A method for bonding rubber and nylon fabric

By using an adhesive containing aminocarbenoic acid and a rubber compounding glue in the bonding process of rubber and nylon fabric, combined with vulcanization treatment, the problem of low bond strength in the prior art is solved, and rubber and nylon fabric is realized High strength bonding.

CN115926214BActive Publication Date: 2024-12-06CHEMCHINA SHUGUANG RUBBER IND RES&DESIGN INST C
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310011588.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-05
Publication Date
2024-12-06
Estimated Expiration
2043-01-05

AI Technical Summary

Technical Problem

In the existing bonding methods of rubber and fabrics, white carbon black in the interstitial white system glue is not easy to disperse, the preparation time is long, and the bonding strength is low, usually between 2-5N/mm, making it difficult to achieve high-strength bonding.

Method used

Adhesives containing resorcinol, aminocarbenol and solvents are coated on the surface of nylon fabric, and zinc oxide, stearic acid, anti-aging agent and vulcanizing agent are added to the rubber mixing glue, through aminocarbenol It forms bonds with amino and carboxyl groups on the surface of the fabric, and is vulcanized to improve the bonding strength.

Benefits of technology

The bonding strength between rubber and nylon fabric is significantly improved, reaching more than 7N/mm, and the method is simple and the bonding system is evenly dispersed, enhancing the bonding effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004037960030000011
    Figure BDA0004037960030000011
  • Figure BDA0004037960030000021
    Figure BDA0004037960030000021
  • Figure BDA0004037960030000031
    Figure BDA0004037960030000031
Patent Text Reader

Abstract

The present invention provides a method for bonding rubber to nylon fabric, and belongs to the field of polymer materials. The present invention provides a method for bonding rubber to nylon fabric, wherein the surface of nylon fabric is modified by aminocarboxylic acid, the amino groups and carboxyl groups in the aminocarboxylic acid and the amino groups and carboxyl groups on the surface of nylon fabric mutually form carboxylic acid ammonium ion bonds or hydrogen bonds, the unsaturated double bonds in the aminocarboxylic acid are bonded to the rubber by vulcanization, the strength of the modified nylon fabric and the rubber is greatly increased, and at the same time, by adding adhesive A to the rubber compound, the adhesive system of the rubber compound and the adhesive system attached to the nylon fabric mutually penetrate, so that the bonding strength between the rubber and the nylon fabric is further improved, and the bonding strength reaches more than 7N / mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a method for bonding rubber and nylon fabric. Background Art

[0002] The bonding between rubber and fabric is a common problem in the preparation of rubber products. The commonly used method is to apply glue on the fabric or add adhesive to the rubber mix. The commonly used bonding system is the m-acetylene white system, but the white carbon black in the m-acetylene white system glue is not easy to disperse and the preparation time is long. At the same time, if only glue is applied on the fabric or adhesive is added to the rubber mix, the bonding strength between rubber and fabric is often too low, usually 2 to 5N / mm, and it is difficult to achieve high-strength bonding. Summary of the invention

[0003] In view of this, the object of the present invention is to provide a method for bonding rubber to nylon fabric. The bonding method provided by the present invention enables the bonding strength between rubber and nylon fabric to be greater than 7N / mm.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for bonding rubber and nylon fabric, comprising the following steps:

[0006] The surface of the nylon fabric is coated with adhesive, dried, calendered with rubber compound and vulcanized in sequence;

[0007] The adhesive comprises the following components in parts by weight: 10 parts of resorcinol, 5 to 20 parts of adhesive A, 0.5 to 10 parts of aminocarbolic acid and 30 to 1000 parts of solvent, wherein the aminocarbolic acid has a structure shown in Formula I:

[0008]

[0009] In Formula I, R1 and R2 are independently a hydrocarbon group or hydrogen, and R1 and / or R2 contain a carbon-carbon double bond;

[0010] The rubber compound comprises the following components in parts by mass: 100 parts of rubber, 0-7 parts of zinc oxide, 0-5 parts of stearic acid, 0-10 parts of antioxidant, 1-10 parts of resorcinol, 1-70 parts of white carbon black, 1-15 parts of adhesive A and 0.5-5 parts of vulcanizing agent, and the parts by mass of the zinc oxide, stearic acid and antioxidant are not 0.

