A ternary composite photocatalyst and its preparation method and application
The ZnO/ZnFe2O4/CuO ternary composite photocatalyst is prepared by electrospinning, which solves the problems of low efficiency and difficult preparation of traditional photocatalytic materials, achieves efficient visible light catalysis and a simple preparation process, and is suitable for wastewater treatment.
Patent Information
- Application Number
- CN202211504949.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-28
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-11-28
AI Technical Summary
Traditional photocatalytic materials have poor photocatalytic efficiency and are difficult to prepare. In particular, ZnO/ZnFe2O4/CuO ternary composite materials lack effective improvements in visible light catalysis.
ZnO/ZnFe2O4/CuO ternary composite photocatalyst is prepared by electrospinning method. By preparing two spinning liquids and spinning under high pressure, a composite structure of nanoribbons and nanospheres is obtained. The ternary composite photocatalyst is obtained by calcination to optimize the quality. ratio and calcination conditions to improve photocatalytic activity.
It achieves a higher photoresponse range and photocatalytic activity, and the degradation rate of rhodamine B reaches more than 93%. It simplifies the preparation process, reduces the cost, and is suitable for the treatment of wastewater organic pollutants.
Smart Images

Figure CN115920906B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalytic materials, and relates to a photocatalyst and a preparation method and application thereof, and specifically relates to a ternary composite photocatalyst and a preparation method and application thereof. Background Art
[0002] With the rapid development of industry and the extensive use of fossil fuels, the world's economic development has been accelerating, but it has also led to the generation and release of a large number of pollutants in the ecosystem, which have had a serious impact on human health and the environment. Common methods for removing environmental pollutants generally include physical methods, biological methods, etc. In recent years, the Fenton process, one of the advanced oxidation techniques (APOs) with better degradation effects, has received more and more attention. In the Fenton process, Fe 2+ It reacts with H2O2 to produce hydroxyl radicals (·OH) with strong oxidizing properties to oxidize and remove organic pollutants in wastewater. However, the above method is prone to produce a large amount of sludge during the reaction process and easily makes the substance colored.
[0003] ZnO is a commonly used wide bandgap semiconductor material in photocatalysis. It can show excellent photocatalytic efficiency under ultraviolet light irradiation, but its absorption capacity of visible light is low, and its application under visible light is limited. By coupling the wide bandgap material ZnO with low bandgap materials such as spinel ferrite, the absorption capacity of visible light can be improved, and the visible light photocatalytic effect can be enhanced. However, there are currently no reports in the industry on ZnO / ZnFe2O4 / CuO ternary composite materials that can improve visible light catalytic effect. In addition, conventional composite photocatalytic degradation materials have the problems of complex preparation methods and poor product photocatalytic efficiency. Summary of the invention
[0004] To this end, the technical problem to be solved by the present invention is that traditional photocatalytic materials have poor photocatalytic efficiency and are difficult to prepare, thereby proposing a ternary composite photocatalyst with excellent photocatalytic effect and easy preparation, as well as its preparation method and application.
[0005] In order to solve the above technical problems, the technical solution of the present invention is:
[0006] A first aspect of the present invention provides a ternary composite photocatalyst, which is a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst, wherein the mass ratio of ZnO, ZnFe2O4 and CuO is 1-5:1-8:1-5.
[0007] Preferably, the ZnO / ZnFe2O4 / CuO ternary composite photocatalyst is a composite structure of nanobelts and nanospheres.
[0008] Preferably, the mass ratio of ZnO, ZnFe2O4 and CuO is 1:1:1.
[0009] The second aspect of the present invention provides a method for preparing the ternary composite catalyst, which comprises the following steps:
[0010] S1. preparing a first spinning solution: uniformly mixing zinc acetate, an organic solvent and a surfactant in a mass ratio of 8-10:16-18:72-76 to obtain a transparent first spinning solution;
[0011] S2. preparing a second spinning solution: uniformly mixing a nitrate, an organic solvent and a surfactant in a mass ratio of 7-10:14-16:74-79 to obtain a second spinning solution, wherein the nitrate comprises ferric nitrate and copper nitrate, and the mass ratio of the ferric nitrate to the copper nitrate is 1.5-4:1;
[0012] S3, electrospinning: injecting the first spinning solution and the second spinning solution into a syringe respectively, and electrospinning at a voltage of 12-18 kV to obtain an electrospinning product;
[0013] S4, calcining the electrospinning product to obtain the ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0014] Preferably, in step S3, each of the syringes is connected to a needle having a bending angle of 20-30°, and a receiving net for receiving the electrospinning product is provided on one side of the syringe, and the distance between the needle and the receiving net is 12-15 cm.
[0015] Preferably, in step S3, the flow rate ratio of the first spinning solution to the second spinning solution is 1:1-3:1.
[0016] Preferably, the organic solvent is N,N-dimethylformamide, and the surfactant is polyvinyl pyrrolidone.
