Preparation method of nano-aluminum oxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier

By using a method of preparing styrene-divinylbenzene copolymer modified by nano-alumina hybridization, the problem of low compressive strength of SDB hydrophobic catalyst support was solved, and a high compressive strength and hydrophobicity HFTMS-Al2O3/SDB hydrophobic catalyst support was prepared for efficient treatment of tritium-containing wastewater.

CN115888819BActive Publication Date: 2024-11-05SHANGHAI YUNSONG TECH DEV CO LTD +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202211406964.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-10
Publication Date
2024-11-05
Estimated Expiration
2042-11-10

AI Technical Summary

Technical Problem

The existing hydrophobic catalyst support for SDB has low compressive strength, which makes it difficult to meet the requirements for efficient treatment of tritium-containing wastewater.

Method used

A method for preparing styrene-divinylbenzene copolymer by hybrid modification of nano-alumina was adopted. By introducing heptadecafluorodecyltrimethoxysilane to modify nano-alumina, the compressive strength and hydrophobicity of the support were improved. HFTMS-Al2O3/SDB hydrophobic catalyst support was prepared by suspension polymerization.

Benefits of technology

The compressive strength and hydrophobicity of the HFTMS-Al2O3/SDB hydrophobic catalyst support were significantly improved, enhancing the stability and catalytic performance of the catalyst, making it suitable for engineering applications such as heavy water tritium extraction and wastewater tritium removal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115888819B_ABST
    Figure CN115888819B_ABST
Patent Text Reader

Abstract

In order to solve the problem of low compressive strength of the existing SDB hydrophobic catalyst carrier, the present invention discloses a preparation method of a nano aluminum oxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier, comprising the following steps: 17-fluorodecyltrimethoxysilane, nano aluminum oxide and ethanol are reacted to obtain modified nano aluminum oxide; an aqueous phase is configured; styrene, divinylbenzene, benzoyl peroxide and modified nano aluminum oxide are mixed to obtain an oil phase; and suspension polymerization is performed to obtain a nano aluminum oxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier. In the preparation method, nano aluminum oxide modified by 17-fluorodecyltrimethoxysilane is introduced, and the compressive strength and hydrophobicity of the SDB hydrophobic catalyst carrier are greatly improved through the excellent mechanical properties of inorganic nanoparticles themselves, and the particle size is larger.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to catalyst technology, in particular to a method for preparing a nano-aluminum oxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier. Background Art

[0002] Nuclear power generation has developed rapidly due to its high and stable power supply efficiency and the fact that it does not emit sulfur oxides, greenhouse gases and nitrogen oxides like traditional fossil fuels. However, with the development of nuclear power generation, the discharge of tritium-containing wastewater is also increasing, and these tritium-containing wastewater cannot be treated by conventional three-waste systems.

[0003] From the perspective of economy and safety, hydrogen-water liquid phase catalytic exchange technology (LPCE) is one of the most effective methods for treating tritium-containing wastewater. The key material of LPCE technology is the hydrophobic catalyst, which is composed of a catalyst carrier and an active component. There are two commonly used hydrophobic catalysts, namely hydrophobic catalysts with polytetrafluoroethylene (PTFE) as a carrier and hydrophobic catalyst carriers with styrene-divinylbenzene copolymer (SDB) as a carrier.