[0011] Preferably, the adhesive comprises the following components in parts by mass: 10 parts of resorcinol, 12 parts of adhesive A, 2 to 5 parts of aminocarbolic acid and 200 parts of solvent.

[0012] Preferably, the aminocarboenoic acid is 4-amino-5-hexenoic acid or 2-amino-8-nonenoic acid.

[0013] Preferably, the rubber compound comprises the following components in parts by mass: 100 parts of rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A and 2.5 parts of vulcanizing agent.

[0014] Preferably, the vulcanizing agent is sulfur or a peroxide vulcanizing agent.

[0015] Preferably, the rubber includes one or more of nitrile rubber, natural rubber, ethylene propylene rubber, chloroprene rubber, butyl rubber, silicone rubber, styrene butadiene rubber and silicone rubber.

[0016] Preferably, the antioxidant includes one or more of antioxidant RD, antioxidant 4020, antioxidant 4010NA, antioxidant MB, antioxidant MBZ, antioxidant NBC, antioxidant 2246, antioxidant 2246S, antioxidant 246, antioxidant SP, antioxidant 6DDP, antioxidant UOP588, antioxidant UOP788, antioxidant DD, antioxidant AW and antioxidant D.

[0017] Preferably, the coating amount after drying is 1 to 50 g / m 2 .

[0018] Preferably, the loading amount of the rubber compound is 50 to 10000 g / m 2 .

[0019] Preferably, the vulcanization temperature is 100-180° C., the time is 3-60 min, and the pressure is 10-25 MPa.

[0020] The present invention provides a method for bonding rubber to nylon fabric, comprising the following steps: coating an adhesive on the surface of the nylon fabric, drying, calendering a rubber mix and vulcanizing in sequence; the adhesive comprises the following components in parts by weight: 10 parts of resorcinol, 5 to 20 parts of an adhesive A, 0.5 to 10 parts of an aminocarbolic acid and 30 to 1000 parts of a solvent, wherein the aminocarbolic acid has a structure shown in Formula I:

[0021]

[0022] In formula I, R1 and R2 are independently a hydrocarbon group or hydrogen, and R1 and / or R2 contain a carbon-carbon double bond;

[0023] The rubber compound comprises the following components in parts by mass: 100 parts of rubber, 0-7 parts of zinc oxide, 0-5 parts of stearic acid, 0-10 parts of antioxidant, 1-10 parts of resorcinol, 1-70 parts of white carbon black, 1-15 parts of adhesive A and 0.5-5 parts of vulcanizing agent, and the parts by mass of the zinc oxide, stearic acid and antioxidant are not 0.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The invention provides a method for bonding rubber and nylon fabric. The surface of the nylon fabric is modified by aminocarbon olefinic acid. The amino groups and carboxyl groups in the aminocarbon olefinic acid form carboxylic acid ammonium ion bonds or hydrogen bonds with the amino groups and carboxyl groups on the surface of the nylon fabric. The unsaturated double bonds in the aminocarbon olefinic acid are bonded to the rubber through vulcanization. The strength of the modified nylon fabric and the rubber is greatly increased. Meanwhile, by adding adhesive A to the rubber compound, the adhesive system of the rubber compound and the adhesive system attached to the nylon fabric penetrate each other, thereby further improving the bonding strength between the rubber and the nylon fabric, and the bonding strength reaches more than 7N / mm.