[0017] Preferably, in step S4, the calcination temperature is 650-800° C., and during the calcination process, the holding time is 3-6 hours.
[0018] Preferably, in the step S1, the first spinning solution is prepared by mixing zinc acetate and an organic solution in proportion, magnetically stirring for 20-40 minutes, and then adding the surfactant in proportion, and magnetically stirring for 8-10 hours; in the step S2, the second spinning solution is prepared by mixing nitrate and an organic solution in proportion, magnetically stirring for 20-40 minutes, and then adding the surfactant in proportion, and magnetically stirring for 8-10 hours.
[0019] The third aspect of the present invention provides an application of the ternary composite photocatalyst in a wastewater organic pollutant treatment agent.
[0020] The above technical solution of the present invention has the following advantages compared with the prior art:
[0021] (1) The ternary composite photocatalyst provided by the present invention is a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst, wherein the mass ratio of ZnO, ZnFe2O4, and CuO is 1-5:1-8:1-5. Compared with the traditional ZnO photocatalyst, the ternary composite photocatalyst provided by the present invention is a heterogeneous photo-Fenton photocatalyst, which has a wider light response range, a higher utilization rate of sunlight, and a higher photocatalytic activity. In the case of adding hydrogen peroxide, the degradation rate of rhodamine B by the ternary composite photocatalyst can reach more than 93%. At the same time, the ternary composite photocatalyst can be recycled, which reduces the use cost of the photocatalyst.
[0022] (2) The method for preparing a ternary composite photocatalyst provided by the present invention only requires the preparation of two spinning solutions to obtain a ternary composite photocatalyst. Compared with the traditional electrospinning method, the steps are simpler and the preparation efficiency is higher. The obtained ternary composite photocatalyst has higher photocatalytic performance and is particularly suitable as a treatment agent for organic pollutants in wastewater. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein
[0024] Figure 1 is the XRD spectrum of the ternary composite photocatalyst in Example 1, Example 5 and Example 6 of the present invention;
[0025] Figure 2 (a) is a scanning electron microscope image of the ZnO / ZnFe2O4 / CuO ternary composite material before calcination in Example 5 of the present invention;
[0026] Figure 2 (b) is a scanning electron microscope image of the ZnO / ZnFe2O4 / CuO ternary composite material after calcination in Example 5 of the present invention;
[0027] Figure 3 is the UV-visible absorption spectra of the ternary composite photocatalysts in Examples 1, 5 and 6 of the present invention;
[0028] Figure 4 is a photoluminescence spectrum of the ternary composite photocatalyst in Example 1, Example 5 and Example 6 of the present invention;
[0029] Figure 5 is a degradation curve diagram of Rhodamine B by the ternary composite photocatalyst in Examples 1, 5 and 6 of the present invention;
[0030] Figure 6 (a) is a graph showing the degradation of Rhodamine B by the ternary composite photocatalyst after adding hydrogen peroxide in Example 1 of the present invention;
[0031] Figure 6 (b) is a graph showing the degradation of Rhodamine B by the ternary composite photocatalyst after adding hydrogen peroxide in Example 5 of the present invention;
[0032] Figure 7 It is a bar graph of free radical capture of the ternary composite photocatalyst in Example 1 of the present invention after adding hydrogen peroxide under photo-Fenton conditions. DETAILED DESCRIPTION
[0033] Example 1
[0034] This embodiment provides a ternary composite photocatalyst, which is composed of ZnO, ZnFe2O4, and CuO, namely, a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0035] The ternary composite photocatalyst provided in this embodiment is prepared by the following steps:
[0036] S1. Prepare the first spinning solution: weigh 2.0012 g zinc acetate and dissolve it in 3.6007 g N,N-dimethylformamide (DMF) organic solvent, stir it magnetically for 20 minutes, then slowly add 3.6007 g surfactant polyvinyl pyrrolidone (PVP), and continue to stir it magnetically for 8-10 hours to form a uniform and transparent first spinning solution.
[0037] S2. Prepare the second spinning solution: weigh 1.4425 g of ferric nitrate and 0.5587 g of copper nitrate, dissolve them in 14.8395 g of organic solvent DMF (wherein the molar ratio of iron element to copper element is 2:1), stir magnetically for 20 min, then slowly add 3.2230 g of surfactant PVP, and continue magnetic stirring for 8-10 h until a uniform second spinning solution is formed.
[0038] The purity and sources of the reagents used in the above steps are as follows: ferric nitrate [Fe(NO3)3·9H2O], analytical grade, Sinopharm Chemical Industry Co., Ltd.; copper nitrate [Cu(NO3)3·3H2O], analytical grade, Xilong Chemical Industry Co., Ltd.; zinc acetate [Zn(CH3COO)2], analytical grade, Xilong Chemical Industry Co., Ltd.; polyvinylpyrrolidone (PVP, Mw=90000), analytical grade, Tianjin Guangfu Technology Development Co., Ltd.; N,N-dimethylformamide (DMF), analytical grade, Tianjin Guangfu Technology Development Co., Ltd.
