A kind of rigid non-isocyanate polyurethane foam and preparation method thereof

By reacting under catalyst conditions to generate rigid cyclic carbonate and diamine, non-isocyanate polyurethane foam with high mechanical properties is prepared, which solves the problems of toxicity and insufficient mechanical properties of traditional polyurethane materials, and realizes the low temperature at normal pressure Effective production.

CN115926157BActive Publication Date: 2024-12-06WUHAN YIKESIN TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211535119.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-02
Publication Date
2024-12-06
Estimated Expiration
2042-12-02

AI Technical Summary

Technical Problem

The isocyanate used in the production of traditional polyurethane materials is highly toxic and easy to react with water, which is not conducive to storage and transportation, and the mechanical properties of non-isocyanate polyurethanes are poor, limiting their development in the field of foam insulation materials.

Method used

By reacting rigid epoxy compounds with carbon dioxide under catalyst conditions to form rigid cyclic carbonate, then reacting with rigid diamine to form rigid non-isocyanate polyurethane, and mixing with foaming agent for foaming, a high mechanical performance is prepared Rigid non-isocyanate polyurethane foam.

Benefits of technology

High-efficiency reaction at normal pressure and low temperature, low catalyst cost, suitable for large-scale production, significantly improves the mechanical properties of non-isocyanate polyurethane, and is suitable for foam insulation materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115926157B_ABST
    Figure CN115926157B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of carbon emission reduction and polyurethane material preparation, and specifically discloses a rigid non-isocyanate polyurethane foam and a preparation method thereof. 2 The reaction is carried out to obtain a rigid cyclic carbonate, and then the product is reacted with a diamine to obtain a rigid non-isocyanate polyurethane, and then mixed with a blowing agent for foaming to obtain a rigid non-isocyanate polyurethane foam. The present invention improves the mechanical properties and adjustability of the non-isocyanate polyurethane by limiting the raw material structure and group; the present invention adopts mild reaction conditions such as normal pressure and low temperature, and adjusts the amount of reactants and blowing agents, so that the degree of reaction is significantly enhanced, and an excellent foaming effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane material preparation, in particular to a rigid non-isocyanate polyurethane foam and a preparation method thereof. Background Art

[0002] Polyurethane materials have excellent physical and chemical properties and can be widely used in the production of plastics, foams and other fields. In recent years, the consumption scale of polyurethane has increased year by year, and it has won unanimous praise from the market and has a very broad market prospect. However, in the production process of traditional polyurethane, phosgene is often used to convert amines into isocyanates, but phosgene is highly toxic and has serious harm to the human body if inhaled for a long time, which has serious disadvantages. At the same time, isocyanate products are easy to react with water, which is not conducive to the preparation of polyurethane and the storage and transportation of isocyanates.

[0003] Non-isocyanate polyurethane based on the reaction of cyclic carbonates and amines is our ideal alternative material. Non-isocyanate polyurethane products not only have better performance than isocyanates and can be used in many fields such as adhesives and foam materials, but also the conditions required for the production of non-isocyanate polyurethane are milder and have lower energy consumption. Due to the small variety of cyclic carbonate products, the complex synthesis process, and the adverse factors such as high temperature and high pressure required for the reaction, the industrial development of non-isocyanate polyurethane is slow. In addition, the current raw materials for the synthesis of non-isocyanate polyurethane are mainly flexible cyclic carbonates and flexible diamines, which leads to its high viscosity and poor mechanical properties, which greatly limits its development and application in fields such as foam insulation materials.

[0004] Therefore, how to provide a rigid non-isocyanate polyurethane foam and a preparation method thereof, and improve the mechanical strength of the non-isocyanate polyurethane foam while reducing the production cost is a difficult problem to be solved urgently in the art. Summary of the invention

[0005] In view of this, the present invention provides a rigid non-isocyanate polyurethane foam and a preparation method thereof, so as to solve the problem of low mechanical strength of the foam material synthesized by non-isocyanate polyurethane on the market.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A method for preparing a rigid non-isocyanate polyurethane foam comprises the following steps:

[0008] 1) A rigid epoxy compound reacts with carbon dioxide under catalyst conditions to obtain a rigid cyclic carbonate;

[0009] 2) reacting a rigid cyclic carbonate with a rigid diamine to obtain a rigid non-isocyanate polyurethane;

[0010] 3) Mixing the rigid non-isocyanate polyurethane with a blowing agent and foaming the mixture, and obtaining the rigid non-isocyanate polyurethane foam after the foaming is completed.

