A carbon-coated lithium manganese iron phosphate positive electrode material and preparation method thereof
By constructing a porous structure of iron metaphosphate precursor and generating a carbon cladding layer during the thermal reduction process, the problems of insufficient reduction and low conductivity of lithium iron manganese phosphate positive electrode material are solved, and the purity and conductivity of the product are significantly improved. The preparation of a high-performance carbon-coated lithium manganese iron phosphate positive electrode material is realized.
Patent Information
- Application Number
- CN202310085648.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-01-17
AI Technical Summary
The existing lithium manganese iron phosphate positive electrode materials have uneven mixing of precursors during thermal reduction, resulting in insufficient reduction and low purity. The unmodified coating materials have low electrical conductivity and insufficient bonding strength and density, which limits performance improvement.
By pre-constructing an iron metaphosphate precursor with a porous structure, and mixing it with raw materials such as manganese source and reducing agent during the thermal reduction process, a carbon cladding layer is synchronized to penetrate into the porous structure, thereby improving binding strength and electrical conductivity.
The uniform dispersion and full reduction of the reducing agent and manganese source are achieved, the purity and conductivity of the product are improved, and the overall performance is improved, especially the discharge specific capacity at a rate of 0.1C reaches more than 155mAh/g.
Smart Images

Figure BDA0004068805800000071 
Figure HDA0004068805820000011 
Figure HDA0004068805820000012
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a carbon-coated lithium manganese iron phosphate positive electrode material and a preparation method thereof. Background Art
[0002] Compared with other batteries, lithium-ion batteries have the advantages of high output voltage and long storage life, and are widely developed and applied in many fields such as automobiles and energy storage. At present, the positive electrode materials used in lithium-ion batteries mainly include lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide, lithium iron phosphate, lithium manganese phosphate, etc. Lithium manganese phosphate and lithium iron phosphate have similar crystal structures. The combination of the two materials can take into account the advantages of both parties. Not only is it safe, but it also has high theoretical capacity, high operating voltage, and high energy density.
[0003] However, the existing lithium manganese iron phosphate is generally prepared by direct thermal reduction of trivalent iron source, composite manganese source and lithium source. These processes have the problem of uneven mixing of precursors, resulting in insufficient reduction of some raw materials in the thermal reduction stage and low purity of the final product. At the same time, the lithium manganese iron phosphate positive electrode material that has not been modified and coated still has the defect of low conductivity. Although some conventional modification processes such as carbon coating can improve the conductivity of the product to a certain extent, these coating layers often have the problems of low bonding strength and low density, and the degree of improvement in product performance is limited. Summary of the invention
[0004] Based on the defects of the prior art, the purpose of the present invention is to provide a method for preparing a carbon-coated lithium manganese iron phosphate positive electrode material, which pre-constructs a ferric ion phosphate precursor with a porous structure, and then mixes the precursor with raw materials such as a manganese source and a reducing agent for thermal reduction. This method can not only make the reducing agent and the manganese source evenly dispersed on the ferric ion phosphate precursor and achieve a sufficient reduction reaction, but also a carbon coating layer is formed synchronously during the thermal reduction process. The carbon coating layer can penetrate into the porous structure of the ferric ion phosphate precursor, has high bonding strength with the obtained lithium manganese iron phosphate positive electrode material, and has a high compaction density, so as to more evenly and effectively improve the conductivity of the overall product.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for preparing a carbon-coated lithium manganese iron phosphate positive electrode material comprises the following steps:
[0007] (1) preparing an iron source into a solution and adding it into an aqueous solution of an organic phosphoric acid and mixing it evenly, and adjusting the pH of the resulting mixed solution to 10 to 12 to obtain a reaction solution A;
[0008] (2) heating the reaction solution A to 75-85° C. and reacting for 2-5 hours, then adjusting the pH to 2-3 and aging for 1-3 hours, filtering, washing and drying the obtained solid, and heating to 400-800° C. in an air atmosphere for 4-6 hours to obtain porous iron metaphosphate B;
[0009] (3) The porous iron metaphosphate B is mixed with a manganese source, a lithium source, a reducing agent and a dispersant, and ball-milled under a protective atmosphere, and then heated to 300-400° C. for 3-5 hours, and then heated to 400-800° C. for 5-15 hours to obtain the carbon-coated manganese iron lithium phosphate positive electrode material.
