Degradable barrier film with antibacterial property and controllable degradation rate and preparation method thereof

Through the three-layer coextruded film structure design and the use of specific components, the long-term barrier performance and rapid degradation of the degradable barrier film during use are achieved, and the problem of slow degradation rate in the existing technology is solved, and environmentally friendly solutions are provided. plan.

CN115891365BActive Publication Date: 2024-11-12WANHUA CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211322660.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-27
Publication Date
2024-11-12
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

The existing degradable barrier membranes are slow to degrade after use, resulting in environmental pollution.

Method used

The three-layer coextruded film structure is designed, the outer layer is PLA layer, the middle layer is PGA layer, the inner layer is PBAT layer, and the silver ions-loaded mesoporous silica is added to the PBAT layer, and photooxygen degradants and amino acids are used. Components to achieve rapid degradation.

Benefits of technology

Maintain long-term barrier properties during use and quickly degrade after use to avoid environmental pollution and also have antibacterial effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003911024310000141
    Figure BDA0003911024310000141
Patent Text Reader

Abstract

The present invention discloses a degradable barrier film with antibacterial properties and controllable degradation rate and a preparation method thereof, wherein the degradable barrier film comprises a three-layer co-extruded film, which is sequentially a first PLA layer, a second PGA layer, and a third PBAT layer from the outside to the inside; the first PLA layer is a blend made of 100 parts of PLA, 5-100 parts of degradable toughening resin, and 0.1-20 parts of barrier filler, in parts by weight; the second PGA layer is a blend made of 100 parts of PGA, 5-20 parts of degradable toughening resin, 1-10 parts of ultraviolet shielding agent, and 0.5-5 parts of photooxidation degradation agent, in parts by weight; the third PBAT layer is a blend composed of 100 parts of PBAT, 5-30 parts of PLA, and 2-15 parts of antibacterial agent, in parts by weight. The present invention can ensure that the degradable barrier film has long-lasting barrier properties during normal use, and can also ensure its rapid degradation after use, thereby realizing the controllable degradation of the degradable barrier film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for recycling by-products, and in particular to a degradable barrier film with antibacterial properties and controllable degradation rate and a preparation method thereof. Background Art

[0002] High-barrier packaging has high barrier properties against water vapor and oxygen. When applied to food, medical, electronic appliances, metal instruments, military weapons packaging and other fields, it can significantly improve the shelf life or service life of the product. Therefore, the development of high-barrier packaging is of great significance to the national economy and people's livelihood.

[0003] The commonly used high barrier films are generally multilayer films obtained by co-extrusion of base layers such as polypropylene (PP), polyethylene (PE), polyethylene terephthalate (PET) and barrier layers such as nylon (PA), polyvinylidene chloride (PVDC), ethylene-vinyl acetate copolymer (EVOH), polyvinyl alcohol (PVA). However, these materials are non-degradable, and the recycling rate after use as barrier films is less than 20%, and most of the rest are left in the natural environment, causing serious environmental pollution. Therefore, from the perspective of environmental protection and sustainable development, the development of degradable barrier films has become an inevitable development trend.

[0004] Polylactic acid (PLA) is an aliphatic polyester that can be made from starch fermentation products of crops such as corn, and because it can be decomposed into carbon dioxide and water under composting conditions, it is a green material with great application prospects. In addition, because PLA has excellent mechanical strength and good processing properties, it has great application potential in the fields of film materials. However, due to the poor barrier properties of PLA, it is difficult to use it alone as a barrier film. Chinese patent CN107652641A gives PLA film higher barrier properties by blending polyglycolide (PGA) with higher barrier properties with PLA, but because PGA is easily hydrolyzed, the barrier properties of the film will fail in a short period of time, making it difficult to meet the shelf life requirements of food packaging. In order to improve the service life of the degradable barrier film, Chinese patent CN113211920A proposes to prepare a multilayer barrier film of PLA and PGA by a multilayer co-extrusion method, wherein a blend of PLA and butylene adipate-butylene terephthalate copolymer (PBAT) is used as an outer protective layer to isolate the PGA barrier layer from the outside world, thereby reducing the hydrolysis rate of the PGA barrier layer and improving the service life of the barrier film. This type of barrier film is expected to meet the shelf life requirements of food packaging, etc. However, due to the characteristics of the barrier packaging film itself, such as light weight and high recycling cost, this type of PLA barrier film is likely to be left in the environment after use, and the degradation rate of PLA in the natural environment is still relatively slow, and the degradation cycle is generally more than 2 years. Therefore, this type of barrier film that cannot be quickly degraded will also cause environmental pollution. For degradable barrier films containing a PLA layer, an ideal barrier film should be able to maintain high barrier properties and a long service life during use, and quickly degrade in the natural environment after use, so that the barrier film can meet packaging requirements while avoiding environmental pollution. However, there are still huge challenges in how to balance the performance and degradation performance of PLA degradable barrier films. Summary of the invention