[0011] Preferably, in step 1), the reaction temperature is 25-50° C., the reaction time is 2-12 h, the molar ratio of the rigid epoxy compound to carbon dioxide is 1:1.2-1.5, and the mass ratio of the catalyst to the rigid epoxy compound is 1:50-1500.

[0012] Preferably, the rigid epoxy compound includes one or more of cyclohexene oxide, styrene oxide, 2-phenylpropylene oxide, epoxy soybean oil, ethyl phenylglycidyl propionate and 1,2-butylene oxide.

[0013] Preferably, the catalyst in step 1) is a polyionic liquid supramolecular catalyst; the preparation method is: firstly, 1-vinyl-3-propylaminoimidazole bromide solution and azobisisobutyronitrile are mixed, and polymerization reaction is carried out to obtain amino polyionic liquid, and then the amino polyionic liquid is mixed with zinc chloride to obtain a polyionic liquid supramolecular catalyst.

[0014] Preferably, the mass ratio of 1-vinyl-3-propylaminoimidazole bromide to azobisisobutyronitrile in the 1-vinyl-3-propylaminoimidazole bromide solution is 100:1-3, the molar ratio of 1-vinyl-3-propylaminoimidazole bromide to zinc chloride in the 1-vinyl-3-propylaminoimidazole bromide solution is 1:1-4, and the molar concentration of the 1-vinyl-3-propylaminoimidazole bromide solution is 0.5-2 mol / L;

[0015] The polymerization reaction temperature is 60-100° C., and the polymerization reaction time is 8-12 hours.

[0016] Preferably, the molar ratio of the rigid cyclic carbonate to the rigid diamine in step 2) is 0.1 to 3:1, the reaction temperature is 25 to 70° C., and the reaction time is 0.5 to 3 hours.

[0017] Preferably, the rigid diamine includes one or more of p-phenylenediamine, hexamethylenediamine, ethylenediamine, isophoronediamine, p-aminodiphenylmethane, p-aminodiphenylethane, 1,5-diaminopentane and diaminodiphenylmethane.

[0018] Preferably, in step 3), the molar ratio of the foaming agent to the rigid diamine is 0.01-0.5:1, the foaming time is 1-5 hours, and the foaming temperature is 20-70°C.

[0019] Preferably, the foaming agent includes one or more of cyclopentane, isopentane, carbon dioxide, sodium bicarbonate, polymethylhydrogensiloxane or pentafluorobutane.

[0020] Another object of the present invention is to provide a rigid non-isocyanate polyurethane foam prepared by the preparation method.

[0021] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention has a mild reaction and can efficiently obtain a rigid polyurethane material through two-step reaction at normal pressure and low temperature;

[0023] 2. The catalyst is independently developed and assembled in an aqueous solution at room temperature. It has mild preparation conditions and low cost, and is suitable for large-scale production applications;

[0024] 3. By limiting the raw material structure and groups, a non-isocyanate polyurethane foam with adjustable rigidity is generated, which significantly improves the mechanical properties of the non-isocyanate polyurethane. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0026] Figure 1 This is the rigid non-isocyanate polyurethane foam prepared in Example 3. DETAILED DESCRIPTION

[0027] The present invention provides a method for preparing a rigid non-isocyanate polyurethane foam, comprising the following steps:

[0028] 1) A rigid epoxy compound reacts with carbon dioxide under catalyst conditions to obtain a rigid cyclic carbonate;

[0029] 2) reacting a rigid cyclic carbonate with a rigid diamine to obtain a rigid non-isocyanate polyurethane;

[0030] 3) Mixing the rigid non-isocyanate polyurethane with a blowing agent and foaming the mixture, and obtaining the rigid non-isocyanate polyurethane foam after the foaming is completed.

