Sodium ion battery and its modified hard carbon negative electrode
By using caffeic acid in situ coating technology in hard carbon negative electrode materials, a uniform coating film is formed, which solves the problem of insufficient performance of hard carbon negative electrode materials in sodium ion batteries, and achieves efficient performance improvement of sodium ion batteries. It is suitable for the Commercial application.
Patent Information
- Application Number
- CN202211670116.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-25
AI Technical Summary
The existing hard carbon anode materials have low first-week Coulomb efficiency, poor rate performance and undesirable cycle performance in sodium ion batteries, and the modification process is complex and cannot form a uniform coating film, which limits the commercialization of sodium ion batteries. application.
By using xylose, glucose or trehalose as hard carbon precursors, hydrothermal reaction and carbonization are performed, caffeic acid is added to form an aqueous solution, and dehydration is carried out at high temperature to form an in-situ coating film to enhance the hard carbon negative electrode Comprehensive performance.
It achieves the first-week Coulomb efficiency of hard carbon anode with an exceeding 90% of the first-week Coulomb efficiency, excellent rate performance and cycle performance, and the process is simple and controllable, with low cost, which is suitable for large-scale production.
Smart Images

Figure BDA0004015974030000051 
Figure BDA0004015974030000052 
Figure BDA0004015974030000061
Abstract
Description
Technical Field
[0001] The invention relates to a sodium ion battery, and in particular to a modified hard carbon negative electrode thereof. Background Art
[0002] Developing and utilizing renewable clean energy, developing "green energy" and "low-carbon economy" to seek sustainable development are key means for my country to deal with energy crises, increasingly prominent environmental pollution and greenhouse effects. Electrochemical energy storage technology can efficiently store and convert intermittent green energy such as wind energy, solar energy, tidal energy, geothermal energy, etc. Among them, lithium-ion batteries have been successfully commercialized. However, factors such as the limited reserves of lithium mineral resources and the uneven distribution of lithium resources have caused social concerns about whether green energy is sustainable. In this context, it is crucial to develop a new energy storage system with low cost and excellent performance. Thanks to the abundant sodium reserves, environmental friendliness, and similar electrochemical properties between sodium and lithium, sodium-ion batteries are considered to be high-quality, low-cost supplementary products for the future energy storage industry. They are considered to be one of the most promising alternatives to lithium-ion batteries and are expected to be used in large-scale energy storage and smart grids. In recent years, the country has also successively issued many relevant documents to promote the commercialization of sodium-ion batteries and guide their high-quality development.
[0003] The development of advanced sodium-ion batteries depends on the construction of high-performance electrode materials. The research and development of low-cost, high-performance negative electrode materials is a key link. Hard carbon (HC) materials have the advantages of abundant reserves, low cost, stable structure, and low sodium insertion voltage platform, making hard carbon the most commercially promising negative electrode material. However, hard carbon negative electrodes are still constrained by bottlenecks such as low first-cycle coulombic efficiency, poor rate performance, and unsatisfactory cycle performance. These performance indicators are key factors in promoting the commercialization of sodium-ion batteries. Although there are a large number of optimized process methods to modify the structure, composition, surface functionalization, etc. of hard carbon materials, these methods can often only improve a single property of the hard carbon negative electrode. For example, although the reversible capacity of sodium storage is improved by introducing doping defects, the first cycle coulombic efficiency is significantly reduced; although the construction of a porous structure promotes the diffusion and rate performance of the electrolyte, the decomposition of the electrolyte is aggravated, and the first cycle coulombic efficiency is also significantly reduced; reducing defects and porosity, although the first cycle coulombic efficiency is improved and the electrode electrolyte interface is stabilized, the reversible capacity and rate performance cannot be guaranteed; or by depositing a coating layer on the hard carbon surface, the contact between the electrolyte and the electrode surface can be blocked, thereby alleviating the decomposition of the electrolyte and optimizing the electrode electrolyte interface, thereby improving the first cycle coulombic efficiency and reversible capacity; however, since the deposited coating layer is non-conductive and has no electrochemical activity, the rate performance and cycle performance of the battery are still not ideal. In addition, the surface coating methods that have been reported or studied require very complex equipment, complicated operation processes, and cannot controllably form a uniform coating film on the hard carbon surface.
[0004] Therefore, it is urgent to develop more effective optimization strategies to improve the sodium storage performance of hard carbon anodes in multiple dimensions, so as to promote the commercial application of sodium-ion batteries based on hard carbon anodes. Summary of the invention
[0005] The object of the present invention is to provide a modified hard carbon negative electrode material for a sodium ion battery, which can at least overcome or improve some of the above-mentioned shortcomings.