[0010] In the preparation method of the carbon-coated lithium manganese iron phosphate positive electrode material of the present invention, a complex of iron and organic phosphoric acid is first prepared under mild conditions by chemical precipitation method, and the complex will generate a large amount of carbon dioxide, nitrogen dioxide and other gases during high temperature insulation, and the escape of gas will leave a loose porous structure on the surface of the generated iron metaphosphate. When the iron metaphosphate B of the porous structure is mixed with raw materials such as manganese source and reducing agent, these raw materials will be attached to the pore structure of porous iron metaphosphate B, increasing the contact area between the reducing agent and each raw material, so that the iron and manganese elements in the raw materials can be effectively and fully reduced, and it is also beneficial to improve the efficiency of lithium ions and manganese ions entering iron metaphosphate, so as to promote the generated lithium manganese iron phosphate positive electrode material composition distribution to be more uniform. On the other hand, the carbon element contained in the raw material will simultaneously generate a carbon coating layer during the thermal reduction process, and this layer of carbon coating layer will penetrate into the interior of the porous structure and combine with it due to the presence of porous iron metaphosphate B, so that the carbon coating layer is not only more bonded to the lithium manganese iron phosphate positive electrode material, but also more conductive to the degree of improvement and uniformity of its conductivity.
[0011] Preferably, in step (1), the iron source is at least one of ferric chloride, ferric sulfate, ferric nitrate and ferric acetate, and the molar concentration of the iron source after being prepared into a solution is 0.1 to 0.2 mol / L.
[0012] Preferably, the organic phosphoric acid in step (1) is at least one of ethylenediaminetetramethylenediphosphonic acid, aminotrimethylenephosphonic acid, hexamethylenediaminetetramethylenephosphonic acid, and diethylenetriaminepenta(methylenephosphonic acid).
[0013] More preferably, the pH of the aqueous solution of organic phosphoric acid is 1.5 to 2.5, and the molar concentration of organic phosphoric acid is 0.1 to 0.2 mol / L.
[0014] Preferably, in step (1), the volume ratio of the solution prepared with the iron source to the aqueous solution of the organic phosphoric acid is 1:(1-1.1).
[0015] Preferably, in step (3), the manganese source is at least one of manganese acetate, manganese oxalate, manganese nitrate, manganese sulfate, and manganese phosphate; the lithium source is at least one of lithium carbonate, lithium hydroxide, lithium acetate, lithium oxalate, lithium chloride, and lithium iodide; the reducing agent is at least one of glucose, sucrose, citric acid, ascorbic acid, malic acid, vitamin C, oxalic acid, formic acid, polyvinyl alcohol, polybutadiene, and ammonium sulfide; and the dispersant is at least one of ethanol and water.
[0016] Preferably, in step (3), a phosphorus source is added and mixed with the porous iron metaphosphate B, manganese source, lithium source, reducing agent and dispersant, and the phosphorus source is at least one of ammonium phosphate, diammonium dihydrogen phosphate, diammonium hydrogen phosphate and phosphoric acid.
[0017] According to the actual ratio requirements, the phosphorus source required by the ratio can be further introduced into the mixture to prepare the product.
[0018] More preferably, in the step (3), the molar ratio of the iron element in the porous iron phosphate B to the manganese element in the manganese source is (1:2) to (1:9); the molar ratio of (total phosphorus element in porous iron phosphate B, manganese source and phosphorus source): (iron element in porous iron phosphate B + manganese element in manganese source) is (1 to 1.1):1.
[0019] More preferably, in step (3), the mass ratio of porous iron metaphosphate B to the reducing agent is 1:(0.05-0.1).
[0020] Preferably, in the step (3), the ball-to-material ratio during ball milling is (5-15):1, the particle size of the ball milling beads used is 5-10 mm, and the ball milling time is 3-8 h; the mass ratio of the sum of the porous iron metaphosphate B, manganese source, lithium source and reducing agent to the dispersant (porous iron metaphosphate B+manganese source+lithium source+reducing agent):dispersant=1:(1.8-2.2).
[0021] Preferably, in step (3), the heating rate during heating is 4 to 6°C / min.
[0022] Another object of the present invention is to provide a carbon-coated lithium manganese iron phosphate positive electrode material prepared by the method for preparing the carbon-coated lithium manganese iron phosphate positive electrode material.