[0005] The purpose of the present invention is to provide a barrier film with antibacterial properties and controllable degradation rate to solve the problem that the current PLA degradable barrier film has a slow degradation rate after use and is easy to cause environmental pollution. The special multi-layer film structure design of the barrier film can ensure that it maintains long-term barrier properties during normal use, and can be quickly degraded after use, thereby avoiding environmental pollution problems; and can also play a sterilizing role on packaging.

[0006] Another object of the present invention is to provide a method for preparing a degradable barrier film having antibacterial properties and controllable degradation rate.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] A degradable barrier film with antibacterial properties and controllable degradation rate, the degradable barrier film comprising three co-extruded film layers, which are, from outside to inside, a first PLA layer, a second PGA layer, and a third PBAT layer;

[0009] The first PLA layer is a blend comprising 100 parts of PLA, 5-100 parts of a degradable toughening resin, and 0.1-20 parts of a barrier filler, in parts by weight;

[0010] The second PGA layer is a blend comprising 100 parts of PGA, 5-20 parts of a degradable toughening resin, 1-10 parts of an ultraviolet shielding agent, and 0.5-5 parts of a photo-oxidation degradation agent, in parts by weight;

[0011] The third PBAT layer is a blend consisting of 100 parts of PBAT, 5-30 parts of PLA, and 2-15 parts of antibacterial agent, calculated by weight.

[0012] In some examples, the thickness ratio of the first PLA layer, the second PGA layer, and the third PBAT layer is 1:(0.5-1.5):(0.1-0.5).

[0013] In some examples, the melt index of the blend of the first PLA layer, the second PGA layer, and the third PBAT layer is 1-10 g / 10 min, respectively.

[0014] In some examples, the melt index of PLA is 1-10 g / 10 min at 190° C. and 2.16 kg.

[0015] In some examples, the melt index of PGA is 1-10 g / 10 min at 230° C. and 2.16 kg.

[0016] In some examples, the melt index of PBAT is 1-10 g / 10 min at 190° C., 2.16 kg test conditions.

[0017] In some examples, the degradable toughening resin is selected from at least one of PBAT (butylene adipate-butylene terephthalate copolymer), PBS (polybutylene succinate), PHA (polyhydroxyalkanoate), PCL (polycaprolactone), and PPC (polymethyl ethylene carbonate);

[0018] Preferably, the barrier filler is at least one of montmorillonite, hydrotalcite, mica and kaolin;

[0019] Preferably, the ultraviolet shielding agent is one or both of titanium dioxide and zinc oxide;

[0020] Preferably, the photo-oxidation degradation agent is at least one of iron stearate, iron acetylacetonate and benzophenone.

[0021] In some examples, the antibacterial agent is mesoporous silica loaded with silver ions and grafted with a terpolymer of citric acid-amino acid-hydroxyalkyl acid;

[0022] Preferably, the antibacterial agent is prepared by the following method:

[0023] 1) adding mesoporous silica to an aqueous solution containing silver ions, shaking and stirring for 0.5-2.5 hours, filtering and drying to obtain mesoporous silica loaded with silver ions;

[0024] Preferably, the aqueous solution containing silver ions has a silver ion concentration of 200-1000 mg / L;

[0025] Preferably, the amount of mesoporous silica added is 1-5% of the mass of the aqueous solution containing silver ions;

[0026] 2) adding the obtained silver ion-loaded mesoporous silica, citric acid, and esterification catalyst into a reactor, stirring and reacting for 0.5-2h under an inert atmosphere at a reaction temperature of 160-190° C.; then adding amino acids and hydroxyalkyl acids to continue the reaction for 3-6h, dehydrating and drying to prepare an antibacterial agent;

[0027] Preferably, the mass ratio of mesoporous silica, citric acid, amino acid and hydroxyalkyl acid is 100:(5-15):(20-50):(50-100).