[0031] In the present invention, the reaction temperature in step 1) is 25-50°C, specifically 26°C, 28°C, 30°C, 35°C, 40°C, 45°C; the reaction time is 2-12h, specifically 4h, 5h, 6h, 8h, 10h; the molar ratio of the rigid epoxy compound to carbon dioxide is 1:1.2-1.5, preferably 1:1.3-1.4, and more preferably 1:1.35; the mass ratio of the catalyst to the rigid epoxy compound is 1:50-1500, preferably 1:100-1200, more preferably 1:400-1000, and further preferably 1:600.

[0032] In the present invention, the rigid epoxy compound includes one or more of cyclohexene oxide, styrene oxide, 2-phenylpropylene oxide, epoxy soybean oil, ethyl phenylglycidyl propionate and 1,2-butylene oxide.

[0033] In the present invention, the catalyst in step 1) is a polyionic liquid supramolecular catalyst; the preparation method is: firstly, 1-vinyl-3-propylaminoimidazole bromide solution and azobisisobutyronitrile are mixed, and polymerization reaction is carried out to obtain amino polyionic liquid, and then the amino polyionic liquid is mixed with zinc chloride to obtain the polyionic liquid supramolecular catalyst.

[0034] In the present invention, the mass ratio of 1-vinyl-3-propylaminoimidazole bromide and azobisisobutyronitrile in the 1-vinyl-3-propylaminoimidazole bromide solution is 100:1-3, specifically 100:1.2, 100:1.4, 100:1.5, 100:1.6, 100:1.8, 100:2, 100:2.2, 100:2.4, 100:2.5, 100:2.6, 100:2.8; the molar ratio of 1-vinyl-3-propylaminoimidazole bromide and zinc chloride in the 1-vinyl-3-propylaminoimidazole bromide solution is 1:1-4, specifically 1:1.2, 1:1.5, 1:1.8, 1:2, 1:2.2, 1:2.5, 1:2.8, 1:3, 1:3.2, 1:3.5, 1:3.8.

[0035] In the present invention, the molar concentration of the 1-vinyl-3-propylaminoimidazole bromide solution is 0.5-2 mol / L, specifically 0.6 mol / L, 0.8 mol / L, 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.8 mol / L.

[0036] In the present invention, the polymerization reaction temperature is 60-100°C, specifically 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C; the polymerization reaction time is 8-12h, specifically 9h, 10h, 11h.

[0037] In the present invention, the amino polyionic liquid and zinc chloride are preferably mixed by stirring, the stirring time is preferably 1 to 4 hours, specifically 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, and the stirring rate is preferably 10 to 40 rpm, specifically 12 rpm, 15 rpm, 20 rpm, 25 rpm, 30 rpm, 35 rpm.

[0038] In the present invention, the molar ratio of the rigid cyclic carbonate to the rigid diamine in the step 2) is 0.1-3:1, preferably 0.5-2.5:1, further preferably 1-2:1, and further preferably 1.5:1; the reaction temperature is 25-70°C, specifically 28°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C; the reaction time is 0.5-3h, specifically 0.8h, 1h, 1.5h, 2h, 2.5h.

[0039] In the present invention, the rigid diamine includes one or more of p-phenylenediamine, hexamethylenediamine, ethylenediamine, isophoronediamine, p-aminodiphenylmethane, p-aminodiphenylethane, 1,5-diaminopentane and diaminodiphenylmethane.

[0040] In the present invention, the molar ratio of the blowing agent to the rigid diamine in the step 3) is 0.01 to 0.5:1, preferably 0.05 to 0.4:1, further preferably 0.1 to 0.3:1, and further preferably 0.2:1; the foaming reaction time is 1 to 5 hours, specifically 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, and 4.5 hours; the foaming reaction temperature is 20 to 70°C, specifically 30°C, 40°C, 50°C, and 60°C.

[0041] In the present invention, the mixing in the step 3) is preferably stirring mixing, and the stirring rate is 100-400rpm, specifically 120rpm, 150rpm, 180rpm, 200rpm, 220rpm, 250rpm, 280rpm, 300rpm, 350rpm, 380rpm; the stirring temperature is 20-200°C, specifically 40°C, 50°C, 60°C, 80°C, 100°C, 120°C, 140°C, 150°C, 160°C, 180°C, and the stirring time is 1-200min, specifically 5min, 10min, 20min, 50min, 60min, 80min, 100min, 120min, 150min, 160min, 180min.