[0006] According to a first aspect of the present invention, a method for preparing a hard carbon negative electrode material for a sodium ion battery is provided, comprising:
[0007] providing a hard carbon precursor selected from at least one of xylose, glucose, sucrose and trehalose;
[0008] The hard carbon precursor is dissolved in water and then subjected to a hydrothermal reaction, wherein the hydrothermal reaction temperature is 180 to 240° C. and the hydrothermal reaction time is 18 to 28 hours;
[0009] The hydrothermal reaction product is separated by centrifugation and washed and dried to obtain an intermediate powder;
[0010] The obtained intermediate powder is carbonized under inert atmosphere to obtain hard carbon powder, wherein the carbonization temperature is 1000-1400° C. and the holding time is 2-4 hours;
[0011] The obtained hard carbon powder is dissolved in water and then caffeic acid is added to form an aqueous solution, wherein the mass ratio of the added caffeic acid to the hard carbon powder is 5% to 20%;
[0012] heating and stirring the formed aqueous solution until the water is completely evaporated to obtain a composite powder; and
[0013] The obtained composite powder is subjected to high-temperature dehydration treatment under vacuum conditions to obtain a hard carbon negative electrode material, wherein the temperature of the high-temperature dehydration treatment is 130-150°C.
[0014] According to the preparation method of the present invention, the heating rate of the carbonization treatment is preferably 1-5°C / min.
[0015] According to the preparation method of the present invention, the drying temperature is preferably 50-70°C.
[0016] According to the preparation method of the present invention, the time of high temperature dehydration treatment is preferably 10 to 14 hours.
[0017] According to the preparation method of the present invention, the temperature when the aqueous solution is heated and stirred is preferably controlled to be about 80°C.
[0018] According to the preparation method of the present invention, the mass ratio of the added caffeic acid to the hard carbon powder is preferably 15%.
[0019] According to the preparation method of the present invention, the hard carbon precursor is preferably xylose.
[0020] According to a second aspect of the present invention, there is provided a sodium ion battery comprising a negative electrode made from the hard carbon negative electrode material prepared according to the above method.
[0021] According to the sodium ion battery of the present invention, the negative electrode is preferably prepared by forming a slurry of the hard carbon negative electrode material, carbon black and sodium alginate, coating the slurry on the current collector and drying the slurry under vacuum conditions. In this case, the mass ratio of the hard carbon negative electrode material, carbon black and sodium alginate is preferably 8:1:1.
[0022] The sodium ion battery according to the present invention further includes a charge and discharge test on the battery, wherein the test voltage range is 0.01-2.5V.
[0023] According to the sodium ion battery of the present invention, after the initial discharge process of the battery, the modifier caffeic acid will self-polymerize in situ on the surface of the hard carbon material due to electrochemical action to form a coating layer, which is critical to comprehensively improve the comprehensive performance of the hard carbon negative electrode. The sodium ion battery hard carbon negative electrode of the present invention therefore has excellent comprehensive performance, with an ultra-high first-cycle coulomb efficiency of more than 90%, excellent rate performance and cycle performance, etc.
[0024] In addition, the preparation process of the hard carbon negative electrode material of the present invention is simple and controllable, the reaction conditions are mild, the cost is low, and it is easy to realize large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 and Figure 2 They are TEM images of P-HC and HC-CA-15% prepared in Example 1, respectively.
[0026] Figure 3 The first week charge and discharge curves of the original hard carbon and caffeic acid coated hard carbon negative electrode prepared in Example 1 of the present invention.
[0027] Figure 4 The rate performance of the original hard carbon and caffeic acid coated hard carbon negative electrode prepared in Example 1 of the present invention.
[0028] Figure 5 The long cycle performance of the original hard carbon and caffeic acid coated hard carbon negative electrode prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0029] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the embodiments described herein are only used to illustrate and not to limit the present invention.
[0030] Example 1
[0031] Step (1): 8 g of xylose was weighed and dissolved in 70 mL of deionized water to form a transparent solution, which was transferred to a high-pressure reactor for hydrothermal reaction at 220° C. for 24 h. After cooling to room temperature, the obtained brown suspension was washed several times by centrifugation with water and ethanol, and then placed in a vacuum oven at 60° C. to dry overnight.