[0039] S3, electrospinning, bend two 8# stainless steel needles at an angle of 30° respectively, and put a plastic spray gun head on the outside of the two stainless steel needles with needle tips closely arranged side by side, so that the two stainless steel needles are in the middle of the plastic spray gun head, and connect a copper wire to each of the two needles. Inject the first spinning solution and the second spinning solution into a 5ml syringe respectively, connect the syringe to the plastic spray gun head, set an iron receiving net for receiving the electrospinning product on one side of the syringe, the distance between the receiving net and the needle is 15cm, tilt the nozzle downward by 15°, and connect the copper wire in the needle to a 14kV high-voltage power supply, control the flow rate ratio of the first spinning solution to the second spinning solution to 3:1, keep the air humidity at 45%, and collect the electrospinning products received on the iron receiving net.
[0040] S4. Calcine the electrospinning product. Place the electrospinning product in a muffle furnace, heat it to 650°C at a heating rate of 2°C / min, and keep it warm for 3 hours. After the temperature in the muffle furnace drops to room temperature, take out the sample to obtain a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0041] Example 2
[0042] This embodiment provides a ternary composite photocatalyst, which is composed of ZnO, ZnFe2O4, and CuO, namely, a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0043] The ternary composite photocatalyst provided in this embodiment is prepared by the following steps:
[0044] S1. Prepare the first spinning solution: according to the mass ratio of Zn(AC)2:PVP:DMF of 8:16:72, weigh zinc acetate and dissolve it in N,N-dimethylformamide (DMF) organic solvent, stir magnetically for 20 minutes, then slowly add surfactant polyvinylpyrrolidone (PVP), and continue to stir magnetically for 8-10 hours to form a uniform and transparent first spinning solution.
[0045] S2. Prepare the second spinning solution: according to the mass ratio of [Cu(NO3)2+Fe(NO3)3]:PVP:DMF of 7:14:74, weigh ferric nitrate and copper nitrate and dissolve them in the organic solvent DMF (wherein the molar ratio of iron element to copper element is 2:1), stir magnetically for 20 minutes, then slowly add the surfactant PVP, and continue magnetic stirring for 8-10 hours until a uniform second spinning solution is formed.
[0046] The purity and sources of the reagents used in the above steps are the same as those in Example 1.
[0047] S3, electrospinning, bend two 8# stainless steel needles at an angle of 20° respectively, and put a plastic spray gun head on the outside of the two stainless steel needles with needle tips closely arranged side by side, so that the two stainless steel needles are in the middle of the plastic spray gun head, and connect a copper wire to each of the two needles. Inject the first spinning solution and the second spinning solution into a 5ml syringe respectively, connect the syringe to the plastic spray gun head, set an iron receiving net for receiving the electrospinning product on one side of the syringe, the distance between the receiving net and the needle is 12cm, tilt the nozzle downward by 12°, and connect the copper wire in the needle to a 12kV high-voltage power supply, control the flow rate ratio of the first spinning solution to the second spinning solution to 3:1, keep the air humidity at 35%, and collect the electrospinning products received on the iron receiving net.
[0048] S4. Calcine the electrospinning product. Place the electrospinning product in a muffle furnace, heat it to 650°C at a heating rate of 1°C / min, and keep it warm for 6 hours. After the temperature in the muffle furnace drops to room temperature, take out the sample to obtain a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0049] Example 3
[0050] This embodiment provides a ternary composite photocatalyst, which is composed of ZnO, ZnFe2O4, and CuO, namely, a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0051] The ternary composite photocatalyst provided in this embodiment is prepared by the following steps:
[0052] S1. Prepare the first spinning solution: according to the mass ratio of Zn(AC)2:PVP:DMF of 10:18:76, weigh zinc acetate and dissolve it in N,N-dimethylformamide (DMF) organic solvent, stir magnetically for 40 minutes, then slowly add surfactant polyvinylpyrrolidone (PVP), and continue to stir magnetically for 8-10 hours to form a uniform and transparent first spinning solution.
[0053] S2. Prepare the second spinning solution: according to the mass ratio of [Cu(NO3)2+Fe(NO3)3]:PVP:DMF of 10:16:79, weigh ferric nitrate and copper nitrate and dissolve them in the organic solvent DMF (wherein the molar ratio of iron to copper is 2:1), stir magnetically for 40 minutes, then slowly add the surfactant PVP, and continue magnetic stirring for 8-10 hours until a uniform second spinning solution is formed.
[0054] The purity and sources of the reagents used in the above steps are the same as those in Example 1.