[0028] Preferably, the aqueous solution containing silver ions is an aqueous silver nitrate solution.

[0029] In some examples, the mesoporous silica has a particle size of 0.5-3 μm, a pore size of 10-40 nm, and a hydroxyl content of 2-4% by molar amount.

[0030] In some examples, the esterification catalyst is one or more of toluenesulfonic acid, benzenesulfonic acid, and tetrabutyl titanate;

[0031] Preferably, the added amount of the esterification catalyst is 0.1-1% of the mass of the mesoporous silica.

[0032] In some examples, the amino acid is one or more of ornithine, glycine, glutamine, and asparagine.

[0033] In some examples, the hydroxyalkyl acid is one or more of 3-hydroxyhexanoic acid, 3-hydroxyoctanoic acid, 3-hydroxydecanoic acid, 3-hydroxydodecanoic acid, and 3-hydroxytetradecanoic acid.

[0034] The present invention also provides a method for preparing the degradable barrier film as described above, characterized in that it comprises the following steps:

[0035] The raw materials of the first PLA layer, the second PGA layer, and the third PBAT layer are melt-extruded in a twin-screw extruder according to the ratio to obtain a three-layer blend, and then a multi-layer co-extrusion device is used to perform multi-layer co-extrusion molding at 180-230° C. according to the filler sequence of the first PLA layer, the second PGA layer, and the third PBAT layer to obtain the degradable barrier film;

[0036] Preferably, the melt extrusion temperatures for preparing the first PLA layer, the second PGA layer, and the third PBAT layer are 160-190° C., 190-230° C., and 150-170° C., respectively.

[0037] As a specific scheme that can be implemented, the melt extrusion temperature for preparing the first PLA layer is, for example, 160°C, 180°C, 190°C, 190°C, 190°C, 190°C, 190°C, 180°C, and the main engine speed is 300 rpm.

[0038] As a specific scheme that can be implemented, the melt extrusion temperature for preparing the second PGA layer is, for example, 190°C, 210°C, 230°C, 230°C, 230°C, 230°C, 230°C, 210°C, and the main engine speed is 300 rpm.

[0039] As a specific scheme that can be implemented, the melt extrusion temperature for preparing the third PBAT layer is, for example, 150°C, 160°C, 170°C, 170°C, 170°C, 170°C, 170°C, 170°C, 160°C, and the main engine speed is 300 rpm.

[0040] As a specific scheme that can be implemented, the melting temperature of the multi-layer co-extrusion molding is, for example, 190°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, and the main engine speed is 300 rpm.

[0041] The degradable barrier film provided by the present invention is composed of a first PLA layer, a second PGA layer and a third PBAT layer from the outside to the inside. The second PGA layer mainly plays a barrier role; the first PLA layer can block the direct contact between the PGA barrier layer and the outside world, reduce the degradation rate of the PGA barrier layer, and thus ensure that the degradable barrier film has a long service life during normal use as a packaging bag. In addition, in the third PBAT layer, the mesoporous silica loaded with silver ions and grafted with a terpolymer of citric acid-amino acid-hydroxyalkyl acid is added. The terpolymer can not only improve the dispersion of mesoporous silica in PBAT, but also play a sustained-release role for silver ions. Therefore, it can be ensured that the barrier film releases silver ion antibacterial agents uniformly and slowly into the packaging during normal use, thereby ensuring that the barrier film has long-lasting antibacterial properties; and the citric acid unit in the terpolymer grafted on the mesoporous silica has strong water absorption. When the barrier film is opened after use, the innermost PBAT layer can quickly absorb moisture in the environment, thereby promoting the hydrolysis and degradation of the terpolymer grafted on the mesoporous silica. At the same time, since the terpolymer contains amino acid units, it can be quickly degraded under the action of proteases secreted by microorganisms, so that the mesoporous silica quickly falls off from the third PBAT layer, thereby forming a large number of hole defects on the third PBAT layer. External water vapor, microorganisms and oxygen come into contact with the second PGA layer through these holes, causing the second PGA layer to degrade rapidly. After the second PGA layer degrades, the small molecule photo-oxidation degradation agent in the layer diffuses to the second PBAT layer and the first PLA layer, catalyzing the rapid photo-oxidation degradation of the PBAT and PLA layers to form low molecular weight degradation products, thereby significantly increasing the degradation rate of the degradable barrier film in the environment.