[0042] In the present invention, the foaming agent includes one or more of cyclopentane, isopentane, carbon dioxide, sodium bicarbonate, polymethylhydrogensiloxane or pentafluorobutane.

[0043] The invention also provides a rigid non-isocyanate polyurethane foam prepared by the preparation method.

[0044] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] Example 1

[0046] 1-vinyl-3-propylaminoimidazole bromide was dissolved in deionized water to obtain a 1 mol / L 1-vinyl-3-propylaminoimidazole bromide solution, an initiator azobisisobutyronitrile (3% of the monomer mass) was added, the polymerization temperature was 70°C, the polymerization time was 8h, and the mixture was cooled to room temperature to obtain an amino polyionic liquid. Zinc chloride was added, and the molar ratio of the amino polyionic liquid to the zinc chloride was 1:1. The mixture was stirred at 20 rpm for 1h at room temperature, centrifuged, the precipitate was collected, and vacuum dried at 60°C to obtain a polyionic liquid supramolecular catalyst.

[0047] In a reactor equipped with a balloon, add a polyionic liquid supramolecular catalyst (50 mg) and epoxidized soybean oil (54 mmol, 51.3 g), fill the balloon with carbon dioxide (the molar ratio of CO2: epoxidized soybean oil is 1.25:1), keep the pressure at normal pressure, and set the temperature to 40°C. React at this temperature for 3 hours to obtain the product. After separation, drying and other treatments, a cyclic carbonate prepared from epoxidized soybean oil is finally obtained.

[0048] The cyclic carbonate (25 mmol, 28.2 g) obtained above and ethylenediamine (100 mmol, 0.6 g) were mixed, stirred at 25°C for 0.5 h, and then sodium bicarbonate (50 mmol, 4.2 g) was added and stirred at 50°C, 150 rpm for 1 h. The stirred material was transferred into a mold, heated to 70°C, and maintained for 3 h, and finally a rigid non-isocyanate polyurethane foam was obtained.

[0049] Example 2

[0050] In a reactor equipped with a balloon, the polyionic liquid supramolecular catalyst (50 mg) prepared in Example 1 and styrene oxide (50 mmol, 6.0 g) were added, carbon dioxide was filled into the balloon (the molar ratio of CO2:styrene oxide was 1.3:1), the pressure was kept at normal pressure, the temperature was set to 50°C, and the reaction was carried out at this temperature for 3 hours to obtain the product. After separation, drying and other treatments, a cyclic carbonate prepared from styrene oxide was finally obtained.

[0051] The cyclic carbonate (100 mmol, 16.4 g) obtained above and diaminodiphenylmethane (100 mmol, 19.8 g) were mixed, stirred at 50°C for 2 h, and then cyclopentane (40 mmol, 2.8 g) was added and stirred at 60°C, 200 rpm for 2 h. The stirred material was transferred into a mold, heated to 70°C, and reacted for 5 h to finally obtain a rigid non-isocyanate polyurethane foam.

[0052] Example 3

[0053] In a reactor equipped with a balloon, the polyionic liquid supramolecular catalyst (50 mg) prepared in Example 1 and cyclohexene oxide (40 mmol, 3.9 g) were added, carbon dioxide was filled into the balloon (the molar ratio of CO2: cyclohexene oxide was 1.5:1), the pressure was kept at normal pressure, the temperature was set to 40°C, and the reaction was carried out at this temperature for 4 hours to obtain the product. The product was then centrifuged to separate the catalyst and the corresponding cyclic carbonate, and after separation, drying and other treatments, the cyclic carbonate prepared from cyclohexene oxide was finally obtained.

[0054] Take a 250ml clean beaker, add the above-obtained cyclic carbonate (200mmol, 28.4g) and 1,5-diaminopentane (100mmol, 10.2g) at 40℃, stir and react for 2h, then add sodium bicarbonate (40mmol, 3.4g) and stir at 65℃, 100rpm for 1h, transfer the stirred material into a mold, heat to 70℃, react for 5h, and finally obtain a rigid non-isocyanate polyurethane foam.