[0026] In addition, the present invention evenly disperses the bonding system of the adhesive and the rubber compound by using a solvent, so that the bonding system penetrates into the surface and the interior of the nylon fabric, and the bonding method is simple. DETAILED DESCRIPTION

[0027] The present invention provides a method for bonding rubber and nylon fabric, comprising the following steps:

[0028] The surface of the nylon fabric is coated with adhesive, dried, calendered with rubber compound and vulcanized in sequence;

[0029] The adhesive comprises the following components in parts by weight: 10 parts of resorcinol, 5 to 20 parts of adhesive A, 0.5 to 10 parts of aminocarbolic acid and 30 to 1000 parts of solvent, wherein the aminocarbolic acid has a structure shown in Formula I:

[0030]

[0031] In formula I, R1 and R2 are independently a hydrocarbon group or hydrogen, and R1 and / or R2 contain a carbon-carbon double bond;

[0032] The rubber compound comprises the following components in parts by mass: 100 parts of rubber, 0-7 parts of zinc oxide, 0-5 parts of stearic acid, 0-10 parts of antioxidant, 1-10 parts of resorcinol, 1-70 parts of white carbon black, 1-15 parts of adhesive A and 0.5-5 parts of vulcanizing agent, and the parts by mass of the zinc oxide, stearic acid and antioxidant are not 0.

[0033] In the present invention, unless otherwise specified, the raw materials used are all commercially available products in the art.

[0034] In the present invention, the mass fraction of adhesive A in the adhesive is preferably 12 parts.

[0035] In the present invention, the adhesive preferably comprises the following components in parts by mass: 10 parts of resorcinol, 12 parts of adhesive A, 2 to 5 parts of aminocarbolic acid and 200 parts of solvent.

[0036] In the present invention, the aminocarbolic acid is preferably 4-amino-5-hexenoic acid or 2-amino-8-nonenoic acid.

[0037] In the present invention, the solvent preferably includes one or more of water, ethanol and ethyl acetate.

[0038] The present invention has no particular limitation on the preparation method of the adhesive, and the adhesive can be prepared by a composition preparation method well known to those skilled in the art.

[0039] In the present invention, the coating amount after drying is preferably 1 to 50 g / m 2 , more preferably 8g / m 2 .

[0040] In the present invention, the function of the drying is to remove the solvent.

[0041] In the present invention, the rubber compound preferably comprises the following components in parts by mass: 100 parts of rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A and 2.5 parts of vulcanizing agent.

[0042] In the present invention, the vulcanizing agent is preferably sulfur or a peroxide vulcanizing agent.

[0043] In the present invention, the rubber preferably includes one or more of nitrile rubber, natural rubber, ethylene propylene rubber, chloroprene rubber, butyl rubber, silicone rubber, styrene butadiene rubber and silicone rubber.

[0044] In the present invention, the antioxidant preferably includes one or more of antioxidant RD, antioxidant 4020, antioxidant 4010NA, antioxidant MB, antioxidant MBZ, antioxidant NBC, antioxidant 2246, antioxidant 2246S, antioxidant 246, antioxidant SP, antioxidant 6DDP, antioxidant UOP588, antioxidant UOP788, antioxidant DD, antioxidant AW and antioxidant D.

[0045] The present invention has no particular limitation on the preparation method of the rubber compound, and the rubber compound can be prepared by a composition preparation method well known to those skilled in the art.

[0046] In the present invention, the loading amount of the rubber compound is preferably 50 to 10000 g / m 2 , more preferably 2000g / m 2 .

[0047] The present invention has no special limitation on the specific method of the calendering. The function of the calendering is to make the rubber compound and the nylon fabric fit better so as to better perform the subsequent vulcanization.

[0048] In the present invention, the vulcanization temperature is preferably 100-180° C., more preferably 160° C., the time is preferably 3-60 min, more preferably 20 min, and the pressure is preferably 10-25 MPa, more preferably 15 MPa.

[0049] In order to further illustrate the present invention, the method for bonding rubber and nylon fabric provided by the present invention is described in detail below with reference to examples, but they should not be construed as limiting the scope of protection of the present invention.