[0004] For example, the Chinese invention patent application (CN113019464A) discloses a method for preparing a size-controllable spherical SDB hydrophobic carrier and a Pt / SDB hydrophobic catalyst, and specifically discloses that the preparation method of the Pt / SDB hydrophobic catalyst specifically includes the following steps: mixing a determined ratio of styrene and divinylbenzene polymerization monomers, a polymerization initiator benzoyl peroxide, a determined ratio of a mixed porogen of toluene and n-heptane, and a density regulator to obtain an organic phase; prepolymerizing the mixed organic phase in a low surface tension aqueous solution at low temperature to cause droplet aggregation, then heating to initiate a polymerization reaction to obtain a spherical SDB hydrophobic carrier crude product, extracting with acetone, and then using mechanical grinding physical etching and oxidizing acid oxidation chemical etching to achieve surface roughening, washing and drying to obtain a spherical SDB hydrophobic carrier, loading the active component on the surface of the carrier by an impregnation method, and then obtaining a Pt / SDB hydrophobic catalyst by high-temperature hydrogenation reduction. According to the catalytic gas phase HD exchange test, the efficiency of the Pt / SDB hydrophobic catalyst can reach more than 94%.

[0005] However, the existing SDB hydrophobic catalyst carrier also has low compressive strength and needs to be improved urgently. Summary of the invention

[0006] The present invention solves the problem of low compressive strength of the existing SDB hydrophobic catalyst carrier and provides a method for preparing a nano-aluminum trioxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier. In the preparation method, nano-aluminum trioxide modified by heptadecafluorodecyltrimethoxysilane is introduced, and the compressive strength and hydrophobicity of the SDB hydrophobic catalyst carrier are greatly improved by the excellent mechanical properties of the inorganic nanoparticles themselves, and the particle size is larger.

[0007] The technical solution adopted by the present invention is:

[0008] The preparation method of a nano-aluminum oxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier comprises the following steps:

[0009] Step S1, mixing heptadecafluorodecyltrimethoxysilane (HFTMS), nano-aluminum trioxide (nano-Al2O3) and ethanol according to a predetermined ratio, and obtaining modified nano-aluminum trioxide after reaction;

[0010] Step S2, mixing hydroxymethyl cellulose, sodium dodecylbenzene sulfonate, polyvinyl alcohol 1788 and water according to a predetermined ratio to obtain an aqueous phase;

[0011] Step S3, mixing styrene, divinylbenzene, benzoyl peroxide and modified nano-aluminum oxide, as well as toluene, n-heptane and ethylene dichloride according to a predetermined ratio to obtain an oil phase;

[0012] Step S4, according to the preset reaction conditions, all the oil phase is added to the water phase for suspension polymerization. After the reaction is completed, the nano-aluminum trioxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier (HFTMS-Al2O3 / SDB hydrophobic catalyst carrier) is obtained by filtration, drying and sieving.

[0013] Furthermore, in step S1, heptadecafluorodecyltrimethoxysilane, nano-aluminum oxide and ethanol are mixed according to a predetermined ratio, and the specific process of obtaining modified nano-aluminum oxide after reaction includes:

[0014] Step S11, mixing heptadecafluorodecyltrimethoxysilane and ethanol in a volume ratio of 1:100 to obtain a modifier dilution solution;

[0015] Step S12, according to the weight ratio of 17fluorodecyltrimethoxysilane to nano-aluminum oxide of 0.2-0.5:1, adding nano-aluminum oxide to the modifier dilution solution for reaction, controlling the reaction temperature to 50-60°C, the reaction time to 4-6 hours, and after the reaction is completed, washing with anhydrous ethanol and water in sequence, and drying to obtain modified nano-aluminum oxide.

[0016] Furthermore, in step S12, the weight ratio of heptadecafluorodecyltrimethoxysilane to nano-aluminum oxide is 0.35:1, the reaction temperature is controlled at 70° C., and the reaction time is 4 hours.

[0017] Furthermore, in step 12, when washing with anhydrous ethanol and water, the amount of anhydrous ethanol and water used is 10 to 20 times the volume of heptadecafluorodecyltrimethoxysilane respectively;

[0018] And / or, in step S12, vacuum drying is adopted during drying, the drying temperature is 70-80° C., and the drying time is 3-4 hours.

[0019] Furthermore, in step S2, the amount of each raw material in the aqueous phase is calculated by weight:

[0020] Hydroxymethyl cellulose, 0.1-0.3 parts;

[0021] Sodium dodecylbenzenesulfonate, 0.1-0.4 parts;

[0022] Polyvinyl alcohol 1788, 2-4 parts;

[0023] Water, 200-400 parts.

