tellurium powder.
[0015] Furthermore, in the step 3), the volume ratio of argon to hydrogen is (10-15):1, the calcination temperature is 500-700° C., and the calcination time is 5-7 hours.
[0016] A layered MoTe2 / C nanoflower is prepared according to the method of the present invention.
[0017] The hierarchical structure MoTe2 / C nanoflower of the present invention is used as a negative electrode material for a sodium ion battery.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention provides a layered MoTe2 / C nanoflower, which has a simple preparation method, a low calcination temperature, is environmentally friendly, uses common and readily available equipment, consumes low energy for preparation, and is conducive to industrial practical applications. Unlike the common MoTe2 nanomaterials, which are often prepared by solid-phase high-temperature sintering, which consumes high energy and is not conducive to industrial popularization, the present invention uses dopamine hydrochloride as a carbon source, which is low in cost and readily available, and chelates it with ammonium molybdate to regulate the morphology, and prepares a product with good electrochemical performance by changing the reaction parameters.
[0020] The layered MoTe2 / C nanoflower of the present invention has distinct morphological characteristics, an amorphous carbon layer is coated on the MoTe2 nanosheet to form a composite nanosheet, and thinner nanosheets are self-assembled into layered MoTe2 / C nanoflowers.
[0021] The hierarchical MoTe2 / C nanoflower of the present invention is used as a negative electrode material for sodium ion batteries. The two-dimensional layered structure is conducive to the embedding and extraction of sodium ions. The carbon coating can inhibit the volume expansion effect caused by the embedding and extraction of sodium ions. The layered structure can provide more active sites, shorten the sodium ion diffusion path, and further improve the transmission efficiency of ions or electrons. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the XRD pattern of the MoTe2 / C nanoflower of Example 1;
[0023] Figure 2 This is a scanning electron microscope image of the MoTe2 / C nanoflower of Example 1;
[0024] Figure 3 This is a transmission electron microscope image of the MoTe2 / C nanoflower of Example 1;
[0025] Figure 4 This is the charge and discharge diagram of MoTe2 / C nanoflowers in Example 1. DETAILED DESCRIPTION
[0026] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0027] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0028] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0029] Example 1
[0030] 1) Adding molybdenum acetylacetonate to 1,4-butanediol to prepare solution A, wherein the concentration of molybdenum ions is 0.01 mol / L;
[0031] Add 2-hydroxyacetanilide to deionized water, adding 0.008 mol of 2-hydroxyacetanilide to every 1 L of deionized water to obtain solution B;
[0032] 2) adding solution B to solution A at a volume ratio of 1:0.3 to obtain a mixed solution, and stirring the mixed solution at room temperature for 4 hours. After the reaction is completed, washing 3 times and vacuum drying at 50°C for 10 hours to obtain a precursor;
[0033] 3) The precursor was calcined at 400°C for 2 hours in an argon environment, and then tellurium powder was added in a mass ratio of 1:1, and calcined at 500°C for 5 hours in an argon-hydrogen environment with a volume ratio of argon to hydrogen of 15:1 to obtain a layered MoTe2 / C nanoflower.
[0034] See also Figure 1 , Figure 1 The XRD pattern of MoTe2 / C nanoflower prepared by the present invention is as follows: Figure 1 The phase composition of MoTe2 / C nanoflowers can be determined, and they have high purity.
[0035] See also Figure 2 , Figure 2 This is a scanning electron microscope image of the product of Example 1, in which the prepared MoTe2 / C nanomaterial has distinct morphological characteristics and is in the shape of a flower assembled by regular nanosheets, with a diameter of about 600nm and a nanosheet thickness of about 40nm.
[0036] See also Figure 3 , Figure 3 This is the transmission electron microscope image of the product. From the image, it can be seen that the carbon-coated MoTe2 two-dimensional nanosheets self-assemble into a unique hierarchical structure MoTe2 / C nanoflowers.
[0037] See also Figure 4 , Figure 4 The charge and discharge diagram of MoTe2 / C nanoflower as the negative electrode material of sodium ion battery is given. Among them, at the current density of 0.1A / g, the first discharge specific capacity and charge specific capacity are 540mAh / g and 280mAh / g respectively, and the subsequent cycle curves have good repeatability, indicating that the material not only has a high specific capacity, but also has good cycle stability.