[0032] Step (2): Pour the brown powder obtained after drying into a crucible, transfer it to a tube furnace, and heat it to 1200°C at a heating rate of 3°C / min under an argon inert atmosphere for carbonization for 3 hours. When the tube furnace cools to room temperature, pristine hard carbon (P-HC) material powder is obtained after carbonization.
[0033] Step (3): 200 mg of hard carbon material powder was dispersed in 50 mL of deionized water and stirred evenly, and then 15% of the mass of the hard carbon material powder was added with caffeic acid (CA) and the mixture was stirred and mixed evenly.
[0034] Step (4): The mixed solution of the hard carbon material powder and caffeic acid is continuously stirred at 80°C until the water evaporates completely to obtain a composite powder of hard carbon and caffeic acid. The composite powder is then transferred to a vacuum oven and heat treated at 140°C for 12 hours for dehydration, so that a chemical reaction is formed between the hard carbon surface and the caffeic acid, and finally a hard carbon negative electrode powder material with 15% caffeic acid (abbreviated as HC-CA-15%) is obtained.
[0035] Step (5): The hard carbon negative electrode powder material is mixed with carbon black and sodium alginate binder in a ratio of (8:1:1) to form a slurry, which is then scraped onto a copper foil current collector, dried at 80°C in vacuum for 24 hours, and cut into pieces to obtain electrode sheets, which are used as working electrodes. In a glove box under an argon atmosphere, a sodium sheet is used as a counter electrode, and the positive electrode shell, negative electrode shell, glass fiber diaphragm, sodium sheet, and electrolyte are assembled into a CR2025 button battery according to the correct operating steps. The electrolyte used is 1M NaPF6 EC / DEC. After the assembled battery is left to stand for 24 hours, a constant current charge and discharge test and a rate performance test are performed in a blue power test system with a voltage range of 0.01-2.5V. During the initial (first cycle) discharge of the battery, the electrochemical process induces the caffeic acid small molecules connected to the hard carbon surface to undergo anionic self-polymerization, thereby in situ coating a layer of polymer film on the hard carbon surface.
[0036] Figure 1 is the TEM image of the original hard carbon P-HC; Figure 2 This is a TEM image of 15% caffeic acid HC-CA-15% after self-polymerization to form a coating film. Figure 3 The first-week charge-discharge curves and first-week Coulombic efficiency of the original hard carbon and caffeic acid-coated hard carbon. Figure 4 Rate performance of original hard carbon and caffeic acid coated hard carbon. Figure 5 Long cycle performance of pristine hard carbon and caffeic acid coated hard carbon.
[0037] Embodiments 2 to 4
[0038] The addition ratio of caffeic acid CA in step (3) of Example 1 was adjusted to 5%, 10%, and 20%, respectively, and the samples were named HC-CA-5%, HC-CA-10%, and HC-CA-20%, and then Examples 2 to 4 were carried out in sequence, and the other parts remained unchanged. Table 1 shows the sodium ion battery performance of the hard carbon prepared in Examples 1 to 4.
[0039] Table 1
[0040]
[0041] Embodiments 5 to 7
[0042] The hard carbon precursor in step (1) of Example 1 was replaced by glucose, sucrose, and trehalose respectively, while the others remained unchanged, and Examples 5 to 7 were carried out in sequence. The test results are shown in Table 2. Table 2 shows the sodium ion battery performance of the hard carbon negative electrode obtained in Examples 5 to 7.
[0043] Table 2
[0044]
[0045] Comparative Examples 1-3
[0046] The rest is the same as Example 1, except that the caffeic acid in step (3) is replaced by glycine, fulvic acid, and lactic acid, respectively, to complete Comparative Examples 1 to 3 in sequence.
[0047] The hard carbon materials prepared in Comparative Examples 1 to 3 were made into electrode sheets and assembled into sodium ion batteries for electrochemical performance testing. The test results are shown in Table 3.
[0048] Table 3
[0049]
[0050] from Figure 1 and Figure 2 The comparative analysis of TEM images shows that the in-situ coating technology of the present invention can successfully construct a uniformly distributed coating on the hard carbon surface.