[0024] Furthermore, in step S2, the water phase mixing temperature is 70-80° C., and the mixing time is 1-2 hours.

[0025] Furthermore, in step S3, the amount of each raw material of the oil phase is calculated by weight:

[0026] Styrene, 2-10 parts;

[0027] Divinylbenzene, 2-10 parts;

[0028] Benzoyl peroxide, 0.1~0.6 parts;

[0029] Modified nano-aluminum oxide, 0.01~2 parts;

[0030] Toluene, 1-16 parts;

[0031] n-heptane, 12-24 parts;

[0032] Ethylene dichloride, 5-12 parts.

[0033] Furthermore, in step S3, the mass ratio of styrene, divinylbenzene and modified nano-aluminum oxide is 10:10:0.05-0.2.

[0034] Furthermore, in step S3, the oil phase is firstly ultrasonically mixed for 30 minutes.

[0035] Furthermore, in step S4, during suspension polymerization, the reaction temperature is controlled to be 90-95° C. and the reaction time is 7-8 h;

[0036] And / or, in step S4, the drying temperature is 60-70° C., and the drying time is 5-6 hours.

[0037] The beneficial effects of the present invention are:

[0038] 1. In order to improve the strength of the SDB hydrophobic catalyst carrier, the present invention uses styrene as a monomer, divinylbenzene as a crosslinking agent, benzoyl peroxide as an initiator, n-heptane as a porogen, 1,2-dichloroethane as a solubilizer, modified nano-aluminum trioxide as a modified functional monomer, polyvinyl alcohol 1788 as an organic polymer dispersant, sodium dodecylbenzene sulfonate and hydroxymethyl cellulose as dispersants. The present invention utilizes the synergistic effect between polyvinyl alcohol 1788, sodium dodecylbenzene sulfonate and hydroxymethyl cellulose, and uses the selected functional monomer HFTMS to introduce a -CF group on the surface of nano-Al2O3 to improve the hydrophobicity of nano-Al2O3, so that the modified nano-Al2O3 (HFTMS-Al2O3) can be better dispersed in the oil phase. At the same time, the introduced modified nano-Al2O3 (HFTMS-Al2O3) itself has excellent mechanical properties, which can greatly improve the compressive resistance and hydrophobicity of the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier.

[0039] 2. The present invention adopts a suspension polymerization method, which is simple, easy to operate, and highly practical. The material is fed in a one-time ratio, which is easy to form stable and uniform oil droplets. At the same time, modified polymerization monomers styrene and divinylbenzene with suitable reactivity ratios, as well as modified nano-Al2O3 as the third functional monomer, are selected to achieve suspension polymerization ternary copolymerization, and synthesize HFTMS-Al2O3 / SDB hydrophobic catalyst carriers with large specific surface area and suitable pore size and pore volume. The hydrophobic angle of the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier can reach 147°, the compressive strength can reach 132N, and the particle size is 2 to 3mm.

[0040] 3. The HFTMS-Al2O3 / SDB hydrophobic catalyst carrier prepared in the present invention has a high loading stability for catalytically active components (i.e., it can provide loading active sites, etc.), can improve the catalytic performance of the catalyst, and has the advantages of reducing the mass transfer resistance of the bed, preventing flooding, and improving the fluid exchange efficiency. The metal-supported catalyst (such as Pt / SDB hydrophobic catalyst) prepared with the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier prepared in the present invention can be used for engineering applications such as heavy water tritium extraction and wastewater tritium removal, has high catalytic efficiency, excellent hydrophobic stability, can be used at room temperature, and has good use effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0042] Figure 1 This is a graph showing the static contact angle test results of the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier in Example 17.