[0042] Therefore, the present invention can ensure that the degradable barrier film has a long-lasting barrier performance during normal use, and can also ensure its rapid degradation after use, thereby achieving controllable degradation of the degradable barrier film. DETAILED DESCRIPTION

[0043] The present invention is further described below by means of specific examples. The examples described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.

[0044] The raw materials used in the following specific embodiments are all purchased from commercially available finished products. Among them, the PLA brand is Total Corbivir LX-175, with a melt index of 3g / 10min; the PBAT brand is Xinjiang Tunhe 801T, with a melt index of 2.5g / 10min; the PGA brand is Kureha Chemical Kuredux, with a melt index of 3g / 10min; the PBS brand is PTT91PM, with a melt index of 5g / 10min; the PPC brand is Zhongke Jinlong T2, with a melt index of 7g / 10min; the PHA brand is PHBV-1000P, with a melt index of 20g / 10min; and the mesoporous silica is purchased from Zhongke Leiming Technology Co., Ltd.

[0045] The test method involved in the following embodiments of the present invention is as follows:

[0046] (1) Antibacterial rate: The test was conducted in accordance with GB / T 31402-2015 standard, and the experimental bacteria was Escherichia coli.

[0047] (2) Tensile properties: The elongation at break was tested according to ASTM D256-1997.

[0048] (3) Water vapor transmission rate: tested in accordance with GB / T 26253 standard.

[0049] (4) Oxygen permeability: tested in accordance with GB / T 19789 standard.

[0050] (5) Degradation rate test: The barrier film is placed in a simulated environment and the sample is subjected to a UV aging test. Test conditions: LUV UV exposure, irradiance 0.8W / m 2 , temperature (40±1)℃, spray the sample every 90min, each spray time is 30min, and record the degradation cycle of the sample. Among them, the degradation rate A means the degradation cycle is 15-20 days, B means the degradation cycle is 30-60 days, and C means no degradation within 60 days.

[0051] The following examples 1-8 are prepared to provide different antimicrobial agents:

[0052] [Preparation Example 1]

[0053] 100 g of mesoporous silica (particle size 0.5 μm, pore size 10 nm, hydroxyl molar content 3%) was added to 2000 g of 500 mg / L silver nitrate aqueous solution, shaken and stirred for 0.5 h, filtered and dried to obtain mesoporous silica loaded with silver ions;

[0054] The obtained silver ion-loaded mesoporous silica, 5 g of citric acid, and 0.3 g of benzenesulfonic acid catalyst were added to a reactor, and the reaction was stirred for 1.5 h under a nitrogen atmosphere at a reaction temperature of 180°C; then 20 g of ornithine and 50 g of 3-hydroxyhexanoic acid were added and the reaction was continued for 5 h, and the antibacterial agent A was prepared by dehydration and drying.

[0055] [Preparation Example 2]

[0056] 100 g of mesoporous silica (particle size 1.5 μm, pore size 25 nm, hydroxyl molar content 2%) was added to 6000 g of 500 mg / L silver nitrate aqueous solution, shaken and stirred for 1.5 h, filtered and dried to obtain mesoporous silica loaded with silver ions;

[0057] The obtained silver ion-loaded mesoporous silica, 10 g of citric acid, and 0.5 g of tetrabutyl titanate catalyst were added to a reactor, and the reaction was stirred for 1 h under a nitrogen atmosphere at a reaction temperature of 185°C; then 40 g of glycine and 80 g of 3-hydroxydodecanoic acid were added and the reaction was continued for 6 h, and the antibacterial agent B was prepared by dehydration and drying.

[0058] [Preparation Example 3]

[0059] 100 g of mesoporous silica (particle size 3 μm, pore size 40 nm, hydroxyl molar content 2%) was added to 10000 g of 500 mg / L silver nitrate aqueous solution, shaken and stirred for 2.5 h, filtered and dried to obtain mesoporous silica loaded with silver ions;

[0060] The obtained silver ion-loaded mesoporous silica, 15 g of citric acid, and 0.8 g of tetrabutyl titanate catalyst were added to a reactor, and the reaction was stirred for 1.5 h under a nitrogen atmosphere at a reaction temperature of 180°C; then 50 g of glutamine and 70 g of 3-hydroxyoctanoic acid were added and the reaction was continued for 5 h, and the mixture was dehydrated and dried to prepare antibacterial agent C.