[0023] The carbon-coated lithium manganese iron phosphate positive electrode material of the present invention has a high degree of reduction and uniformity of reduction of each raw material during the thermal reduction process due to the construction of the precursor with a special morphology of porous iron metaphosphate B, and the purity of the product is higher than that of the lithium manganese iron phosphate positive electrode material prepared by ordinary processes; at the same time, the coated and modified carbon coating layer has a high bonding strength with the active lithium manganese iron phosphate positive electrode material contained therein, and the degree of electrical conductivity improvement is high. The overall product has high electrochemical activity, and the discharge specific capacity at a rate of 0.1C can reach more than 155mAh / g.
[0024] The beneficial effect of the present invention is that the present invention provides a method for preparing a carbon-coated lithium manganese iron phosphate positive electrode material. The method pre-constructs a ferric iron phosphate precursor with a porous structure, and then mixes the precursor with raw materials such as a manganese source and a reducing agent for thermal reduction. Not only can the reducing agent and the manganese source be evenly dispersed on the ferric iron phosphate precursor and achieve a sufficient reduction reaction, but a carbon coating layer is also formed synchronously during the thermal reduction process, and the carbon coating layer can penetrate into the porous structure of the ferric iron phosphate precursor, has a high bonding strength with the obtained lithium manganese iron phosphate positive electrode material, and has a high compaction density, and can more evenly and effectively improve the conductivity of the overall product. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the XRD spectra of the products obtained from Example 1, Comparative Example 1 and Comparative Example 2 in Effect Example 1 of the present invention.
[0026] Figure 2 This is a scanning electron microscope image of the porous iron metaphosphate B obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0027] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.
[0028] Example 1
[0029] An embodiment of a method for preparing a carbon-coated lithium manganese iron phosphate positive electrode material according to the present invention comprises the following steps:
[0030] (1) preparing a solution with a concentration of 0.15 mol / L by mixing ferric chloride with water and adding the solution to an aqueous solution of ethylenediaminetetramethylenediphosphonic acid with a pH of 2 and a molar concentration of 0.15 mol / L at a volume ratio of 1:1, and mixing the mixture evenly; adjusting the pH of the mixture to 11 with sodium carbonate to obtain a reaction solution A;
[0031] (2) heating the reaction solution A to 80° C. and stirring the reaction for 3 h, then adjusting the pH to 2 with hydrochloric acid and aging for 2 h, filtering the suspension, washing the obtained solid with water, drying at 60° C. for 12 h, and heating to 750° C. in an air atmosphere for 6 h to obtain porous iron metaphosphate B;
[0032] (3) Porous iron metaphosphate B is mixed with manganese oxalate, lithium hydroxide, citric acid and ethanol, ball-milled for 8 hours under a protective atmosphere, and then heated to 400°C at a rate of 5°C / min for 5 hours, and then heated to 750°C for 8 hours, to obtain the carbon-coated manganese iron phosphate lithium positive electrode material; wherein the molar ratio of manganese element in manganese oxalate, iron element in porous iron metaphosphate B, and lithium element in lithium hydroxide is 2:1:3; the amount of citric acid added is 8% of the mass of porous iron metaphosphate B. The mass ratio of the sum of the porous iron metaphosphate B, manganese source, lithium source and reducing agent to the dispersant (porous iron metaphosphate B+manganese source+lithium source+reducing agent): dispersant=1:2; the ball-to-material ratio during ball milling is 10:1, and the particle size of the ball milling beads used is 5 mm.