[0043] Figure 2 This is a scanning electron microscope image of the HFTMS-Al2O3 / SDB hydrophobic catalyst support in Example 17.

[0044] Figure 3 This is the infrared detection result of the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier in Example 17.

[0045] Figure 4 This is the thermogravimetric result of the HFTMS-Al2O3 / SDB hydrophobic catalyst support in Example 17.

[0046] Figure 5 This is the elemental analysis diagram of the HFTMS-Al2O3 / SDB hydrophobic catalyst support in Example 17. DETAILED DESCRIPTION

[0047] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0048] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention.

[0049] The embodiments of the invention are described in detail below with reference to the accompanying drawings.

[0050] The preparation method of a nano-aluminum oxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier comprises the following steps:

[0051] Step S1, according to a predetermined ratio, HFTMS, nano-aluminum trioxide (nano-Al2O3) and ethanol are mixed to obtain modified nano-aluminum trioxide (modified nano-Al2O3) after reaction. 3) ;

[0052] Step S2, mixing hydroxymethyl cellulose, sodium dodecylbenzene sulfonate, polyvinyl alcohol 1788 and water according to a predetermined ratio to obtain an aqueous phase;

[0053] Step S3, mixing styrene, divinylbenzene, benzoyl peroxide and modified nano-aluminum oxide, as well as toluene, n-heptane and ethylene dichloride according to a predetermined ratio to obtain an oil phase;

[0054] Step S4, according to the preset reaction conditions, all the oil phase is added to the water phase for suspension polymerization. After the reaction is completed, the nano-aluminum trioxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier (HFTMS-Al2O3 / SDB hydrophobic catalyst carrier) is obtained by filtration, drying and sieving.

[0055] Furthermore, in step S1, heptadecafluorodecyltrimethoxysilane, nano-aluminum oxide and ethanol are mixed according to a predetermined ratio, and the specific process of obtaining modified nano-aluminum oxide after reaction includes:

[0056] Step S11, mixing heptadecafluorodecyltrimethoxysilane and ethanol in a volume ratio of 1:100 to obtain a modifier dilution solution;

[0057] Step S12, according to the weight ratio of 17fluorodecyltrimethoxysilane to nano-aluminum trioxide (nano-Al2O3) of 0.2~0.5:1, add nano-aluminum trioxide to the modifier dilution solution for reaction, control the reaction temperature to 50~60°C, the reaction time to 4~6h, after the reaction is completed, wash with anhydrous ethanol and water in turn, and dry to obtain modified nano-aluminum trioxide.

[0058] Furthermore, in step S12, the weight ratio of heptadecafluorodecyltrimethoxysilane to nano-aluminum oxide is 0.35:1, the reaction temperature is controlled at 70° C., and the reaction time is 4 hours.

[0059] Furthermore, in step 12, when washing with anhydrous ethanol and water, the amount of anhydrous ethanol and water used is 10 to 20 times the volume of heptadecafluorodecyltrimethoxysilane respectively;

[0060] And / or, in step S12, vacuum drying is adopted during drying, the drying temperature is 70-80° C., and the drying time is 3-4 hours.

[0061] Furthermore, in step S2, the amount of each raw material in the aqueous phase is calculated by weight:

[0062] Hydroxymethyl cellulose, 0.1-0.3 parts;

[0063] Sodium dodecylbenzenesulfonate, 0.1-0.4 parts;

[0064] Polyvinyl alcohol 1788, 2-4 parts;

[0065] Water (distilled or deionized), 200-400 parts.

[0066] Furthermore, in step S2, the water phase mixing temperature is 70-80° C., and the mixing time is 1-2 hours.

[0067] Furthermore, in step S3, the amount of each raw material of the oil phase is calculated by weight:

[0068] Styrene, 2-10 parts;

[0069] Divinylbenzene, 2-10 parts;

[0070] Benzoyl peroxide, 0.1~0.6 parts;

[0071] Modified nano-aluminum oxide, 0.01~2 parts;

[0072] Toluene, 1-16 parts;

[0073] n-heptane, 12-24 parts;

[0074] Ethylene dichloride, 5-12 parts.