[0061] [Preparation Example 4]

[0062] 100 g of mesoporous silica (particle size 1.5 μm, pore size 25 nm, hydroxyl molar content 3%) was added to 6000 g of 500 mg / L silver nitrate aqueous solution, shaken and stirred for 2.5 h, filtered and dried to obtain mesoporous silica loaded with silver ions;

[0063] The obtained silver ion-loaded mesoporous silica, 15 g of citric acid, and 1 g of tetrabutyl titanate catalyst were added to a reactor, and the mixture was stirred and reacted for 2 h under a nitrogen atmosphere at a reaction temperature of 175°C; then 50 g of asparagine and 100 g of 3-hydroxydodecanoic acid were added and the reaction was continued for 5 h, and the mixture was dehydrated and dried to prepare antibacterial agent D.

[0064] [Preparation Example 5]

[0065] 100 g of mesoporous silica (particle size 2 μm, pore size 25 nm, hydroxyl molar content 2%) was added to 8000 g of 500 mg / L silver nitrate aqueous solution, shaken and stirred for 2.5 h, filtered and dried to obtain mesoporous silica loaded with silver ions;

[0066] The obtained silver ion-loaded mesoporous silica, 12 g of citric acid, and 1 g of toluenesulfonic acid catalyst were added to a reactor, and the reaction was stirred for 1.5 h under a nitrogen atmosphere at a reaction temperature of 180°C; then 35 g of ornithine and 90 g of 3-hydroxytetradecanoic acid were added and the reaction was continued for 4 h, and the antibacterial agent E was prepared by dehydration and drying.

[0067] [Preparation Example 6]

[0068] Antimicrobial agent F was prepared in substantially the same manner as in Preparation Example 1, except that citric acid was not added.

[0069] [Preparation Example 7]

[0070] Antimicrobial Agent G was prepared in substantially the same manner as in Preparation Example 1, except that no ornithine was added.

[0071] [Preparation Example 8]

[0072] Antimicrobial Agent I was prepared in substantially the same manner as in Preparation Example 1, except that 3-hydroxyhexanoic acid was not added.

[0073] [Preparation Example 9]

[0074] 100 g of mesoporous silica (particle size 0.5 μm, pore size 10 nm, hydroxyl molar content 3%) was added to 2000 g, 500 mg / L silver nitrate aqueous solution, shaken and stirred for 0.5 h, filtered and dried to obtain mesoporous silica loaded with silver ions as antibacterial agent H.

[0075] The following Examples 1-5 are used to prepare different multilayer barrier films:

[0076] [Example 1]

[0077] 100 g of PLA, 10 g of PBAT and 1 g of montmorillonite were melt-extruded in a twin-screw extruder at melt temperatures of 160°C, 180°C, 190°C, 190°C, 190°C, 190°C, 190°C, 180°C, respectively, and the main engine speed was 300 rpm. The mixture was cooled and granulated to obtain a first PLA layer blend.

[0078] 100 g of PGA, 5 g of PBAT, 1 g of titanium dioxide and 1 g of iron stearate were melt-extruded in a twin-screw extruder. The melting temperatures were 190°C, 210°C, 230°C, 230°C, 230°C, 230°C, 230°C, 210°C, respectively. The main engine speed was 300 rpm. The mixture was cooled and granulated to obtain a second PGA layer blend.

[0079] 100 g PBAT, 10 g PLA and 3 g antibacterial agent A were melt-extruded in a twin-screw extruder. The melt temperatures were 170 ° C, 150 ° C, 160 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 160 ° C, and the main engine speed was 300 rpm. Then cooled and granulated to obtain a third PBAT layer blend.

[0080] According to the thickness ratio of 1:0.5:0.1, the first PLA layer, the second PGA layer and the third PBAT layer blend were sequentially fed into the multi-layer co-extrusion equipment, and multi-layer co-extrusion molding was carried out under the conditions of segmented temperatures: 190°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, and a main engine speed of 300 rpm to obtain a degradable barrier film.