[0055] S3, electrospinning, bend two 8# stainless steel needles at an angle of 30° respectively, and put a plastic spray gun head on the outside of the two stainless steel needles with needle tips closely arranged side by side, so that the two stainless steel needles are in the middle of the plastic spray gun head, and connect a copper wire to each of the two needles. Inject the first spinning solution and the second spinning solution into a 5ml syringe respectively, connect the syringe to the plastic spray gun head, set an iron receiving net for receiving the electrospinning product on one side of the syringe, the distance between the receiving net and the needle is 15cm, tilt the nozzle downward by 16°, and connect the copper wire in the needle to a 18kV high-voltage power supply, control the flow rate ratio of the first spinning solution to the second spinning solution to 2:1, keep the air humidity at 55%, and collect the electrospinning products received on the iron receiving net.
[0056] S4. Calcine the electrospinning product. Place the electrospinning product in a muffle furnace, heat it to 800°C at a heating rate of 1°C / min, and keep it warm for 3 hours. After the temperature in the muffle furnace drops to room temperature, take out the sample to obtain a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0057] Example 4
[0058] This embodiment provides a ternary composite photocatalyst, which is composed of ZnO, ZnFe2O4, and CuO, namely, a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0059] The ternary composite photocatalyst provided in this embodiment is prepared by the following steps:
[0060] S1. Prepare the first spinning solution: according to the mass ratio of Zn(AC)2:PVP:DMF of 9:17:74, weigh zinc acetate and dissolve it in N,N-dimethylformamide (DMF) organic solvent, stir magnetically for 30 minutes, then slowly add surfactant polyvinylpyrrolidone (PVP), and continue to stir magnetically for 8-10 hours to form a uniform and transparent first spinning solution.
[0061] S2. Prepare the second spinning solution: according to the mass ratio of [Cu(NO3)2+Fe(NO3)3]:PVP:DMF of 8:15:76, weigh ferric nitrate and copper nitrate and dissolve them in the organic solvent DMF (wherein the molar ratio of iron element to copper element is 2:1), stir magnetically for 30 minutes, then slowly add the surfactant PVP, and continue magnetic stirring for 8-10 hours until a uniform second spinning solution is formed.
[0062] The purity and sources of the reagents used in the above steps are the same as those in Example 1.
[0063] S3, electrospinning, bend two 8# stainless steel needles at an angle of 25° respectively, and put a plastic spray gun head on the outside of the two stainless steel needles with needle tips closely arranged side by side, so that the two stainless steel needles are in the middle of the plastic spray gun head, and connect a copper wire to each of the two needles. Inject the first spinning solution and the second spinning solution into a 5ml syringe respectively, connect the syringe to the plastic spray gun head, set an iron receiving net for receiving the electrospinning product on one side of the syringe, the distance between the receiving net and the needle is 13cm, tilt the nozzle downward by 15°, and connect the copper wire in the needle to a 15kV high-voltage power supply, control the flow rate ratio of the first spinning solution to the second spinning solution to 2:1, keep the air humidity at 50%, and collect the electrospinning products received on the iron receiving net.
[0064] S4. Calcine the electrospinning product. Place the electrospinning product in a muffle furnace, heat it to 700°C at a heating rate of 2°C / min, and keep it warm for 4 hours. After the temperature in the muffle furnace drops to room temperature, take out the sample to obtain a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0065] Example 5
[0066] This embodiment provides a ternary composite photocatalyst, which is composed of ZnO, ZnFe2O4, and CuO, namely, a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0067] The ternary composite photocatalyst provided in this embodiment is prepared by the following steps:
[0068] S1. Prepare the first spinning solution: weigh 2.0012 g zinc acetate and dissolve it in 3.6007 g N,N-dimethylformamide (DMF) organic solvent, stir it magnetically for 20 minutes, then slowly add 3.6007 g surfactant polyvinyl pyrrolidone (PVP), and continue to stir it magnetically for 8-10 hours to form a uniform and transparent first spinning solution.
[0069] S2. Prepare the second spinning solution: weigh 1.4425 g of ferric nitrate and 0.5587 g of copper nitrate, dissolve them in 14.8395 g of organic solvent DMF (wherein the molar ratio of iron element to copper element is 2:1), stir magnetically for 20 min, then slowly add 3.2230 g of surfactant PVP, and continue magnetic stirring for 8-10 h until a uniform second spinning solution is formed.
[0070] The purity and sources of the reagents used in the above steps are the same as those in Example 1.
[0071] S3, electrospinning, bend two 8# stainless steel needles at an angle of 30° respectively, and put a plastic spray gun head on the outside of the two stainless steel needles with needle tips closely arranged side by side, so that the two stainless steel needles are in the middle of the plastic spray gun head, and connect a copper wire to each of the two needles. Inject the first spinning solution and the second spinning solution into a 5ml syringe respectively, connect the syringe to the plastic spray gun head, set an iron receiving net for receiving the electrospinning product on one side of the syringe, the distance between the receiving net and the needle is 15cm, tilt the nozzle downward by 15°, and connect the copper wire in the needle to a 14kV high-voltage power supply, control the flow rate ratio of the first spinning solution to the second spinning solution to be 1:1, keep the air humidity at 45%, and collect the electrospinning products received on the iron receiving net.
