Easy-to-spray polypropylene composite material and preparation method thereof
By adding bisaminosilane oligomer and ethylene-vinyl acetate copolymer to polypropylene material, the surface polarity of the material is improved, which solves the problem of difficulty in painting polypropylene material and achieves efficient spray adhesion and improved mechanical properties.
Patent Information
- Application Number
- CN202110997520.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-08-27
AI Technical Summary
Due to the extremely low surface energy and poor polarity of polypropylene materials, it is difficult to carry out effective surface coating. The existing treatment process is costly and difficult to balance stability and operability.
By adding highly polar and easily migrating bisaminosilane oligomer, the surface polarity of the polypropylene material is improved, and combined with ethylene-vinyl acetate copolymer, the surface polarity and spray adhesion strength of the material are improved. Twin-screw extrusion is used Out of the machine for mixing and extrusion processing.
On the premise of ensuring the stability of the material, the surface spraying adhesion strength and mechanical properties of the polypropylene material are significantly improved, the bonding force between the material and the paint film is enhanced, and the painting process is simplified.
Smart Images

Figure BDA0003234345360000011 
Figure BDA0003234345360000061 
Figure FDA0004767076460000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of modified materials, in particular to an easy-to-spray polypropylene composite material and a preparation method thereof. Background Art
[0002] Polypropylene has good mechanical properties and can be directly manufactured or modified to manufacture various mechanical equipment parts, such as industrial pipes, agricultural water pipes, motor fans, infrastructure templates, etc. Modified polypropylene can be molded into bumpers, anti-scratch strips, car steering wheels, instrument panels and interior decorations, as well as insulating shells for household appliances and washing machine liners. It is widely used as an insulating material for wires and cables and other electrical appliances.
[0003] While polypropylene is widely used, the demand for the appearance and decoration of polypropylene materials is also increasing. However, since polypropylene is a non-polar crystalline material, its surface energy is extremely low, the surface wettability is poor, and the polarity difference with the coating components is too large, which makes it difficult to carry out surface coating operations on polypropylene materials. Therefore, it is necessary to perform additional treatment processes on the surface of polypropylene to improve the surface polarity of the product. Common treatment processes include: flame treatment, chemical oxidation treatment, corona discharge treatment, plasma treatment, surface coating treatment, etc. The use of such methods is not only costly, but also stability and operability cannot be guaranteed at the same time. Summary of the invention
[0004] The object of the present invention is to provide an easy-to-spray polypropylene composite material and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology. Under the premise of ensuring the stability of the material, the surface polarity of the material is improved by adding a highly polar and easily migrating bisaminosilane polymer, thereby improving its surface spray adhesion strength.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] The first aspect of the present invention discloses an easy-to-spray polypropylene composite material, which is prepared from the following raw materials in parts by weight:
[0007]
[0008]
[0009] As a further solution of the present invention: the melt flow rate of the copolymerized polypropylene is 25-35 g / 10 min at 230°C / 2.16 kg, and the notched impact strength is ≥8 KJ / m 2 .
[0010] As a further solution of the present invention: the mass concentration of vinyl acetate in the ethylene-vinyl acetate copolymer is 25-45%. Vinyl acetate is an important component of the copolymer to enhance the surface polarity. Vinyl acetate has a high polarity. If the content is too low, the use effect cannot be achieved. If the content is too high, the overall rigidity and heat resistance of the composite material will be affected.
[0011] As a further solution of the present invention: the water content of the bisaminosilane oligomer is ≤1%, the silicone content in the bisaminosilane oligomer is ≥85%, and silicone is an effective ingredient therein, which plays an amphiphilic role, increases surface polarity, and improves paint surface bonding.
[0012] As a further solution of the present invention: the inorganic filler is talcum powder, and the particle size of the talcum powder is 4-8 μm.
[0013] As a further solution of the present invention: the other additives include toughening agents, antioxidants and lubricants.
[0014] As a further solution of the present invention: the toughening agent is an ethylene-octene copolymer, the melt flow rate of which is 4-6 g / 10 min at 190°C / 2.16 kg and the density is ≤0.88 g / cm 3 .
