A method for preparing highly surface-active materials

By stirring hydrothermal treatment and heat treatment in sodium hydroxide solution, a highly surface-active titanium dioxide nanostructure is prepared, which solves the problem of low conductivity and conductivity rate of titanium dioxide electrode materials and improves the capacity and cycle stability of sodium-ion batteries.

CN115947368BActive Publication Date: 2024-10-18佛山(华南)新材料研究院
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211615076.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-14
Publication Date
2024-10-18
Estimated Expiration
2042-12-14

AI Technical Summary

Technical Problem

Titanium dioxide has low electronic conductivity and sodium ion conductivity among electrode materials, making it difficult to achieve fast charging and capacity performance of sodium-ion batteries, and it is difficult for existing preparation processes to achieve a one-step construction of highly dispersed and stable heterogeneous nanostructures.

Method used

By in-situ stirring and hydrothermal treatment of ferric chloride and titanium dioxide P25 nanoparticles in a sodium hydroxide solution, a composite precursor of ferric oxide and titanate is obtained, followed by proton exchange in a hydrochloric acid solution to obtain iron-doped metatitanic acid. Nanosheets and heat treatment in air to prepare highly surface active materials.

Benefits of technology

The prepared high surface active material has good specific capacity and rate performance, increased surface charge transmission and ion migration rate, significantly improved electrode performance, strong process controllability, and can obtain titanium dioxide heterogeneous nanosheet substrates of different sizes and different loads. Large and small iron oxide quantum dots.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115947368B_ABST
    Figure CN115947368B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a high-surface-activity material. After in-situ stirring hydrothermal treatment and heat treatment, a high-surface-activity nano heterostructure can be prepared in-situ during the hydrothermal process. The overall preparation process is simple, and the product is stable and easy to disperse. The material prepared by the invention has a high-activity surface heterostructure, which is beneficial to surface charge transmission and ion migration. The prepared electrode has good specific capacity and rate performance. The process controllability of the invention is strong. By changing the process conditions, titanium dioxide heterogeneous nanosheet substrates of different sizes and iron oxide quantum dots loaded with different sizes can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material preparation, and in particular to a method for preparing a highly active material. Background Art

[0002] Lithium-ion batteries are the most popular electrochemical energy storage technology currently being studied and have been widely used in portable electronic devices, electric vehicles and other fields. However, with the increasing demand for lithium-ion batteries, the consumption of lithium has increased year by year, and the price has continued to rise. Therefore, it is necessary to find suitable energy storage methods and technologies to supplement the lithium-ion battery system. Sodium-ion energy storage, due to its abundant reserves and low price, is more suitable for the development and upgrading of China's new energy industry. Titanium dioxide has attracted much attention due to its advantages such as wide sources, low prices, environmental friendliness, high storage capacity and good structural stability. However, among electrode materials, the electronic conductivity and sodium ion conduction rate of titanium dioxide are both low, making it difficult for the assembled sodium-ion battery to meet the fast charging and capacity performance standards. To solve the above problems, researchers began to design and prepare nanostructured titanium dioxide as a new type of sodium-ion energy storage material. The purpose is to enhance the fast sodium storage performance by shortening the diffusion distance of charge in the solid electrode. However, from the perspective of the surface and interface structure of nanomaterials, due to the lack of surface and interface heterojunctions, the electron migration and ion exchange between energy storage sites in a single nanostructure are relatively slow. From the perspective of material structure design, the rational construction of titanium dioxide surface electron transport and composite structure can not only enhance the inherent surface activity and energy storage sites of the nanostructure to a certain extent to enhance the capacity, but also increase the rate of electron surface transport and recombination to improve the rate performance of the electrode. The preparation of titanium dioxide nanostructures based on the hydrothermal growth method is a common preparation method. However, this method has a long preparation process and utilizes the liquid-liquid interface hydrolysis polymerization mechanism. However, the selection of raw materials is complex, and it is difficult to achieve a one-step method to construct highly dispersed and stable heterogeneous nanostructures. Therefore, it is extremely important to optimize the process to prepare new titanium dioxide nanostructures with high surface activity. Summary of the invention