[0033] Example 2
[0034] An embodiment of a method for preparing a carbon-coated lithium manganese iron phosphate positive electrode material according to the present invention comprises the following steps:
[0035] (1) preparing a solution with a concentration of 0.15 mol / L by mixing ferric chloride with water and adding the solution to an aqueous solution of ethylenediaminetetramethylenediphosphonic acid with a pH of 2 and a molar concentration of 0.15 mol / L at a volume ratio of 1:1, and mixing the mixture evenly; adjusting the pH of the mixture to 11 with sodium carbonate to obtain a reaction solution A;
[0036] (2) heating the reaction solution A to 75° C. and stirring the reaction for 5 h, then adjusting the pH to 2 with hydrochloric acid and aging for 2 h, filtering the suspension, washing the obtained solid with water, drying at 60° C. for 12 h, and heating to 700° C. in an air atmosphere for 6 h to obtain porous iron metaphosphate B;
[0037] (3) Porous iron metaphosphate B is mixed with manganese oxalate, lithium hydroxide, citric acid and ethanol, ball-milled for 8 hours under a protective atmosphere, and then heated to 400°C at a rate of 5°C / min for 5 hours, and then heated to 700°C for 12 hours, to obtain the carbon-coated manganese iron phosphate lithium positive electrode material; wherein the molar ratio of manganese element in manganese oxalate, iron element in porous iron metaphosphate B, and lithium element in lithium hydroxide is 2:1:3; the amount of citric acid added is 8% of the mass of porous iron metaphosphate B. The mass ratio of the sum of the porous iron metaphosphate B, manganese source, lithium source and reducing agent to the dispersant (porous iron metaphosphate B+manganese source+lithium source+reducing agent): dispersant=1:2; the ball-to-material ratio during ball milling is 10:1, and the particle size of the ball milling beads used is 5 mm.
[0038] Example 3
[0039] An embodiment of a method for preparing a carbon-coated lithium manganese iron phosphate positive electrode material according to the present invention comprises the following steps:
[0040] (1) preparing a solution with a concentration of 0.15 mol / L by using water to prepare ferric nitrate, and adding the solution to an aqueous solution of hexamethylenediaminetetramethylenephosphonic acid with a pH of 2 and a molar concentration of 0.15 mol / L at a volume ratio of 1:1, and mixing the mixture evenly; adjusting the pH of the mixture to 11 with sodium carbonate to obtain a reaction solution A;
[0041] (2) heating the reaction solution A to 80° C. and stirring the reaction for 3 h, then adjusting the pH to 2 with hydrochloric acid and aging for 2 h, filtering the suspension, washing the obtained solid with water, drying at 60° C. for 12 h, and heating to 750° C. in an air atmosphere for 6 h to obtain porous iron metaphosphate B;
[0042] (3) Porous iron metaphosphate B is mixed with manganese nitrate, lithium carbonate, ascorbic acid and ethanol, ball-milled for 8 hours under a protective atmosphere, and then heated to 400°C at a rate of 5°C / min for 5 hours, and then heated to 650°C for 15 hours, to obtain the carbon-coated manganese iron phosphate lithium positive electrode material; wherein the molar ratio of manganese element in manganese nitrate, iron element in porous iron metaphosphate B, and lithium element in lithium carbonate is 2:1:3; the amount of ascorbic acid added is 8% of the mass of porous iron metaphosphate B. The mass ratio of the sum of the porous iron metaphosphate B, manganese source, lithium source and reducing agent to the dispersant (porous iron metaphosphate B+manganese source+lithium source+reducing agent): dispersant=1:2; the ball-to-material ratio during ball milling is 10:1, and the particle size of the ball milling beads used is 5 mm.
[0043] Example 4
[0044] The only difference between this embodiment and embodiment 1 is that the molar ratio of the manganese element in manganese oxalate, the iron element in porous iron metaphosphate B, the lithium element in lithium hydroxide, and the diammonium phosphate added in step (3) is 0.75:0.25:1:0.25; and the amount of citric acid added is 5% of the mass of porous iron metaphosphate B.
[0045] Example 5
[0046] The only difference between this embodiment and embodiment 1 is that the molar ratio of the manganese element in manganese oxalate, the iron element in porous iron metaphosphate B, the lithium element in lithium hydroxide, and the diammonium phosphate added in step (3) is 0.8:0.2:1:0.4; and the amount of citric acid added is 5% of the mass of porous iron metaphosphate B.
[0047] Example 6
[0048] The only difference between this embodiment and embodiment 1 is that the molar ratio of the manganese element in manganese oxalate, the iron element in porous iron metaphosphate B, the lithium element in lithium hydroxide, and the diammonium phosphate added in step (3) is 0.9:0.1:1:0.7; and the amount of citric acid added is 10% of the mass of porous iron metaphosphate B.