[0075] Furthermore, in step S3, the mass ratio of styrene, divinylbenzene and modified nano-aluminum oxide is 10:10:0.05-0.2.

[0076] Furthermore, in step S3, the oil phase is firstly ultrasonically mixed for 30 minutes.

[0077] Furthermore, in step S4, during suspension polymerization, the reaction temperature is controlled to be 90-95° C. and the reaction time is 7-8 h;

[0078] And / or, in step S4, the drying temperature is 60-70° C., and the drying time is 5-6 hours.

[0079] The present application is described in detail below through specific examples. In order to obtain a HFTMS-Al2O3 / SDB hydrophobic catalyst carrier with excellent performance, the inventors conducted the following research.

[0080] (1) Research on modification of nano-aluminum oxide

[0081] The particle size of nano-Al2O3 is 20nm, and it is easy to cause powder agglomeration due to the intermolecular force. When it is directly added to the oil phase, there will be a problem of poor dispersibility. Therefore, the inventors conducted relevant tests and research on the modification process of nano-aluminum oxide, and tested the static contact angle (hydrophobic angle) of the modified nano-Al2O3.

[0082] The preparation process of modified nano-alumina in Examples 1 to 5 is as follows: 0.5 g of KH560, KH570, stearic acid, 13-fluorooctyl trimethoxysilane (PFOTMS) and 17-fluorodecyl trimethoxysilane (HFTMS) are used as modifiers, and the modifiers and ethanol are mixed at a volume ratio of 1:100 to obtain a modifier dilution; wherein, since stearic acid is solid at room temperature, it is converted into the corresponding weight and then configured. 1 g of nano-Al2O3 is added to the modifier dilution, the reaction temperature is controlled to 50°C, the reaction time is 5h, and after the reaction is completed, anhydrous ethanol and water are washed in turn, and dried to obtain modified nano-Al2O3. The test results related to the modified nano-Al2O3 prepared in Examples 1 to 5 are shown in Table 1 below.

[0083] Control Example 1 is to test the initial unmodified nano-aluminum oxide without any treatment in the same test method.

[0084] Table 1 Static contact angle test results of modified nano-Al2O3 in Examples 1 to 5

[0085]

[0086] From the test results of Examples 1 to 5 in Table 1, it can be seen that KH560, KH570, stearic acid, PFOTMS and HFTMS can all significantly improve the hydrophobicity of nano-Al2O3. The hydrophobic modification effects of KH560, KH570, stearic acid, PFOTMS and HFTMS on nano-Al2O3 are better than those of KH560, KH570 and stearic acid on nano-Al2O3. The inventors analyzed that the reason is that HFTMS and PFOTMS introduce CF bonds into nano-Al2O3 through their own chemical structures, thereby improving the hydrophobicity of nano-Al2O3.

[0087] At the same time, the hydrophobic modification effect of HFTMS on nano-Al2O3 is better than that of PFOTMS. The inventors analyzed that the reason is that HFTMS contains more CF bonds than PFOTMS, so the modification effect of HFTMS on nano-Al2O3 is more advantageous. In addition, when the inventors placed HFTMS- and PFOTMS-modified nano-Al2O3 in oil phase (mixed liquids such as styrene, divinylbenzene, toluene, dichloroethane, and n-heptane), the sedimentation stability of HFTMS-modified nano-Al2O3 (HFTMS-Al2O3) was better than that of PFOTMS-modified nano-Al2O3 (PFOTMS-Al2O3) at continuous time (24h), that is, the dispersion effect of HFTMS-modified nano-Al2O3 in oil phase is better.