[0003] Based on this, in order to solve the problem that the material in the prior art lacks surface heterojunctions and the electron migration and ion exchange between energy storage sites in a single nanostructure are relatively slow, the present invention provides a method for preparing a highly active material, and the specific technical solution is as follows:

[0004] A method for preparing a high-surface-activity material comprises the following steps:

[0005] Ferric chloride and titanium dioxide P25 nanoparticles are dispersed in a sodium hydroxide solution, stirred in situ and subjected to hydrothermal treatment to obtain a composite precursor of ferric oxide and titanate;

[0006] Proton exchange of the ferric oxide and titanate composite precursor in a hydrochloric acid solution is performed to obtain iron-doped metatitanate nanosheets;

[0007] The iron-doped metatitanate nanosheets are subjected to heat treatment in air to obtain a high-surface activity material.

[0008] Furthermore, the titanium source is titanium dioxide P25 nanoparticles.

[0009] Furthermore, the titanium dioxide nanoparticles are in anatase phase, rutile phase, or a mixture of the two.

[0010] Furthermore, the mass ratio of the titanium dioxide P25 nanoparticles to the ferric chloride is 1:1 to 1:10.

[0011] Furthermore, the parameters of the in-situ stirring hydrothermal treatment are: the in-situ stirring rate is 100r / min to 600r / min; the temperature of the hydrothermal treatment is 100°C to 200°C; and the time of the hydrothermal treatment is 10h to 48h.

[0012] Furthermore, the temperature of the heat treatment is 300 to 1300° C., and the time of the heat treatment is 3 to 150 minutes.

[0013] Furthermore, the alkali solution is one or more of sodium hydroxide aqueous solution, ammonia water, and potassium hydroxide aqueous solution.

[0014] Furthermore, the concentration of the alkali solution is 1 mol / L to 10 mol / L.

[0015] Furthermore, the protonation treatment time is 1 to 10 hours, and the insulation treatment temperature is 25 to 100°C.

[0016] Furthermore, the surface of the high surface activity material is a nano-heterogeneous structure with a specific surface area of ​​50m 2 / g~200m 2 / g, and the particle size distribution is 2nm~50nm.

[0017] In the above scheme, after in-situ stirring hydrothermal and heat treatment, a high surface activity nano heterostructure can be prepared in situ during the hydrothermal process, the overall preparation process is simple, and the product is stable and easy to disperse; the material prepared by the present invention has a high active surface heterostructure, which is beneficial to surface charge transfer and ion migration, and the prepared electrode has good specific capacity and rate performance, and the process controllability of the present application is strong. By changing the process conditions, titanium dioxide heterogeneous nanosheet substrates of different sizes and iron oxide quantum dots loaded with different sizes can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a scanning electron microscope photo of the composite precursor of ferric oxide and titanate in Example 1 of the present invention, which is magnified 50,000 times;

[0019] Figure 2 This is a scanning electron microscope photo of the iron oxide quantum dots / titanium dioxide heterogeneous nanosheets in Example 1 of the present invention, and the magnification in the figure is 10000 times;

[0020] Figure 3 This is a scanning electron microscope photo of the iron oxide quantum dots / titanium dioxide heterogeneous nanosheets in Example 3 of the present invention, and the magnification in the figure is 150,000 times;

[0021] Figure 4 This is a transmission electron microscope photograph of the iron oxide quantum dots / titanium dioxide heterogeneous nanosheets in Example 2 of the present invention. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0024] A method for preparing a high surface activity material in one embodiment of the present invention comprises the following steps:

[0025] Ferric chloride and titanium dioxide P25 nanoparticles are dispersed in a sodium hydroxide solution, stirred in situ and subjected to hydrothermal treatment to obtain a composite precursor of ferric oxide and titanate;

[0026] Proton exchange of the ferric oxide and titanate composite precursor in a hydrochloric acid solution is performed to obtain iron-doped metatitanate nanosheets;

[0027] The iron-doped metatitanate nanosheets are subjected to heat treatment in air to obtain a high-surface activity material.