[0055] The rigid non-isocyanate polyurethane foam prepared in this example is as follows Figure 1 shown.

[0056] Experimental Example 1

[0057] The properties of the rigid non-isocyanate polyurethane foams prepared in Examples 1 to 3 were tested (corresponding to samples A, B, and C, respectively). The standards and test results are shown in Table 1.

[0058] Table 1 Structural properties of rigid non-isocyanate polyurethane foam

[0059]

[0060]

[0061] It can be seen from Table 1 that the rigid non-isocyanate polyurethane foams prepared in Examples 1 to 3 are resistant to chemical corrosion and have high thermal stability; they have excellent waterproof and vapor barrier properties; at the same time, they have good thermal insulation properties, are safe and non-toxic, and have excellent product performance.

[0062] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0063] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a rigid non-isocyanate polyurethane foam, comprising the following steps: 1) Rigid epoxides react with carbon dioxide under catalyst conditions to obtain rigid cyclic carbonates; 2) reacting a rigid cyclic carbonate with a rigid diamine to obtain a rigid non-isocyanate polyurethane; 3) mixing the rigid non-isocyanate polyurethane with a blowing agent, foaming the mixture, and obtaining a rigid non-isocyanate polyurethane foam after the foaming is completed; In the step 1), the reaction temperature is 25-45°C, the reaction time is 2-12 hours, the molar ratio of the rigid epoxy compound to carbon dioxide is 1:1.2-1.5, and the mass ratio of the catalyst to the rigid epoxy compound is 1:50-1500; Features: The catalyst in step 1) is a polyionic liquid supramolecular catalyst, which is obtained by first mixing 1-vinyl-3-propylaminoimidazole bromide solution and azobisisobutyronitrile to perform polymerization reaction to obtain amino polyionic liquid, and then mixing the amino polyionic liquid with zinc chloride to obtain the polyionic liquid supramolecular catalyst.

2. The method for preparing a rigid non-isocyanate polyurethane foam according to claim 1, characterized in that: The rigid epoxy compound includes one or more of cyclohexene oxide, styrene oxide, 2-phenylpropylene oxide, epoxy soybean oil, ethyl phenylglycidyl propionate and 1,2-butylene oxide.

3. The method for preparing a rigid non-isocyanate polyurethane foam according to claim 1, characterized in that: The mass ratio of 1-vinyl-3-propylaminoimidazole bromide to azobisisobutyronitrile in the 1-vinyl-3-propylaminoimidazole bromide solution is 100:1-3, the molar ratio of 1-vinyl-3-propylaminoimidazole bromide to zinc chloride is 1:1-4, and the concentration of the 1-vinyl-3-propylaminoimidazole bromide solution is 0.5-2 mol / L; The polymerization reaction temperature is 60-100° C., and the polymerization reaction time is 8-12 hours.

4. The method for preparing a rigid non-isocyanate polyurethane foam according to claim 1, characterized in that: The molar ratio of the rigid cyclic carbonate to the rigid diamine in step 2) is 0.1-3:1, the reaction temperature is 25-70° C., and the reaction time is 0.5-3 hours.

5. The method for preparing a rigid non-isocyanate polyurethane foam according to claim 1 or 4, characterized in that: The rigid diamine includes one or more of p-phenylenediamine, isophoronediamine, p-aminodiphenylmethane, p-aminodiphenylethane and diaminodiphenylmethane.

6. The method for preparing a rigid non-isocyanate polyurethane foam according to claim 5, characterized in that: In the step 3), the molar ratio of the foaming agent to the rigid diamine is 0.01-0.5:1, the foaming time is 1-5 hours, and the foaming temperature is 20-70°C.

7. The method for preparing a rigid non-isocyanate polyurethane foam according to claim 6, characterized in that: The foaming agent includes one or more of cyclopentane, isopentane, carbon dioxide, sodium bicarbonate, polymethylhydrogensiloxane or pentafluorobutane.

8. The rigid non-isocyanate polyurethane foam prepared by the preparation method according to any one of claims 1 to 7.