[0050] Example 1

[0051] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 2 parts of 4-amino-5-hexenoic acid, and 200 parts of solvent ethanol; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0052] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0053] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0054] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 8.7 N / mm.

[0055] Example 2

[0056] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 3 parts of 4-amino-5-hexenoic acid, and 200 parts of ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0057] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0058] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0059] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 9.1 N / mm.

[0060] Example 3

[0061] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 5 parts of 4-amino-5-hexenoic acid, and 200 parts of ethanol; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0062] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0063] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0064] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 9.4 N / mm.

[0065] Example 4

[0066] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 3 parts of 2-amino-8-nonenoic acid, and 200 parts of ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0067] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0068] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0069] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 9.8 N / mm.

[0070] Example 5

[0071] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 4 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0072] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0073] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0074] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 10.1 N / mm.

[0075] Example 6

[0076] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 0.5 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0077] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0078] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0079] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 7.2 N / mm.

[0080] Example 7

[0081] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 10 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0082] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0083] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0084] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 9.5 N / mm.

[0085] Example 8

[0086] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 20 parts of adhesive A, 5 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0087] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0088] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0089] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 8.7 N / mm.

[0090] Example 9

[0091] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 5 parts of adhesive A, 5 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0092] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0093] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0094] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 9.2 N / mm.

[0095] Example 10

[0096] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 5 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 10 parts of resorcinol, 30 parts of white carbon black, 15 parts of adhesive A, and 2.5 parts of sulfur;

[0097] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0098] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0099] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 9.6 N / mm.

[0100] Embodiment 11

[0101] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 5 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 1 part of resorcinol, 30 parts of white carbon black, 1 part of adhesive A, and 2.5 parts of sulfur;

[0102] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0103] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0104] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 7.2 N / mm.

[0105] Example 12

[0106] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 20 parts of adhesive A, 5 parts of 2-amino-8-nonenoic acid, and 1000 parts of solvent ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 5 parts of resorcinol, 30 parts of white carbon black, 6 parts of adhesive A, and 2.5 parts of sulfur;

[0107] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0108] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0109] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 8.1 N / mm.

[0110] Example 13

[0111] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 4 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0112] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 50 g / m 2 );

[0113] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0114] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 10.5 N / mm.

[0115] Embodiment 14

[0116] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 4 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0117] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 50 g / m 2 );

[0118] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0119] 4) Vulcanization at 160°C for 20 min, 25 MPa; after testing, the bonding strength between rubber and fabric is 11.0 N / mm.

[0120] Embodiment 15

[0121] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 4 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0122] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 50 g / m 2 );

[0123] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0124] 4) Vulcanization at 160°C for 20 min, 10 MPa; after testing, the bonding strength between rubber and fabric is 10.4 N / mm.

[0125] Example 16

[0126] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 15 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent ethyl acetate; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 1 part of resorcinol, 30 parts of white carbon black, 1 part of adhesive A, and 2.5 parts of sulfur;

[0127] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0128] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0129] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 8.7 N / mm.

[0130] Embodiment 17

[0131] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 15 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 10 parts of resorcinol, 30 parts of white carbon black, 20 parts of adhesive A, and 2.5 parts of sulfur;

[0132] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0133] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0134] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 7.5 N / mm.

[0135] Comparative Example 1

[0136] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, and 200 parts of ethanol; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0137] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0138] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0139] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 5.7 N / mm.

[0140] Comparative Example 2

[0141] The adhesive is made of the following components by weight: 10 parts of resorcinol, 12 parts of adhesive A, 2 parts of 4-amino-5-hexenoic acid, and 200 parts of ethanol; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 30 parts of white carbon black, and 2.5 parts of sulfur;

[0142] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0143] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0144] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 6.2 N / mm.