[0028] In one embodiment, the titanium source is titanium dioxide P25 nanoparticles.

[0029] In one embodiment, the titanium dioxide nanoparticles are in anatase phase, rutile phase, or a mixture of the two.

[0030] In one embodiment, the mass ratio of the titanium dioxide P25 nanoparticles to the ferric chloride is 1:1 to 1:10.

[0031] In one of the embodiments, the parameters of the in-situ stirring hydrothermal treatment are: the in-situ stirring rate is 100 r / min to 600 r / min; the temperature of the hydrothermal treatment is 100° C. to 200° C., and the time of the hydrothermal treatment is 10 h to 48 h.

[0032] In one embodiment, the heat treatment temperature is 300° C. to 1300° C., and the heat treatment time is 3 min to 150 min.

[0033] In one embodiment, the alkali solution is one or more of sodium hydroxide aqueous solution, ammonia water, and potassium hydroxide aqueous solution.

[0034] In one embodiment, the concentration of the alkali solution is 1 mol / L to 10 mol / L.

[0035] In one embodiment, the protonation treatment time is 1 to 10 hours, and the insulation treatment temperature is 25 to 100°C.

[0036] In one embodiment, the surface of the high surface activity material is a nano-heterogeneous structure with a specific surface area of ​​50 m 2 / g~200m 2 / g, and the particle size distribution is 2nm~50nm.

[0037] In the above scheme, after in-situ stirring hydrothermal and heat treatment, a high surface activity nano heterostructure can be prepared in situ during the hydrothermal process, the overall preparation process is simple, and the product is stable and easy to disperse; the material prepared by the present invention has a high active surface heterostructure, which is beneficial to surface charge transfer and ion migration, and the prepared electrode has good specific capacity and rate performance, and the process controllability of the present application is strong. By changing the process conditions, titanium dioxide heterogeneous nanosheet substrates of different sizes and iron oxide quantum dots loaded with different sizes can be obtained.

[0038] The embodiments of the present invention will be described in detail below with reference to specific examples.

[0039] Embodiment 1:

[0040] A method for preparing a high-surface-activity material comprises the following steps:

[0041] 1.0 g of titanium dioxide P25 nanoparticles and 1.0 g of ferric chloride in a mass ratio of 1:1 were mixed, dispersed in a 3 mol / L sodium hydroxide solution by mechanical stirring, and then subjected to in-situ stirring hydrothermal treatment to prepare a composite precursor of ferric oxide and titanate. The parameters of the in-situ stirring hydrothermal treatment were: stirring rate of 300 r / min; hydrothermal treatment temperature of 120°C; and hydrothermal treatment time of 36 h.

[0042] The obtained ferric oxide and titanate composite precursor was placed in a 0.3 mol / L hydrochloric acid solution and treated for 5 hours at a holding temperature of 50° C. to obtain iron-doped metatitanate nanosheets;

[0043] The iron-doped titanate nanosheets were heat treated in a muffle furnace at a heating rate of 10°C / min, a heat treatment temperature of 500°C, and a heat treatment time of 15min. After natural cooling, crystallized iron oxide quantum dots / titanium dioxide heterogeneous nanosheets were obtained.

[0044] The ferric oxide quantum dots / titanium dioxide heterogeneous nanosheets were ultrasonically cleaned in deionized water at room temperature for 3 times, each time for 5 minutes, and collected by vacuum filtration; then, the ferric oxide quantum dots / titanium dioxide heterogeneous nanosheets were dried at 60°C for 2 hours to obtain a dry high-surface activity material.

[0045] The dried high-surface active material prepared in Example 1 was applied to the negative electrode material of the sodium ion battery and assembled into a sodium ion half-cell. The electrochemical sodium storage performance was tested: at a current density of 100 mA / g for charging and discharging, the initial charging capacity was 120 mA h / g, and after 100 cycles, the capacity retention rate was 94%.