[0072] S4. Calcine the electrospinning product. Place the electrospinning product in a muffle furnace, heat it to 650°C at a heating rate of 2°C / min, and keep it warm for 3 hours. After the temperature in the muffle furnace drops to room temperature, take out the sample to obtain a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0073] Example 6
[0074] This embodiment provides a ternary composite photocatalyst, which is composed of ZnO, ZnFe2O4, and CuO, namely, a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0075] The ternary composite photocatalyst provided in this embodiment is prepared by the following steps:
[0076] S1. Prepare the first spinning solution: weigh 2.0012 g zinc acetate and dissolve it in 3.6007 g N,N-dimethylformamide (DMF) organic solvent, stir it magnetically for 20 minutes, then slowly add 3.6007 g surfactant polyvinyl pyrrolidone (PVP), and continue to stir it magnetically for 8-10 hours to form a uniform and transparent first spinning solution.
[0077] S2. Prepare the second spinning solution: weigh 1.4425 g of ferric nitrate and 0.5587 g of copper nitrate, dissolve them in 14.8395 g of organic solvent DMF (wherein the molar ratio of iron element to copper element is 2:1), stir magnetically for 20 min, then slowly add 3.2230 g of surfactant PVP, and continue magnetic stirring for 8-10 h until a uniform second spinning solution is formed.
[0078] The purity and sources of the reagents used in the above steps are the same as those in Example 1.
[0079] S3, electrospinning, bend two 8# stainless steel needles at an angle of 30° respectively, and put a plastic spray gun head on the outside of the two stainless steel needles with needle tips closely arranged side by side, so that the two stainless steel needles are in the middle of the plastic spray gun head, and connect a copper wire to each of the two needles. Inject the first spinning solution and the second spinning solution into a 5ml syringe respectively, connect the syringe to the plastic spray gun head, set an iron receiving net for receiving the electrospinning product on one side of the syringe, the distance between the receiving net and the needle is 15cm, tilt the nozzle downward by 15°, and connect the copper wire in the needle to a 14kV high-voltage power supply, control the flow rate ratio of the first spinning solution to the second spinning solution to 3:1, keep the air humidity at 45%, and collect the electrospinning products received on the iron receiving net.
[0080] S4. Calcine the electrospinning product. Place the electrospinning product in a muffle furnace, heat it to 800°C at a heating rate of 2°C / min, and keep it warm for 3 hours. After the temperature in the muffle furnace drops to room temperature, take out the sample to obtain a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst.
[0081] Experimental example
[0082] 1. Test XRD patterns of Example 1, Example 5 and Example 6
[0083] The XRD patterns of the ternary composite catalysts obtained at calcination temperatures of 650°C and 800°C and flow rate ratios of the first spinning solution to the second spinning solution of 1:1 and 3:1 were tested. The test results show that diffraction peaks appear at 2θ angles of 31.70°, 34.39°, 36.18°, 47.46°, 56.46°, 62.76°, 66.21°, 67.80° and 68.92°. By comparing with the standard card (PDF#79-0207), it can be seen that the above diffraction peaks correspond to (100), (002), (101), (102), (110), (103), (200), (112) and (201) of ZnO, respectively. The diffraction peaks at 2θ of 29.91°, 35.22°, 42.81° and 62.14° correspond to the (220), (311), (400) and (440) crystal planes of the ZnFe2O4 standard card (PDF#74-2397), respectively; the diffraction peaks at 2θ of 35.50°, 38.93° and 48.66° correspond to the (002), (200) and (-202) crystal planes of the CuO standard card (PDF#80-1917), respectively. Therefore, in the ZnO / ZnFe2O4 / CuO composite material, the existence of ZnO, ZnFe2O4 and CuO is proved, and no diffraction peaks of other substances appear.
[0084] Further, under the condition that the flow rate ratio of the first spinning solution and the second spinning solution is 3:1, as the reaction temperature increases, the relative peak intensity of the diffraction peak of the sample calcined at 800°C becomes sharper and the half-peak width becomes narrower, indicating that the crystallinity of the sample is improved. When the calcination temperature is 650°C and the flow rate ratio of the first spinning solution and the second spinning solution is 1:1, compared with the flow rate ratio of the first spinning solution and the second spinning solution being 3:1, due to the decrease in the amount of the first spinning solution and the increase in the amount of the second spinning solution, the diffraction peak intensity of zinc oxide is relatively weak, and the diffraction peak intensity of zinc ferrite and copper oxide is relatively strong.