[0081] [Example 2]

[0082] 100 g of PLA, 30 g of PBAT and 3 g of hydrotalcite were melt-extruded in a twin-screw extruder at melt temperatures of 160°C, 180°C, 190°C, 190°C, 190°C, 190°C, 190°C, 180°C, and a main engine speed of 300 rpm. The mixture was cooled and granulated to obtain a first PLA layer blend.

[0083] 100 g of PGA, 10 g of PBAT, 5 g of titanium dioxide and 2 g of iron stearate were melt-extruded in a twin-screw extruder. The melting temperatures were 190°C, 210°C, 230°C, 230°C, 230°C, 230°C, 230°C, 210°C, respectively. The main engine speed was 300 rpm. The mixture was cooled and granulated to obtain a second PGA layer blend.

[0084] 100 g PBAT, 15 g PLA and 5 g antibacterial agent B were melt-extruded in a twin-screw extruder. The melt temperatures were 170 ° C, 150 ° C, 160 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 160 ° C, and the main engine speed was 300 rpm. Then cooled and granulated to obtain a third PBAT layer blend.

[0085] According to the thickness ratio of 1:0.8:0.3, the first PLA layer, the second PGA layer and the third PBAT layer blend were sequentially fed into the multi-layer co-extrusion equipment, and multi-layer co-extrusion molding was carried out under the conditions of segmented temperatures: 190°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, and a main engine speed of 300 rpm to obtain a degradable barrier film.

[0086] [Example 3]

[0087] 100 g of PLA, 50 g of PBS and 10 g of hydrotalcite were melt-extruded in a twin-screw extruder at melt temperatures of 160° C., 180° C., 190° C., 190° C., 190° C., 190° C., 190° C., 180° C., respectively, and the main engine speed was 300 rpm. The mixture was cooled and granulated to obtain a first PLA layer blend.

[0088] Take 100g PGA, 15g PBS, 5g zinc oxide and 5g iron stearate and melt extrude in a twin-screw extruder. The melting temperatures are 190°C, 210°C, 230°C, 230°C, 230°C, 230°C, 230°C, 210°C, respectively. The main engine speed is 300 rpm. Then cool and granulate to obtain a second PGA layer blend.

[0089] 100 g PBAT, 20 g PLA and 8 g antibacterial agent C were melt-extruded in a twin-screw extruder. The melt temperatures were 170 ° C, 150 ° C, 160 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 160 ° C, and the main engine speed was 300 rpm. Then cooled and granulated to obtain a third PBAT layer blend.

[0090] According to the thickness ratio of 1:1:0.3, the first PLA layer, the second PGA layer and the third PBAT layer blend were sequentially fed into the multi-layer co-extrusion equipment, and multi-layer co-extrusion molding was carried out under the conditions of segmented temperatures: 190°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, and a main engine speed of 300 rpm to obtain a degradable barrier film.

[0091] [Example 4]

[0092] 100 g of PLA, 80 g of PPC and 15 g of hydrotalcite were melt-extruded in a twin-screw extruder at melt temperatures of 160° C., 180° C., 190° C., 190° C., 190° C., 190° C., 190° C., 180° C., respectively, and the main engine speed was 300 rpm. The mixture was cooled and granulated to obtain a first PLA layer blend.

[0093] Take 100g PGA, 20g PPC, 8g zinc oxide and 5g ferric acetylacetonate and melt extrude in a twin-screw extruder. The melting temperatures are 190°C, 210°C, 230°C, 230°C, 230°C, 230°C, 230°C, 210°C, respectively. The main engine speed is 300 rpm. Then cool and granulate to obtain a second PGA layer blend.

[0094] 100 g PBAT, 30 g PLA and 10 g antibacterial agent D were melt-extruded in a twin-screw extruder. The melt temperatures were 170 ° C, 150 ° C, 160 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 160 ° C, and the main engine speed was 300 rpm. Then cooled and granulated to obtain a third PBAT layer blend.

[0095] According to the thickness ratio of 1:1.2:0.5, the first PLA layer, the second PGA layer and the third PBAT layer blend were sequentially fed into the multi-layer co-extrusion equipment, and multi-layer co-extrusion molding was carried out under the conditions of segmented temperatures: 190°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, and a main engine speed of 300 rpm to obtain a degradable barrier film.