[0049] Comparative Example 1
[0050] A method for preparing a carbon-coated lithium manganese iron phosphate positive electrode material, the preparation method comprising the following steps:
[0051] The ferric phosphate is mixed with manganese oxalate, lithium hydroxide, citric acid and ethanol, ball-milled for 8 hours under a protective atmosphere, and then heated to 400°C at a rate of 5°C / min for 5 hours, and then heated to 750°C for 8 hours to obtain the carbon-coated manganese iron phosphate lithium positive electrode material; wherein the manganese element in manganese oxalate, the iron element in the ferric phosphate, and the lithium element in the lithium hydroxide are 2:1:3; the amount of citric acid added is 8% of the mass of the ferric phosphate. The mass ratio of the sum of the ferric phosphate, manganese source, lithium source and reducing agent to the dispersant (ferric phosphate + manganese source + lithium source + reducing agent): dispersant = 1:2; the ball-to-material ratio during ball milling is 10:1, and the particle size of the ball milling beads used is 5mm. The ferric phosphate is a non-porous ferric phosphate particle with an average particle size of 1.5 to 2.5μm.
[0052] Comparative Example 2
[0053] A method for preparing a carbon-coated lithium manganese iron phosphate positive electrode material, the preparation method comprising the following steps:
[0054] 0.015 mol of ferric chloride, 0.045 mol of lithium hydroxide, 0.03 mol of manganese oxalate and 0.2 g of ascorbic acid are mixed and transferred into an aqueous solution of ethylenediaminetetramethylenediphosphonic acid with a molar concentration of 0.15 mol / L, the pH is controlled to be 2, and the mixture is ground and mixed evenly at room temperature. The resulting mixed solution is dried at room temperature under vacuum conditions for 12 hours, and then heated to 400°C at a rate of 5°C / min in a tubular furnace under a protective atmosphere for 5 hours, and then heated to 750°C for 8 hours to obtain the carbon-coated lithium manganese iron phosphate positive electrode material.
[0055] Effect Example 1
[0056] In order to verify the performance of the product prepared by the preparation method of the present invention, the products of each embodiment and comparative example were assembled in a glove box with commercial metal lithium sheets as negative electrodes and commercial polypropylene diaphragms as diaphragms to prepare CR2032 button batteries, and then charge and discharge tests were carried out at an operating voltage of 2.5 to 4.5 V and a rate of 0.1C. The test results are shown in Table 1.
[0057] Table 1
[0058]
[0059] As can be seen from Table 1, the carbon-coated lithium manganese iron phosphate positive electrode materials prepared in each embodiment of the present invention have high electrochemical activity, and their discharge specific capacity can reach up to 156 mAh / g at a rate of 0.1C. The products obtained in Example 1, Comparative Example 1 and Comparative Example 2 were subjected to XRD analysis. The results are as follows: Figure 1 As shown, it can be seen that although the raw materials used in Comparative Examples 1 and 2 are very similar to the technical solution of Example 1, they do not have a precursor for constructing porous materials. The characteristic peaks in the XRD spectrum of the carbon-coated lithium manganese iron phosphate positive electrode material finally prepared are not as strong or corresponding as those of the product in Example 1, indicating that when ordinary precursor raw materials or ordinary processes are used to prepare products, the reducing agent cannot fully play its role, and the electrochemical performance of the prepared product is inevitably not as good as that of the product in Example 1. The porous iron metaphosphate B prepared in Example 1 was observed by scanning electron microscopy, and the results are as follows Figure 2 As shown, it can be seen that the porous iron metaphosphate B has a small particle size and a rich porous structure, which can fully load the manganese source, lithium source and reducing agent and achieve a uniform reduction reaction during the thermal reduction process.
[0060] The products of Example 1, Comparative Example 1 and Comparative Example 2 were subjected to a cycle performance test, and 50 charge and discharge cycles were performed at the same rate. The discharge specific capacity and capacity retention rate after 50 cycles were calculated, and the results are shown in Table 1. It can be seen that the discharge specific capacity of the products prepared in each embodiment of the present invention can still reach about 150 mAh / g after 50 cycles, and the capacity retention rate is relatively high. However, due to the defects of the material configuration of the products of Comparative Examples 1 and 2, the discharge specific capacity attenuation degree after 50 cycles is relatively high, and the capacity retention rate is relatively low.