[0088] Therefore, the inventors studied the modification of nano-Al2O3 using HFTMS as a modifier in the subsequent examples. At the same time, the inventors used orthogonal experiments (orthogonal experimental design table 2-1) to study and test the effects of reaction temperature, reaction time and modifier dosage on the modified nano-Al2O3, namely, Examples 6 to 14. Among them, the preparation process of Examples 6 to 14 is similar to that of Examples 1 to 5, except that different experimental factors (time, temperature and modifier dosage) are replaced. The static contact angle test results of the modified nano-Al2O3 prepared in Examples 6 to 14 are shown in Table 2-2.

[0089] Table 2-1 Orthogonal test design table

[0090]

[0091] Table 2-2 Static contact angle test results of modified nano-Al2O3 in Examples 6 to 14

[0092]

[0093] From the test results of Examples 6 to 14 in Table 2-2, it can be seen that in the process of modifying nano-Al2O3 with HFTMS as a modifier, prolonging the reaction time, increasing the reaction temperature or increasing the amount of the modifier can improve the hydrophobic properties of nano-Al2O3, thereby improving the dispersibility of the modified nano-Al2O3 in the oil phase.

[0094] At the same time, the above test results also show that when the weight ratio of HFTMS to nano-Al2O3 is 0.35:1, the reaction temperature is 70℃, and the reaction time is 4h, the static water contact angle of the prepared modified nano-Al2O3 is the largest, which can reach 141.76 0 .

[0095] Therefore, the inventors used this as the control condition in the subsequent research of the embodiments (i.e., the process in Example 11 was used as the control standard) to prepare HFTMS-modified nano-Al2O3 (HFTMS-Al2O3) and conduct the preparation research of HFTMS-Al2O3 / SDB hydrophobic catalyst carrier.

[0096] (II) Study on HFTMS-Al2O3 / SDB hydrophobic catalyst support

[0097] In order to explore the effect of HFTMS-Al2O3 on the preparation process of HFTMS-Al2O3 / SDB hydrophobic catalyst carrier, the inventors designed the preparation study of HFTMS-Al2O3 / SDB hydrophobic catalyst carrier under different HFTMS-Al2O3 dosages, namely, Examples 15 to 18. The micromorphology and static contact angle test results of the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier prepared in Examples 15 to 18 are shown in Table 3 below.

[0098] Preparation process of HFTMS-Al2O3 / SDB hydrophobic catalyst carrier in Examples 15-18: 400g of distilled water, 0.2g of hydroxymethyl cellulose, 0.3g of sodium dodecylbenzene sulfonate and 3g of polyvinyl alcohol 1788 were placed in a reactor, stirred, heated to 75°C, and kept warm for 2h until the powder was completely dissolved to obtain an aqueous phase. 10g of styrene, 10g of divinylbenzene, 11g of dichloroethane, 15g of toluene, 12g of n-heptane, 0.2g of benzoyl peroxide and different amounts of modified nano-Al2O3 were added to a beaker to form an oil phase. The oil phase was slowly added to the water phase, and ultrasonic treatment was performed for 30 minutes. Then the agitator speed was adjusted to 200-300 rpm to form uniform small oil droplets. Nitrogen was introduced and the heating rate was strictly controlled to rise to 70°C. After isothermal reaction for 1 hour, the nitrogen was turned off. The temperature was continued to rise to 89°C and the isothermal reaction was carried out for 1 hour. When the temperature was raised to 90°C, the isothermal reaction was terminated after 5 hours. After filtration, drying and sieving, the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier was obtained.

[0099] The preparation process of Control Example 2 is similar to that of Examples 15 to 18, except that modified nano-Al2O3 is not added, and a SDB hydrophobic catalyst carrier is obtained.