[0096] [Example 5]

[0097] 100 g PLA, 100 g PHA and 15 g kaolin were melt-extruded in a twin-screw extruder at melt temperatures of 160° C., 180° C., 190° C., 190° C., 190° C., 190° C., 190° C., 180° C., respectively. The main engine speed was 300 rpm. The mixture was cooled and granulated to obtain a first PLA layer blend.

[0098] 100 g of PGA, 20 g of PHA, 10 g of zinc oxide and 5 g of benzophenone were melt-extruded in a twin-screw extruder. The melt temperatures were 190°C, 210°C, 230°C, 230°C, 230°C, 230°C, 230°C, 210°C, respectively. The main engine speed was 300 rpm. The mixture was cooled and granulated to obtain a second PGA layer blend.

[0099] 100 g PBAT, 30 g PLA and 12 g antibacterial agent E were melt-extruded in a twin-screw extruder. The melt temperatures were 170 ° C, 150 ° C, 160 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 170 ° C, 160 ° C, and the main engine speed was 300 rpm. Then cooled and granulated to obtain a third PBAT layer blend.

[0100] According to the thickness ratio of 1:1.5:0.5, the first PLA layer, the second PGA layer and the third PBAT layer blend were sequentially fed into the multi-layer co-extrusion equipment, and multi-layer co-extrusion molding was carried out under the conditions of segmented temperatures: 190°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C, and a main engine speed of 300 rpm to obtain a degradable barrier film.

[0101] [Comparative Example 1]

[0102] A degradable barrier film was prepared in substantially the same manner as in Example 1, except that the antimicrobial agent A was replaced by the antimicrobial agent F.

[0103] [Comparative Example 2]

[0104] A degradable barrier film was prepared in substantially the same manner as in Example 1, except that the antimicrobial agent A was replaced by the antimicrobial agent G.

[0105] [Comparative Example 3]

[0106] A degradable barrier film was prepared in substantially the same manner as in Example 1, except that the antimicrobial agent A was replaced by the antimicrobial agent H.

[0107] [Comparative Example 4]

[0108] A degradable barrier film was prepared in substantially the same manner as in Example 1, except that antimicrobial agent A was replaced by antimicrobial agent I.

[0109] [Comparative Example 5]

[0110] The degradable barrier film was prepared in substantially the same manner as in Example 1, except that the antimicrobial agent A was not added.

[0111] [Comparative Example 6]

[0112] The degradable barrier film was prepared in substantially the same manner as in Example 1, except that no iron stearate was added when preparing the second PGA layer blend.

[0113] The degradable barrier films prepared in the embodiments and comparative examples were subjected to various performance tests shown in Table 1, and the test results are as follows:

[0114] Table 1. Performance test of degradable barrier film

[0115]

[0116] From the above comparative data, it can be seen that the present invention can ensure that the degradable barrier film has long-lasting barrier properties during normal use while also having certain antibacterial properties and ensuring that it degrades rapidly after use, thereby achieving controllable degradation of the degradable barrier film and broadening its application field.

[0117] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.

Claims

1. A degradable barrier film with antibacterial properties and controllable degradation rate, characterized in that: The degradable barrier film comprises three co-extruded film layers, which are, from the outside to the inside, a first PLA layer, a second PGA layer, and a third PBAT layer; The first PLA layer is a blend comprising 100 parts of PLA, 5-100 parts of a degradable toughening resin, and 0.1-20 parts of a barrier filler, in parts by weight; The second PGA layer is a blend comprising 100 parts of PGA, 5-20 parts of a degradable toughening resin, 1-10 parts of an ultraviolet shielding agent, and 0.5-5 parts of a photo-oxidation degradation agent, in parts by weight; The third PBAT layer is a blend consisting of 100 parts of PBAT, 5-30 parts of PLA, and 2-15 parts of antibacterial agent, in parts by weight; The antibacterial agent is mesoporous silica loaded with silver ions and grafted with a terpolymer of citric acid-amino acid-hydroxyalkyl acid; The antibacterial agent is prepared by the following method: 1) adding mesoporous silica to an aqueous solution containing silver ions, shaking and stirring for 0.5-2.5 hours, filtering and drying to obtain mesoporous silica loaded with silver ions; 2) adding the obtained silver ion-loaded mesoporous silica, citric acid, and esterification catalyst into a reactor, stirring and reacting for 0.5-2 hours under an inert atmosphere at a reaction temperature of 160-190° C.; then adding amino acids and hydroxyalkyl acids and continuing the reaction for 3-6 hours, dehydrating and drying to prepare an antibacterial agent.