[0085] 2. Scanning electron microscope (SEM) images of the ternary composite catalyst in Test Example 5 before and after calcination
[0086] Figure 2 (a) is the SEM image of ZnO / ZnFe2O4 / CuO ternary composite material before calcination. Figure 2 (b) is the SEM image of the ZnO / ZnFe2O4 / CuO ternary composite photocatalyst after calcination at 650℃ for 3h. It can be seen from the figure that before calcination, the ZnO / ZnFe2O4 / CuO ternary composite material has a uniform dispersion, random arrangement, and smooth surface fibrous morphology. After calcination, due to the presence of DMF, PVP and salt ions NO3 - ,CH3COO - The evaporation of ZnO removed the ZnO, and the surface of the formed nanofibers was rough, and a spherical nanostructure of ZnO was formed on the surface of the nanofibers.
[0087] 3. Test the UV-visible absorption spectra of Example 1, Example 5, Example 6, ZnFe2O4 and ZnO
[0088] The light absorption performance of the photocatalytic material will greatly affect its photocatalytic performance. Therefore, the UV-visible absorption spectra of the ZnO / ZnFe2O4 / CuO ternary composite photocatalysts provided in Examples 1, 5 and 6 of the present invention were tested, and the UV-visible absorption spectra of the ZnFe2O4 nanomaterial and the ZnO nanomaterial were tested as control examples. The test results are as follows: Figure 3 shown.
[0089] The test results show that ZnFe2O4 has obvious absorption in the 200-700nm region, and the absorption edge appears at 690nm, indicating that ZnFe2O4 nanomaterials can absorb both ultraviolet light and visible light, while ZnO can only absorb ultraviolet light, and the absorption edge appears at 380nm. In the UV-visible absorption spectrum of the ZnO / ZnFe2O4 / CuO ternary composite photocatalyst, it can be seen that there are absorption edges of ZnO and ZnFe2O4. Compared with pure ZnO, the absorption edge of the ZnO / ZnFe2O4 / CuO ternary composite material shows an obvious red shift, indicating that the composite material has a wider light response range and a higher utilization rate of sunlight. Furthermore, when the flow rate ratio of the first spinning solution to the second spinning solution is 3:1, the ZnO / ZnFe2O4 / CuO sample calcined at 650℃ has stronger light absorption than that at 800℃.
[0090] 4. Photoluminescence spectra (PL) of test examples 1, 5, 6, ZnFe2O4, ZnO and CuO
[0091] The photoluminescence spectrum can reflect the separation rate of photogenerated electron-hole pairs in the sample. The higher the peak intensity, the higher the recombination rate of photogenerated electrons and hole pairs. Conversely, the lower the recombination rate of photogenerated carriers, the stronger the photocatalytic activity of the sample. Photoluminescence tests were conducted on ZnO, ZnFe2O4, CuO and ZnO / ZnFe2O4 / CuO ternary composite materials. The test results are shown in Figure 2. Figure 4 As shown, Figure 4 The PL spectra of the samples at an excitation wavelength of 345 nm are shown.
[0092] As can be seen from the figure, the ZnO photocatalyst has a strong emission peak, while the ZnO / ZnFe2O4 / CuO ternary nanocomposite shows a much lower luminescence intensity than ZnO, which indicates that the recombination of photogenerated electrons and hole pairs in the ZnO / ZnFe2O4 / CuO ternary nanocomposite is greatly inhibited, proving that the ternary nanocomposite may have higher photocatalytic activity.
[0093] Among them, the ZnO / ZnFe2O4 / CuO ternary composite material obtained under the preparation condition of the flow rate ratio of the first spinning solution to the second spinning solution being 1:1 showed a weaker luminescence intensity than the ZnO / ZnFe2O4 / CuO ternary composite material obtained under the preparation condition of the flow rate ratio of 3:1, indicating that the ZnO / ZnFe2O4 / CuO ternary composite material obtained under the preparation condition of the flow rate ratio of the first spinning solution to the second spinning solution being 1:1 has the lowest electron-hole pair recombination rate, so it can be inferred that it has the highest photocatalytic activity. This is consistent with the photocatalytic degradation results.
[0094] 5. Degradation curves of photocatalytic degradation of Rhodamine B (RhB) by testing Example 1, Example 5, Example 6, and ZnFe2O4, ZnO and CuO
[0095] In order to study the performance of ZnO / ZnFe2O4 / CuO ternary composite photocatalyst in photocatalytic degradation of RhB, a series of comparative experiments were carried out under the conditions of 300W metal halide lamp as light source, 30ml RhB volume, 10mg / L RhB mass concentration and 15mg photocatalyst. The experimental results are shown in Figure 5.