[0100] Table 3 Micromorphology and static contact angle test results of HFTMS-Al2O3 / SDB hydrophobic catalyst carrier in Examples 15 to 18

[0101]

[0102] From the test results of Examples 15 to 18 in Table 3, it can be seen that as the amount of HFTMS-Al2O3 added increases, the sphericity of the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier will change, and may even become an irregular shape. At the same time, the hydrophobic angle of the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier will increase as the amount of HFTMS-Al2O3 added increases, that is, the hydrophobicity is improved. When the amount of HFTMS-Al2O3 added reaches 0.15g (that is, when the weight ratio of styrene, divinylbenzene and modified nano-Al2O3 is 10:10:0.15), the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier exhibits the most outstanding hydrophobic properties.

[0103] Attached Figure 1 Schematic diagram of the static contact angle test of the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier in Example 17 and the SDB hydrophobic catalyst carrier in Comparative Example 2. Figure 1 a is the test picture of SDB hydrophobic catalyst carrier, attached Figure 1 b is the test picture of HFTMS-Al2O3 / SDB hydrophobic catalyst carrier. Figure 1 It can be clearly seen that HFTMS-Al2O3 / SDB hydrophobic catalyst support is better than SDB hydrophobic catalyst support, that is, HFTMS-Al2O3 gives SDB hydrophobic catalyst support good hydrophobic properties.

[0104] Attached Figure 2 Figure 2 is a scanning electron microscope image of the SDB hydrophobic catalyst support and the HFTMS-Al2O3 / SDB hydrophobic catalyst support. Figure 2 a is a scanning electron microscope image of the SDB hydrophobic catalyst support in Comparative Example 2, Figure 2 b is a scanning electron microscope image of the HFTMS-Al2O3 / SDB hydrophobic catalyst support in Example 17. It can be seen that the spherical shape of the HFTMS-Al2O3 / SDB hydrophobic catalyst support is relatively intact and the surface is relatively smooth in macroscopic terms, and the surface of the support has multiple structures and a larger pore size in microscopic terms.

[0105] Taking Examples 16 to 17 and Control Example 2 as examples, the compressive strength test was performed on the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier and the SDB hydrophobic catalyst carrier (7 groups were tested and the average value was taken). The test results are shown in Table 4.

[0106] Table 4 Compressive strength of HFTMS-Al2O3 / SDB hydrophobic catalyst carrier in Examples 16-17

[0107]

[0108] It can be seen from the test results of Examples 16 to 17 in Table 4 that the modified HFTMS-Al2O3 can significantly improve the compressive strength of the SDB hydrophobic catalyst support.

[0109] Taking Example 17 and Comparative Example 2 as examples, the specific surface area, pore volume and pore size of the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier or the SDB hydrophobic catalyst carrier were tested. The test results are shown in Table 5.

[0110] Table 5 Specific surface area, pore volume and pore size test results of HFTMS-Al2O3 / SDB hydrophobic catalyst support in Example 17

[0111]

[0112] It can be seen from the test results of Example 17 in Table 5 that after adding HFTMS-Al2O3, the specific surface area, pore volume and pore size of the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier increased.

[0113] Taking Example 17 and Comparative Example 2 as examples, infrared detection and thermogravimetric analysis were performed on the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier and the SDB hydrophobic catalyst carrier. The test results are shown in the attached Figure 3 and attached Figure 4 As shown in. Among them, Figure 3 The blue curve is the infrared spectrum of the SDB hydrophobic catalyst support, and the orange-red curve is the infrared spectrum of the HFTMS-Al2O3 / SDB hydrophobic catalyst support. Figure 3 It can be seen that 3015.16cm -1 、3075.64cm -1 The corresponding peak is the vibration absorption peak of the CH bond on the benzene ring, 2934.01 cm -1 The corresponding peak is the stretching vibration absorption peak of -CH2; 1640.27cm -1 The corresponding peak is the carbon-carbon double bond stretching vibration absorption peak; 1498.72cm -1 、1455.01cm -1 The corresponding peak is the conjugated double bond stretching vibration peak of the benzene ring skeleton; the absorption peak at 724.06 cm-1 is the carbon chain vibration absorption peak; -1 The corresponding stretching vibration absorption peak of -CF2. From the above analysis, it can be seen that the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier was successfully synthesized in Example 17.