[0145] Comparative Example 3

[0146] 1) The adhesive is made of the following components by weight: 10 parts of resorcinol, 25 parts of adhesive A, 5 parts of 2-amino-8-nonenoic acid, and 200 parts of solvent; the rubber compound is made of the following components by weight: 100 parts of nitrile rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant RD, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A, and 2.5 parts of sulfur;

[0147] 2) Adhesive coating on nylon 66 cord fabric, followed by drying at 80°C (coating weight after drying: 8 g / m 2 );

[0148] 3) Calender the rubber compound onto the fabric (load 2000g / m 2 );

[0149] 4) Vulcanization at 160°C for 20 min, 15 MPa; after testing, the bonding strength between rubber and fabric is 6.5 N / mm.

[0150] The results of Example 1 and Comparative Example 2 show that the addition of aminocarbonyl acid can greatly increase the bonding strength between rubber and nylon fabric. The results of Example 1 and Comparative Example 1 show that, compared with simply coating the nylon fabric with an adhesive, the bonding strength between rubber and nylon fabric is much lower than adding an adhesive to the rubber compound.

[0151] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for bonding rubber and nylon fabric, characterized in that: The following steps are involved: The surface of the nylon fabric is coated with adhesive, dried, calendered with rubber compound and vulcanized in sequence; The adhesive comprises the following components in parts by weight: 10 parts of resorcinol, 5 to 20 parts of adhesive A, 0.5 to 10 parts of aminocarbolic acid and 30 to 1000 parts of solvent, wherein the aminocarbolic acid has a structure shown in Formula I: In Formula I, R1 and R2 are independently a hydrocarbon group or hydrogen, and R1 and / or R2 contain a carbon-carbon double bond; The rubber compound comprises the following components in parts by mass: 100 parts of rubber, 0-7 parts of zinc oxide, 0-5 parts of stearic acid, 0-10 parts of antioxidant, 1-10 parts of resorcinol, 1-70 parts of white carbon black, 1-15 parts of adhesive A and 0.5-5 parts of vulcanizing agent, and the parts by mass of the zinc oxide, stearic acid and antioxidant are not 0.

2. The bonding method according to claim 1, characterized in that: The adhesive comprises the following components in parts by weight: 10 parts of resorcinol, 12 parts of adhesive A, 2 to 5 parts of aminocarbolic acid and 200 parts of solvent.

3. The bonding method according to claim 1 or 2, characterized in that: The aminocarbolic acid is 4-amino-5-hexenoic acid or 2-amino-8-nonenoic acid.

4. The bonding method according to claim 1, characterized in that: The rubber compound comprises the following components in parts by mass: 100 parts of rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant, 2.5 parts of resorcinol, 30 parts of white carbon black, 3 parts of adhesive A and 2.5 parts of vulcanizing agent.

5. The bonding method according to claim 1 or 4, characterized in that: The vulcanizing agent is sulfur or a peroxide vulcanizing agent.

6. The bonding method according to claim 1 or 4, characterized in that: The rubber includes one or more of nitrile rubber, natural rubber, ethylene propylene rubber, chloroprene rubber, butyl rubber, silicone rubber, styrene butadiene rubber and silicone rubber.

7. The bonding method according to claim 1 or 4, characterized in that: The antioxidant includes one or more of antioxidant RD, antioxidant 4020, antioxidant 4010NA, antioxidant MB, antioxidant MBZ, antioxidant NBC, antioxidant 2246, antioxidant 2246S, antioxidant 246, antioxidant SP, antioxidant 6DDP, antioxidant UOP588, antioxidant UOP788, antioxidant DD, antioxidant AW and antioxidant D.

8. The bonding method according to claim 1, characterized in that: The coating amount after drying is 1 to 50 g / m 2 .

9. The bonding method according to claim 1 or 8, characterized in that: The loading amount of the rubber compound is 50 to 10000 g / m 2 .

10. The bonding method according to claim 1, characterized in that: The vulcanization temperature is 100-180° C., the time is 3-60 min, and the pressure is 10-25 MPa.