[0096] Depend on Figure 5 The test results show that the degradation rates of RhB for the ZnO / ZnFe2O4 / CuO ternary composite nanomaterial prepared at a calcination temperature of 650°C and a flow rate ratio of the first spinning solution to the second spinning solution of 3:1, the ZnO / ZnFe2O4 / CuO composite material prepared at a calcination temperature of 650°C and a flow rate ratio of the first spinning solution to the second spinning solution of 3:1, pure ZnO, pure ZnFe2O4 and pure CuO are 59.84%, 46.36%, 56.24%, 42.44% and 36.01% respectively under 210 minutes of illumination. The ZnO / ZnFe2O4 / CuO composite material obtained under the condition of the flow rate ratio of the first spinning solution to the second spinning solution being 3:1 has better photocatalytic effect than pure ZnO, pure ZnFe2O4 and pure CuO. At the same time, the photocatalyst obtained under the condition of the flow rate ratio of the first spinning solution to the second spinning solution being 1:1 has better photocatalytic effect. This may be due to the decrease in the amount of the first spinning solution and the increase in the amount of the second spinning solution, resulting in poor photocatalytic effect. 4 / The degradation rate of RhB by CuO ternary composite material was 53.65% after 210min of illumination. Compared with the calcination temperature of 650℃, the photocatalytic effect was not ideal. However, it can be seen from the XRD graph that the diffraction peak intensity of the sample calcined at 800℃ was higher and the crystallinity was better, which may be caused by the excessively high reaction temperature and the destruction of the fiber.
[0097] 6. Test the effect of hydrogen peroxide on photocatalytic performance
[0098] Based on Experimental Example 5, the ZnO / ZnFe2O 4 / The CuO ternary composite photocatalyst was tested for photocatalysis after adding different amounts of hydrogen peroxide. The degradation curve of RhB by the ternary composite photocatalyst after adding hydrogen peroxide was tested. The test results are shown in Figure 6(a)-(b) ZnO / ZnFe2O prepared under the conditions of calcination temperature of 650℃ and flow rate ratio of the first spinning solution to the second spinning solution of 3:1 4 / After adding 0.05mL, 0.1mL and 0.2mL H2O2 to the CuO ternary composite catalyst, the degradation rates of RhB were 83.02%, 93.33% and 90.34% respectively. Figure 6 (a)). ZnO / ZnFe2O prepared under the conditions of calcination temperature of 650°C and flow rate ratio of the first spinning solution to the second spinning solution of 1:1 4 / After adding 0.05mL, 0.mL1, 0.2mL and 0.4mL H2O2 to the CuO ternary composite catalyst, the degradation rates of RhB were 58.44%, 77.81%, 78.26% and 88.71% respectively.
[0099] The above results show that with the increase of H2O2 content, the degradation effect of RhB is getting better and better. Among them, when 0.1mLH2O2 was added to the ZnO / ZnFe2O4 / CuO prepared under the condition that the flow rate ratio of the first spinning solution and the second spinning solution was 3:1, the best photocatalytic efficiency was shown, and the degradation rate was 93.33%. At the same time, it can be found that the degradation rate of RhB of ZnO / ZnFe2O4 / CuO prepared under the condition that the flow rate ratio of the first spinning solution and the second spinning solution was 3:1 showed a trend of first increasing and then decreasing with the increase of H2O2 content. After adding H2O2, the iron ions in the ternary composite catalyst can undergo a cycle process from divalent to trivalent and then from trivalent back to divalent, thereby improving the photocatalytic effect. In addition, with the increase of H2O2 content, more hydroxyl radicals (·OH) were generated under light irradiation, and H2O2 and Fe in ZnO / ZnFe2O4 / CuO reacted with each other. 2+ A Fenton-like system is formed, thereby improving the degradation rate of rhodamine B. However, when the H2O2 content is too high, the excess H2O2 will react with ·OH to generate peroxyl radicals (HO2·, H2O2+·OH→H2O+HO2·), and then react with ·OH to generate O2 and H2O. Since ·OH will compete with HO2· and H2O2 (·OH+H2O2→H2O+HO2· and ·OH+HO2·→H2O+O2), a large amount of ·OH is consumed, so that ·OH cannot effectively react with RhB, resulting in a decrease in the degradation rate and a waste of H2O2. In summary, the above results show that the appropriate amount of H2O2 plays a key role in the degradation of RhB by the photo-Fenton reaction.