[0061] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a carbon-coated lithium manganese iron phosphate positive electrode material, characterized in that: The following steps are involved: (1) preparing an iron source into a solution and adding it into an aqueous solution of an organic phosphoric acid and mixing it evenly, and adjusting the pH of the resulting mixed solution to 10 to 12 to obtain a reaction solution A; (2) heating the reaction solution A to 75-85° C. and reacting for 2-5 hours, then adjusting the pH to 2-3 and aging for 1-3 hours, filtering, washing and drying the obtained solid, and heating to 400-800° C. in an air atmosphere for 4-6 hours to obtain porous iron metaphosphate B; (3) The porous iron metaphosphate B is mixed with a manganese source, a lithium source, a reducing agent and a dispersant, and ball-milled under a protective atmosphere, and then heated to 300-400° C. for 3-5 hours, and then heated to 400-800° C. for 5-15 hours to obtain the carbon-coated manganese iron lithium phosphate positive electrode material.
2. The method for preparing the carbon-coated lithium manganese iron phosphate positive electrode material according to claim 1, characterized in that: In the step (1), the iron source is at least one of ferric chloride, ferric sulfate, ferric nitrate and ferric acetate, and the molar concentration of the iron source after being prepared into a solution is 0.1-0.2 mol / L.
3. The method for preparing the carbon-coated lithium manganese iron phosphate positive electrode material according to claim 1, characterized in that: In the step (1), the organic phosphoric acid is at least one of ethylenediaminetetramethylenediphosphonic acid, aminotrimethylenephosphonic acid, hexamethylenediaminetetramethylenephosphonic acid, and diethylenetriaminepenta(methylenephosphonic acid).
4. The method for preparing the carbon-coated lithium manganese iron phosphate positive electrode material according to claim 3, characterized in that: The pH of the aqueous solution of organic phosphoric acid is 1.5-2.5, and the molar concentration of organic phosphoric acid is 0.1-0.2 mol / L.
5. The method for preparing the carbon-coated lithium manganese iron phosphate positive electrode material according to claim 1, characterized in that: In the step (1), the volume ratio of the solution prepared with the iron source to the aqueous solution of the organic phosphoric acid is 1:(1-1.1).
6. The method for preparing the carbon-coated lithium manganese iron phosphate positive electrode material according to claim 1, characterized in that: In the step (3), the manganese source is at least one of manganese acetate, manganese oxalate, manganese nitrate, manganese sulfate, and manganese phosphate; the lithium source is at least one of lithium carbonate, lithium hydroxide, lithium acetate, lithium oxalate, lithium chloride, and lithium iodide; the reducing agent is at least one of glucose, sucrose, citric acid, ascorbic acid, malic acid, oxalic acid, formic acid, polyvinyl alcohol, polybutadiene, and ammonium sulfide; and the dispersant is at least one of ethanol and water.
7. The method for preparing the carbon-coated lithium manganese iron phosphate positive electrode material according to claim 6, characterized in that: In the step (3), a phosphorus source is added and mixed with the porous iron metaphosphate B, the manganese source, the lithium source, the reducing agent and the dispersant, and the phosphorus source is at least one of ammonium phosphate, diammonium phosphate, diammonium hydrogen phosphate and phosphoric acid.
8. The method for preparing the carbon-coated lithium manganese iron phosphate positive electrode material according to claim 7, characterized in that: In the step (3), the molar ratio of the iron element in the porous iron phosphate B to the manganese element in the manganese source is (1:2) to (1:9); the molar ratio of (total phosphorus element in the porous iron phosphate B, the manganese source and the phosphorus source): (iron element in the porous iron phosphate B + manganese element in the manganese source) is (1 to 1.1):
1.
9. The method for preparing the carbon-coated lithium manganese iron phosphate positive electrode material according to claim 8, characterized in that: In the step (3), the mass ratio of the porous iron metaphosphate B to the reducing agent is 1:(0.05-0.1).
10. The method for preparing the carbon-coated lithium manganese iron phosphate positive electrode material according to claim 1, characterized in that: In the step (3), the ball-to-material ratio during ball milling is (5-15):1, the particle size of the ball milling beads used is 5-10 mm, and the ball milling time is 3-8 hours; the mass ratio of the sum of the porous iron metaphosphate B, manganese source, lithium source and reducing agent to the dispersant (porous iron metaphosphate B+manganese source+lithium source+reducing agent):dispersant=1:(1.8-2.2).