[0038] Example 2
[0039] 1) Potassium molybdate was added to 1,4-butanediol to prepare solution A, wherein the concentration of molybdenum ions was 0.02 mol / L;
[0040] 2,4-dihydroxyphenylethylamine was added to deionized water, and 0.01 mol of 2-hydroxyacetanilide was added to 1 L of deionized water to obtain solution B;
[0041] 2) adding solution B to solution A at a volume ratio of 1:0.5 to obtain a mixed solution, and stirring the mixed solution at room temperature for 5 hours. After the reaction is completed, washing 4 times and vacuum drying at 60° C. for 11 hours to obtain a precursor;
[0042] 3) The precursor was calcined at 500°C for 3 hours in an argon environment, and then tellurium powder was added in a mass ratio of 1:2, and calcined at 600°C for 6 hours in an argon-hydrogen environment with a volume ratio of argon to hydrogen of 13:1 to obtain a layered MoTe2 / C nanoflower.
[0043] Example 3
[0044] 1) Add molybdic acid to 1,4-butanediol to prepare solution A, wherein the concentration of molybdenum ions is 0.03 mol / L;
[0045] 4-(2-aminoethyl)-1,2-benzenediol was added to deionized water, and 0.02 mol of 2-hydroxyacetanilide was added to each 1 L of deionized water to obtain solution B;
[0046] 2) adding solution B to solution A at a volume ratio of 1:0.8 to obtain a mixed solution, and stirring the mixed solution at room temperature for 6 hours. After the reaction is completed, washing 4 times and vacuum drying at 70°C for 12 hours to obtain a precursor;
[0047] 3) The precursor was calcined at 500°C for 3 hours in an argon environment, and then tellurium powder was added in a mass ratio of 1:3, and calcined at 700°C for 7 hours in an argon-hydrogen environment with a volume ratio of argon to hydrogen of 10:1 to obtain a layered MoTe2 / C nanoflower.
[0048] Example 4
[0049] 1) Adding molybdenum acetylacetonate to 1,4-butanediol to prepare solution A, wherein the concentration of molybdenum ions is 0.01 mol / L;
[0050] 4-(2-aminoethyl)-1,2-benzenediol was added to deionized water, and 0.02 mol of 2-hydroxyacetanilide was added to each 1 L of deionized water to obtain solution B;
[0051] 2) adding solution B to solution A at a volume ratio of 1:0.4 to obtain a mixed solution, and stirring the mixed solution at room temperature for 4 hours. After the reaction is completed, washing 3 times and vacuum drying at 70°C for 10 hours to obtain a precursor;
[0052] 3) The precursor was calcined at 500°C for 3 hours in an argon environment, and then tellurium powder was added in a mass ratio of 1:3, and calcined at 700°C for 5 hours in an argon-hydrogen environment with a volume ratio of argon to hydrogen of 15:1 to obtain a layered MoTe2 / C nanoflower.
[0053] The present invention utilizes cheap and readily available raw materials and simple and efficient preparation conditions to complete the preparation of MoTe2 / C nanoflowers, and obtains a unique layered structure MoTe2 / C nanoflower, which has good electrochemical performance as a negative electrode material for sodium ion batteries.
[0054] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing layered MoTe2 / C nanoflowers, characterized in that: The following steps are involved: 1) Add a molybdenum source to 1,4-butanediol to prepare solution A, wherein the concentration of molybdenum ions in solution A is 0.01-0.03 mol / L; Add the carbon source into deionized water to prepare solution B with a concentration of 0.008-0.02 mol / L; 2) adding solution B to solution A at a volume ratio of 1: (0.3-0.8) to obtain a mixed solution, stirring the mixed solution at room temperature for 4-6 hours, and after the reaction is completed, washing and vacuum drying to obtain a precursor; 3) The precursor is calcined at 400-500 °C for 2-3 hours in an argon environment, and then a tellurium source is added at a mass ratio of the precursor to the tellurium source of 1:(1-3), and calcined in an argon-hydrogen environment to obtain a layered MoTe2 / C nanoflower; In step 1), the molybdenum source is molybdenum acetylacetonate, potassium molybdate or molybdic acid; The carbon source is 2-hydroxyacetanilide, 2,4-dihydroxyphenylethylamine or 4-(2-aminoethyl)-1,2-benzenediol.
2. The method for preparing the hierarchical MoTe2 / C nanoflower according to claim 1, characterized in that: In the step 2), washing is performed 3 to 4 times, the vacuum drying temperature is 50 to 70° C., and the drying time is 10 to 12 hours.
3. The method for preparing the hierarchical MoTe2 / C nanoflower according to claim 1, characterized in that: In the step 3), the tellurium source is tellurium powder.
4. The method for preparing the hierarchical MoTe2 / C nanoflower according to claim 1, characterized in that: In the step 3), the volume ratio of argon to hydrogen is (10-15):1, the calcination temperature is 500-700°C, and the calcination time is 5-7 hours.
5. A layered MoTe2 / C nanoflower, characterized in that: Prepared according to the method according to any one of claims 1 to 4.
6. Application of the layered MoTe2 / C nanoflowers according to claim 5 as negative electrode materials for sodium ion batteries.