[0100] 7. Photocatalytic mechanism test analysis
[0101] In order to understand and analyze the mechanism of photo-Fenton reaction, 0.1 mL of H2O2 was added to ZnO / ZnFe2O4 / CuO prepared at a flow rate ratio of 3:1 between the first spinning solution and the second spinning solution, and free radical and electron hole capture experiments were carried out. Triethanolamine (TEOA), p-benzoquinone (BQ) and isopropyl alcohol (IPA) were used to capture holes (h+), superoxide radicals (·O 2- ) and hydroxyl radicals (·OH) to conduct free radical capture experiments. The test results are as follows Figure 7 As shown in the figure, the experimental results show that when triethanolamine (TEOA) and isopropanol (IPA) are added, the degradation rate of RhB by the ZnO / ZnFe2O4 / CuO photocatalyst prepared under the condition of a flow rate ratio of 3:1 between the first spinning solution and the second spinning solution is reduced from 93.33% to 34.79% and 37.37%, respectively, which obviously plays an inhibitory role. However, after adding p-benzoquinone (BQ), the degradation rate of RhB by ZnO / ZnFe2O4 / CuO is reduced to 68.76%, and its photocatalytic activity is significantly improved compared with the addition of triethanolamine (TEOA) and isopropanol (IPA). Therefore, it is proved that holes (h+) and hydroxyl radicals (·OH) are the main active species in the photocatalytic reaction.
[0102] The above experimental examples show that the present application successfully synthesized the ZnO / ZnFe2O4 / CuO ternary composite material by one-step electrospinning method, and characterized and analyzed the samples by XRD, SEM, UV-vis and PL. The results show that this new type of photocatalytic material was successfully prepared. We conducted photodegradation tests on the material and the effect of H2O2 dosage. The results show that the prepared ternary composite material belongs to a heterogeneous photo-Fenton photocatalyst with good photo-Fenton activity. Under the conditions of metal halide lamp irradiation and the absence of H2O2, the degradation rate of RhB in the ZnO / ZnFe2O4 / CuO composite material prepared at a flow rate ratio of 3:1 between the first spinning solution and the second spinning solution was 59.84% within 210min, and the degradation rate of RhB was significantly improved under the condition of the presence of H2O2. With the increase of H2O2 content, the degradation effect of RhB is getting better and better. However, the presence of too much H2O2 will cause a competitive reaction, which will reduce the degradation efficiency. When 0.1 mL of H2O2 was added to ZnO / ZnFe2O4 / CuO prepared at a flow rate ratio of 3:1 between the first spinning solution and the second spinning solution, the best photocatalytic efficiency was achieved, with a degradation rate of 93.33%. The results show that the appropriate amount of H2O2 plays a key role in the degradation of RhB by the photo-Fenton reaction.
[0103] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A ternary composite photocatalyst, characterized in that: The ternary composite photocatalyst is a ZnO / ZnFe2O4 / CuO ternary composite photocatalyst, wherein the mass ratio of ZnO, ZnFe2O4 and CuO is (1-5): (1-8): (1-5); The preparation method of the ternary composite photocatalyst comprises the following steps: S1. preparing a first spinning solution: uniformly mixing zinc acetate, a surfactant and an organic solvent according to a mass ratio of (8-10): (16-18): (72-76) to obtain a transparent first spinning solution; S2. preparing a second spinning solution: uniformly mixing a nitrate, a surfactant and an organic solvent in a mass ratio of (7-10):(14-16):(74-79) to obtain a second spinning solution, wherein the nitrate comprises ferric nitrate and copper nitrate, and the mass ratio of the ferric nitrate to the copper nitrate is (1.5-4):1; S3, electrospinning: injecting the first spinning solution and the second spinning solution into a syringe respectively, and electrospinning at a voltage of 12-18 kV, wherein the flow rate ratio of the first spinning solution to the second spinning solution is 3:1, to obtain an electrospinning product; S4, calcining the electrospinning product at a temperature of 650° C. and holding the product for 3-6 hours to obtain the ZnO / ZnFe2O4 / CuO ternary composite photocatalyst; In S1 and S2, the organic solvent is N,N-dimethylformamide, and the surfactant is polyvinyl pyrrolidone.
2. The ternary composite photocatalyst according to claim 1, characterized in that: The ZnO / ZnFe2O4 / CuO ternary composite photocatalyst is a composite structure of nanofibers and nanospheres.
3. The ternary composite photocatalyst according to claim 1 or 2, characterized in that: The mass ratio of ZnO, ZnFe2O4 and CuO is 1:1:
1.
4. The ternary composite photocatalyst according to claim 3, characterized in that: In step S3, each of the syringes is connected to a needle having a bending angle of 20-30°. A receiving net for receiving the electrospinning product is provided on one side of the syringe, and the distance between the needle and the receiving net is 12-15 cm.
5. The ternary composite photocatalyst according to claim 4, characterized in that: In step S1, the first spinning solution is prepared by mixing zinc acetate and an organic solvent in proportion, magnetically stirring for 20-40 minutes, then adding the surfactant in proportion, and magnetically stirring for 8-10 hours; in step S2, the second spinning solution is prepared by mixing nitrate and an organic solvent in proportion, magnetically stirring for 20-40 minutes, then adding the surfactant in proportion, and magnetically stirring for 8-10 hours.
6. Use of the ternary composite photocatalyst as described in any one of claims 1 to 5 in heterogeneous photo-Fenton catalytic degradation of organic pollutants in wastewater.