[0015] As a further embodiment of the present invention: the antioxidant is at least three of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, n-octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris-(2,4-di-tert-butylphenyl)phosphite, and distearyl thiodipropionate.
[0016] As a further solution of the present invention: the lubricant is a mixture of ethylene bisstearamide, white oil and calcium stearate in a mass ratio of 2:2:1.
[0017] The second aspect of the present invention discloses a method for preparing the easy-to-spray polypropylene composite material as described above, comprising the following steps:
[0018] S1: Weigh copolymerized polypropylene, ethylene-vinyl acetate copolymer, bisaminosilane oligomer, talcum powder, toughening agent, antioxidant and lubricant according to weight parts, add them into a high-speed mixer and mix them thoroughly for 5-15 minutes to obtain a mixed material;
[0019] S2: adding the mixture obtained in step S1 into a twin-screw extruder for mixing and extrusion, cooling and pelletizing to obtain easy-to-spray polypropylene composite material pellets;
[0020] Wherein, the extrusion temperatures in each extrusion zone of the twin-screw extruder are 175-185°C, 180-190°C, 190-200°C, 200-210°C, 200-210°C, 200-210°C, 200-210°C, 200-210°C, 200-210°C, 200-210°C, and 220-230°C respectively.
[0021] Compared with the prior art, the present invention has the following beneficial effects: the bisaminosilane oligomer added by the present invention has the characteristics of high polarity and easy migration, which can not only effectively improve the surface polarity of the material and improve the adhesion strength of the spray paint, but also act as an effective powder dispersant to prevent the agglomeration of the filling powder, further improving the mechanical properties of the material; the vinyl acetate component in the ethylene-vinyl acetate added by the present invention has a strong polarity, which can significantly improve the surface polarity of the material, improve the bonding force between the surface of the material and the paint film, and improve the spray performance of the material. In addition, the copolymer can be effectively compatible with copolymerized polypropylene and toughening agents, has little effect on the overall mechanical properties of the material, and does not affect the application range of the material. DETAILED DESCRIPTION
[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] The specific information of the raw materials used in the following examples and comparative examples is as follows:
[0024] Copolymer polypropylene, brand PP-K7227H, purchased from Sino-Korea Petrochemical;
[0025] Ethylene-vinyl acetate copolymer, with a vinyl acetate content of 25-45, brand 210W, purchased from DuPont, USA;
[0026] Bisaminosilane oligomer, with a water content of ≤1% and a silicone content of ≥85%, brand SIC6652, purchased from Guangzhou Silicon Carbon New Materials;
[0027] The inorganic filler is talcum powder, with an average particle size of 4-8 μm, brand AH51210L, purchased from Liaoning Aihai;
[0028] Toughening agent, which is ethylene-octene copolymer, with a melt flow rate of 4-6g / 10min at 190℃ / 2.16kg and a density of ≤0.88g / cm 3 , brand 8200, purchased from Dow Chemical;
[0029] An antioxidant, which is a mixture of at least three of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol (i.e., antioxidant 1010), β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate octadecyl (i.e., antioxidant 1076), tris-(2,4-di-tert-butylphenyl)phosphite (i.e., antioxidant 168), and distearyl thiodipropionate (i.e., antioxidant DSTDP), all purchased from BASF;
[0030] The lubricant is a mixture of ethylene bisstearamide, white oil and calcium stearate in a mass ratio of 2:2:1, all of which are commercially available products.
[0031] In addition, "parts" described in the Examples and Comparative Examples refer to parts by weight unless otherwise specified.
[0032] Example 1
[0033] 60 parts of copolymerized polypropylene, 10 parts of ethylene-vinyl acetate copolymer, 10 parts of toughening agent, 0.5 parts of bisaminosilane oligomer, 20 parts of talc, 0.5 parts of antioxidant and 0.5 parts of lubricant are added into a high mixer and mixed for 5-15 minutes; then the uniformly mixed materials are added into a twin-screw extruder, mixed and extruded, cooled and pelletized to obtain easy-to-spray polypropylene composite material pellets 1; wherein the extrusion temperatures of each extrusion zone in the twin-screw extruder are 175°C, 180°C, 190°C, 200°C, 200°C, 200°C, 200°C, 200°C, 200°C and 220°C respectively.