[0114] At the same time, Figure 4The green curve in the middle is the red TG curve of the SDB hydrophobic catalyst support, and the red curve is the TG curve of the HFTMS-Al2O3 / SDB hydrophobic catalyst support. Figure 4 It can be seen that the thermal decomposition temperature of the SDB hydrophobic catalyst carrier is 382.47°C, while the thermal decomposition temperature of the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier is 383.56°C, which means that the addition of HFTMS-Al2O3 has no significant effect on the thermal properties of the SDB hydrophobic catalyst carrier. The inventors analyzed that the possible reason is that HFTMS will gradually decompose at around 380°C, but since the general catalytic reaction temperature is 50~80°C, HFTMS will not decompose at this temperature, so it does not affect the use of the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier.

[0115] Taking Example 17 and Comparative Example 2 as examples, elemental analysis was performed on the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier. The analysis results are as follows: Figure 5 As shown in the figure, it can be seen that the HFTMS-Al2O3 / SDB carrier contains F and Si elements, which means that the HFTMS-Al2O3 / SDB hydrophobic catalyst carrier is successfully prepared in this embodiment.

Claims

1. A method for preparing a nano-aluminum oxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier, It is characterized in that Include: Preparation of modified nano-alumina: 0.35 g of heptadecafluorodecyltrimethoxysilane is used as a modifier, and the modifier and ethanol are mixed in a ratio of 1:100 by volume to obtain a modifier dilution; 1 g of nano-alumina is added to the modifier dilution, the reaction temperature is controlled to be 70°C, the reaction time is 4 hours, and after the reaction is completed, anhydrous ethanol and water are used for washing and drying to obtain modified nano-alumina, and the hydrophobic angle of the modified nano-alumina is 141.76°; Preparation of nano-aluminum trioxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier: 400g of distilled water, 0.2g of hydroxymethyl cellulose, 0.3g of sodium dodecylbenzene sulfonate and 3g of polyvinyl alcohol 1788 are placed in a reactor, stirred, heated to 75°C, and kept warm for 2h until the powder is completely dissolved to obtain an aqueous phase; 10g of styrene, 10g of divinylbenzene, 11g of dichloroethane, 15g of toluene, 12g of n-heptane, 0.2g of benzoyl peroxide and 0.15g of modified nano-aluminum trioxide are added to a beaker to form an oil phase; the oil phase is slowly added to the aqueous phase, first ultrasonically treated for 30min, and then the stirrer speed is adjusted to 200-300rpm to form uniform small oil droplets; nitrogen is introduced The temperature was raised to 70°C at a strictly controlled rate, and the nitrogen was turned off after the isothermal reaction for 1 hour; the temperature was continued to rise to 89°C and the isothermal reaction was continued for 1 hour; when the temperature was raised to 90°C, the isothermal reaction was ended after 5 hours; after filtration, drying and sieving, a nano-aluminum oxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier was obtained; the hydrophobic angle of the nano-aluminum oxide hybrid modified styrene-divinylbenzene copolymer hydrophobic catalyst carrier was 146.94°, the average compressive strength was 56.18N, and the specific surface area was 439.834m 2 / g, pore volume 0.892cm 3 / g, pore size 1.692nm.

Citation Information

Patent Citations

  • Preparation method of size-controllable spherical SDB hydrophobic carrier and Pt / SDB hydrophobic catalyst

    CN113019464A

  • Methods and devices for steam driven carbon dioxide capture

    CA3179546A1

  • Bimetallic catalyst, method of polymerization and bimodal polyolefins therefrom

    CN101166575A

  • Organic / inorganic composite hollow microspheres, and preparation method and application thereof

    CN103387717A

  • Synthetic method for modified biomorphic alumina composite high-oil absorption resin

    CN104004127A