[0051] The electrochemical performance tests of the original hard carbon and caffeic acid coated hard carbon materials prepared in Examples 1 to 4 show (see Table 1) that in-situ coating of a caffeic acid layer on the hard carbon surface can effectively improve the first-week coulombic efficiency, rate performance and cycle stability of the hard carbon material. However, there should be an optimal ratio for the construction of the coating layer. Because an overly thick coating layer will lead to a larger internal resistance and ion transport resistance, thus affecting the performance improvement. The test results show that when the mass proportion of caffeic acid is 15%, the prepared hard carbon material has the best electrochemical performance, and its first-week coulombic efficiency can be increased from 69% to 93.2% ( Figure 3 ); the reversible capacity increased from 329.3mAh / g to 379.6mAh / g; and maintained good rate performance, with the capacity maintained at 160.5mAh / g (0.6A / g(2C)) at a current density of 0.6A / g Figure 4 ); after 500 cycles at a current density of 0.05A / g, the capacity retention rate can reach 95.4% ( Figure 5 ).
[0052] Examples 5 to 7 also show that, from the battery performance test results (Table 2), the first-week coulombic efficiency of the hard carbon negative electrode obtained from several other sugar small molecule precursors also exceeded 87%, the reversible capacity was also around 360 mAh / g, and good rate performance was maintained. This shows that the in-situ reconstruction technology provided by the present invention has universality and can be extended to modify other hard carbon materials.
[0053] The principle of the in-situ coating modification of caffeic acid of the present invention can be explained as follows: due to the presence of unsaturated carbon-carbon double bonds in caffeic acid molecules, during the initial discharge process of the battery, when electrons are transferred from the hard carbon surface to the caffeic acid, an anionic polymerization reaction is induced, that is, the carbon-carbon double bonds in adjacent caffeic acid molecules are opened and cross-linked, thereby forming an in-situ coating layer on the hard carbon surface.
[0054] Comparative Examples 1 to 3 provide three small molecules that are also rich in characteristic oxygen groups (such as hydroxyl groups, carboxyl groups, etc.). However, due to the absence of unsaturated carbon-carbon double bonds, although they will be adsorbed on the hard carbon surface, they will not form a coating film, and therefore fail to effectively modify the hard carbon surface. The test results in Table 3 show that compared with the original hard carbon, the addition of this type of modifier has extremely limited improvement in the performance of the hard carbon negative electrode. In addition, since this type of modifier itself is not conductive, its addition will increase the internal resistance of the hard carbon negative electrode, thus affecting the capacity and rate performance of the modified negative electrode. This further demonstrates the particularity and effectiveness of the in-situ coating modification of caffeic acid in the present invention.
Claims
1. A method for preparing a hard carbon negative electrode material for a sodium ion battery, comprising: providing a hard carbon precursor selected from at least one of xylose, glucose, sucrose and trehalose; The hard carbon precursor is dissolved in water and then subjected to a hydrothermal reaction, wherein the hydrothermal reaction temperature is 180 to 240° C. and the hydrothermal reaction time is 18 to 28 hours; The hydrothermal reaction product is separated by centrifugation and washed and dried to obtain an intermediate powder; The obtained intermediate powder is carbonized under inert atmosphere to obtain hard carbon powder, wherein the carbonization temperature is 1000-1400° C., the holding time is 2-4 hours, and the heating rate is 1-5° C. / min; The obtained hard carbon powder is dissolved in water and then caffeic acid is added to form an aqueous solution, wherein the mass ratio of the added caffeic acid to the hard carbon powder is 5% to 20%; heating and stirring the formed aqueous solution until the water is completely evaporated to obtain a composite powder; and The obtained composite powder is subjected to high-temperature dehydration treatment under vacuum conditions to obtain a hard carbon negative electrode material, wherein the temperature of the high-temperature dehydration treatment is 130-150°C.
2. The preparation method according to claim 1, wherein the high temperature dehydration treatment time is 10 to 14 hours.
3. The preparation method according to claim 1, wherein the temperature when the aqueous solution is heated and stirred is controlled to be 80°C.
4. The preparation method according to claim 1, wherein the mass ratio of the added caffeic acid to the hard carbon powder is 15%. The preparation method according to claim 1 , wherein the hard carbon precursor is xylose.
6. A sodium ion battery comprising a negative electrode made from a hard carbon negative electrode material prepared by a method according to any one of claims 1 to 5.
7. The sodium ion battery according to claim 6, wherein the negative electrode is prepared by forming a slurry from the hard carbon negative electrode material, carbon black and sodium alginate, coating the slurry on a current collector and drying the slurry under vacuum conditions.
8. The sodium ion battery according to claim 7, wherein the mass ratio of the hard carbon negative electrode material, carbon black and sodium alginate is 8:1:
1.
9. The sodium ion battery according to claim 6, further comprising a charge and discharge test on the battery, wherein the test voltage range is 0.01-2.5V.