[0034] Example 2
[0035] 70 parts of copolymerized polypropylene, 8 parts of ethylene-vinyl acetate copolymer, 7 parts of toughening agent, 0.7 parts of bisaminosilane oligomer, 15 parts of talc, 0.5 parts of antioxidant and 0.5 parts of lubricant are added into a high mixer and mixed for 5-15 minutes; then the uniformly mixed materials are added into a twin-screw extruder, mixed and extruded, cooled and pelletized to obtain easy-to-spray polypropylene composite material pellets 2; wherein the extrusion temperatures of each extrusion zone in the twin-screw extruder are 180°C, 185°C, 195°C, 205°C, 205°C, 205°C, 205°C, 205°C, 225°C respectively.
[0036] Example 3
[0037] 80 parts of copolymerized polypropylene, 5 parts of ethylene-vinyl acetate copolymer, 5 parts of toughening agent, 1.0 part of bisaminosilane oligomer, 10 parts of talc, 0.5 parts of antioxidant and 0.5 parts of lubricant are added into a high mixer and mixed for 5-15 minutes; then the uniformly mixed materials are added into a twin-screw extruder, mixed and extruded, and cooled and pelletized to obtain easy-to-spray polypropylene composite material pellets 3; wherein the extrusion temperatures of each extrusion zone in the twin-screw extruder are 185°C, 190°C, 200°C, 210°C, 210°C, 210°C, 210°C, 210°C, 210°C and 230°C respectively.
[0038] Comparative Example 1
[0039] 70 parts of copolymerized polypropylene, 7 parts of toughening agent, 0.7 parts of bisaminosilane oligomer, 15 parts of talc, 0.5 parts of antioxidant and 0.5 parts of lubricant are added into a high mixer and mixed for 5-15 minutes; then the uniformly mixed materials are added into a twin-screw extruder, mixed and extruded, and after cooling and pelletizing, easy-to-spray polypropylene composite material pellets 4 are obtained; wherein the extrusion temperatures in each extrusion zone of the twin-screw extruder are 180°C, 185°C, 195°C, 205°C, 205°C, 205°C, 205°C, 205°C, 225°C respectively.
[0040] Comparative Example 2
[0041] 70 parts of copolymerized polypropylene, 8 parts of ethylene-vinyl acetate copolymer, 7 parts of toughening agent, 15 parts of talc, 0.5 parts of antioxidant and 0.5 parts of lubricant are added into a high mixer and mixed for 5-15 minutes; then the uniformly mixed materials are added into a twin-screw extruder, mixed and extruded, and cooled and pelletized to obtain easy-to-spray polypropylene composite material pellets 5; wherein the extrusion temperatures of each extrusion zone in the twin-screw extruder are 180°C, 185°C, 195°C, 205°C, 205°C, 205°C, 205°C, 205°C, 205°C and 225°C respectively.
[0042] Comparative Example 3
[0043] 70 parts of copolymerized polypropylene, 8 parts of ethylene-vinyl acetate copolymer, 7 parts of toughening agent, 0.7 parts of epoxy silane polymer, 15 parts of talc, 0.5 parts of antioxidant and 0.5 parts of lubricant are added into a high mixer and mixed for 5-15 minutes; then the uniformly mixed materials are added into a twin-screw extruder, mixed and extruded, cooled and pelletized to obtain easy-to-spray polypropylene composite material pellets 6; wherein the extrusion temperatures of each extrusion zone in the twin-screw extruder are 180°C, 185°C, 195°C, 205°C, 205°C, 205°C, 205°C, 205°C, 225°C respectively.
[0044] The obtained easy-to-spray polypropylene composite material pellets 1-6 were tested. The following Table 1 shows the test items and standards:
[0045] Table 1: Test items and standards
[0046] Test items / units Test Standards Tensile strength / Mpa ISO 527 Bending strength / Mpa ISO 178 Flexural modulus / Mpa ISO 178 Izod notched impact strength / KJ / ㎡ ISO 180 Dyne value Dyne pen test 100 grid test GB / T 9286
[0047] Note: The test conditions and test specimen dimensions in Table 1 are as follows:
[0048] Tensile strength test: 1A type molded specimen, tensile speed 50mm / min;
[0049] Bending strength and bending modulus: sample size 100mm*10mm*4mm, test speed: 2mm / min;
[0050] Izod notched impact strength: A-type molded notch, sample size 100mm*10mm*4mm;
[0051] Dyne value: For injection molded samples that are flat and free of surface defects, a line of 30 mm is drawn, and no shrinkage beads of dyne liquid appear within 3 seconds;
[0052] 100-grid test: The sample is flat and has no surface defects. The size is 150mm*100mm. It is only cleaned and blown dry before spraying, without other pre-treatment procedures. The paint film thickness is 61-120μm, and the paint surface should contain at least primer and color paint.