2. The degradable barrier film with antibacterial properties and controllable degradation rate according to claim 1, characterized in that: The thickness ratio of the first PLA layer, the second PGA layer, and the third PBAT layer is 1:(0.5-1.5):(0.1-0.5).

3. The degradable barrier film with antibacterial properties and controllable degradation rate according to claim 2, characterized in that: The melt indexes of the blends of the first PLA layer, the second PGA layer and the third PBAT layer are 1-10 g / 10 min respectively.

4. The degradable barrier film with antibacterial properties and controllable degradation rate according to any one of claims 1 to 3, characterized in that: The degradable toughening resin is selected from at least one of PBAT, PBS, PHA, PCL and PPC.

5. The degradable barrier film with antibacterial properties and controllable degradation rate according to claim 4, characterized in that: The barrier filler is at least one of montmorillonite, hydrotalcite, mica and kaolin.

6. The degradable barrier film with antibacterial properties and controllable degradation rate according to claim 4, characterized in that: The ultraviolet shielding agent is one or both of titanium dioxide and zinc oxide.

7. The degradable barrier film with antibacterial properties and controllable degradation rate according to claim 4, characterized in that: The photo-oxidation degradation agent is at least one of iron stearate, iron acetylacetonate and benzophenone.

8. The degradable barrier film with antibacterial properties and controllable degradation rate according to any one of claims 1 to 3, characterized in that: In the preparation method of the antibacterial agent, the silver ion concentration in the aqueous solution containing silver ions is 200-1000 mg / L.

9. The degradable barrier film with antibacterial properties and controllable degradation rate according to any one of claims 1 to 3, characterized in that: In the preparation method of the antibacterial agent, the added amount of mesoporous silica is 1-5% of the mass of the aqueous solution containing silver ions.

10. The degradable barrier film with antibacterial properties and controllable degradation rate according to any one of claims 1 to 3, characterized in that: In the preparation method of the antibacterial agent, the mass ratio of mesoporous silica, citric acid, amino acid and hydroxyalkyl acid is 100:(5-15):(20-50):(50-100).

11. The degradable barrier film with antibacterial properties and controllable degradation rate according to claim 1, characterized in that: In the preparation method of the antibacterial agent, the particle size of the mesoporous silica is 0.5-3 μm, the pore size is 10-40 nm, and the hydroxyl content thereof is 2-4% in terms of molar amount.

12. The degradable barrier film with antibacterial properties and controllable degradation rate according to claim 1, characterized in that: In the method for preparing the antibacterial agent, the esterification catalyst is one or more of toluenesulfonic acid, benzenesulfonic acid, and tetrabutyl titanate.

13. The degradable barrier film with antibacterial properties and controllable degradation rate according to claim 12, characterized in that: In the preparation method of the antibacterial agent, the added amount of the esterification catalyst is 0.1-1% of the mass of the mesoporous silica.

14. The degradable barrier film with antibacterial properties and controllable degradation rate according to any one of claims 1 to 3, characterized in that: The amino acid is one or more of ornithine, glycine, glutamine and asparagine.

15. The degradable barrier film with antibacterial properties and controllable degradation rate according to claim 14, characterized in that: The hydroxyalkyl acid is one or more of 3-hydroxyhexanoic acid, 3-hydroxyoctanoic acid, 3-hydroxydecanoic acid, 3-hydroxydodecanoic acid, and 3-hydroxytetradecanoic acid.

16. A method for preparing a degradable barrier film according to any one of claims 1 to 15, characterized in that: The following steps are involved: The raw materials of the first PLA layer, the second PGA layer, and the third PBAT layer are melt-extruded in a twin-screw extruder according to the ratio to obtain a three-layer blend, and then a multi-layer co-extrusion device is used to perform multi-layer co-extrusion molding at 180-230° C. in the order of the fillers of the first PLA layer, the second PGA layer, and the third PBAT layer to obtain the degradable barrier film.