[0053] The test results of the easy-to-spray polypropylene composite material pellets 1-6 are shown in Table 2:
[0054] Table 2: Test results
[0055]
[0056] It can be seen from Table 2 that the dyne value and the baic test value of the polypropylene composite materials in Examples 1-3 are better than those in Comparative Examples 1-3, indicating that the bonding force between the polypropylene surface and the coating can be improved by adding ethylene-vinyl acetate and bisaminosilane oligomer at the same time, and a polypropylene composite material more suitable for spraying can be obtained. Combining Example 2 with Comparative Example 1, it can be seen that ethylene-vinyl acetate copolymer contributes to the easy spraying performance of the polypropylene composite material. It can be seen from Example 2, Comparative Example 2 and Comparative Example 3 that bisaminosilane oligomer not only improves the dyne value and baic test of the material, but also improves its mechanical properties.
[0057] Although this specification is described according to implementation modes, not every implementation mode includes only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
[0058] Therefore, the above description is only a preferred embodiment of the present application and is not intended to limit the scope of implementation of the present application; that is, all equivalent changes made according to the scope of the claims of the present application are within the protection scope of the claims of the present application.
Claims
1. An easy-to-spray polypropylene composite material, characterized in that: It is prepared from the following raw materials in parts by weight: The mass concentration of vinyl acetate in the ethylene-vinyl acetate copolymer is 25-45%; The water content of the bisaminosilane oligomer is ≤1%, and the organic silicon content in the bisaminosilane oligomer is ≥85%.
2. The easy-to-spray polypropylene composite material according to claim 1, characterized in that: The melt flow rate of the copolymerized polypropylene is 25-35 g / 10 min at 230°C / 2.16 kg, and the notched impact strength is ≥8 KJ / m 2 .
3. The easy-to-spray polypropylene composite material according to claim 1, characterized in that: The inorganic filler is talcum powder, and the particle size of the talcum powder is 4-8 μm.
4. The easy-to-spray polypropylene composite material according to claim 1, characterized in that: The other additives include toughening agents, antioxidants and lubricants.
5. The easy-to-spray polypropylene composite material according to claim 4, characterized in that: The toughening agent is ethylene-octene copolymer, the melt flow rate of which is 4-6 g / 10 min at 190 ° C / 2.16 kg, and the density is ≤ 0.88 g / cm 3 .
6. The easy-to-spray polypropylene composite material according to claim 4, characterized in that: The antioxidant is at least three of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, n-octadecylβ-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris-(2,4-di-tert-butylphenyl)phosphite, and distearyl thiodipropionate.
7. The easy-to-spray polypropylene composite material according to claim 4, characterized in that: The lubricant is prepared by mixing ethylene bisstearamide, white oil and calcium stearate in a mass ratio of 2:2:
1.
8. The method for preparing an easily sprayable polypropylene composite material according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1: Weigh copolymerized polypropylene, ethylene-vinyl acetate copolymer, bisaminosilane oligomer, talcum powder, toughening agent, antioxidant and lubricant according to weight parts, add them into a high-speed mixer and mix them thoroughly for 5-15 minutes to obtain a mixed material; S2: adding the mixture obtained in step S1 into a twin-screw extruder for mixing and extrusion, cooling and pelletizing to obtain easy-to-spray polypropylene composite material pellets; Wherein, the extrusion temperatures in each extrusion zone of the twin-screw extruder are 175-185°C, 180-190°C, 190-200°C, 200-210°C, 200-210°C, 200-210°C, 200-210°C, 200-210°C, 200-210°C, 200-210°C, and 220-230°C respectively.