[0046] Embodiment 2:

[0047] A method for preparing a high-surface-activity material comprises the following steps:

[0048] 2.0 g of titanium dioxide P25 nanoparticles and 1.0 g of ferric chloride in a mass ratio of 2:1 were mixed, dispersed in a 1 mol / L sodium hydroxide solution by mechanical stirring, and then subjected to in-situ stirring hydrothermal treatment to prepare a composite precursor of ferric oxide and titanate. The parameters of the in-situ stirring hydrothermal treatment were as follows: stirring rate of 150 r / min; hydrothermal treatment temperature of 150 ° C; hydrothermal treatment time of 24 h;

[0049] The obtained ferric oxide and titanate composite precursor was placed in a 1.0 mol / L hydrochloric acid solution, and subjected to proton exchange treatment for 2 h at a holding temperature of 60° C. to obtain iron-doped metatitanate nanosheets;

[0050] The iron-doped titanate nanosheets were heat treated in a muffle furnace at a heating rate of 5°C / min, a heat treatment temperature of 300°C, and a heat treatment time of 50min. After natural cooling, crystallized iron oxide quantum dots / titanium dioxide heterogeneous nanosheets were obtained.

[0051] The ferric oxide quantum dots / titanium dioxide heterogeneous nanosheets were ultrasonically cleaned in deionized water at room temperature for 3 times, each time for 5 minutes, and collected by vacuum filtration; then, the ferric oxide quantum dots / titanium dioxide heterogeneous nanosheets were dried at 90° C. for 2 hours to obtain a dry high-surface activity material.

[0052] The dried high-surface activity material prepared in Example 2 was applied to the preparation of a negative electrode material for a sodium ion battery and assembled into a sodium ion half-cell. The electrochemical sodium storage performance was tested: at a current density of 100 mA / g for charging and discharging, the initial charging capacity was 150 mA h / g, and after 100 cycles, the capacity retention rate was 90%.

[0053] Embodiment 3:

[0054] A method for preparing a high-surface-activity material comprises the following steps:

[0055] 2.0 g of titanium dioxide P25 nanoparticles and 0.5 g of ferric chloride in a mass ratio of 4:1 were mixed, dispersed in a 5 mol / L sodium hydroxide solution by mechanical stirring, and then subjected to in-situ stirring hydrothermal treatment to prepare a composite precursor of ferric oxide and titanate. The parameters of the in-situ stirring hydrothermal treatment were as follows: stirring rate of 500 r / min; hydrothermal temperature of 170°C; hydrothermal time of 10 h;

[0056] The obtained ferric oxide and titanate composite precursor was placed in a 3.0 mol / L hydrochloric acid solution for 3 hours at a holding temperature of 80° C. to obtain iron-doped metatitanate nanosheets;

[0057] The iron-doped metatitanate nanosheets are placed in a muffle furnace for heat treatment, the heating rate of the heat treatment is 3°C / min, the heat treatment temperature is 1000°C, the heat treatment time is 100min, and after natural cooling, crystallized iron oxide quantum dots / titanium dioxide heterogeneous nanosheets are obtained;

[0058] The iron oxide quantum dots / titanium dioxide heterogeneous nanosheets were ultrasonically cleaned in deionized water for 3 times, each time for 5 minutes, and collected by vacuum filtration; then, the iron oxide quantum dots / titanium dioxide heterogeneous nanosheets were vacuum dried at 120°C for 2 hours to obtain a dry high-surface activity material.

[0059] The high surface activity material prepared in Example 3 was applied to the preparation of negative electrode materials for sodium ion batteries and assembled into sodium ion half-cells to test their electrochemical sodium storage performance: -1 Under charge and discharge, the first charge capacity is 90mA h / g, and after 100 cycles, the capacity retention rate is 85%.

[0060] Comparative Example 1:

[0061] The difference between Comparative Example 1 and Example 3 is that Comparative Example 1 does not undergo in-situ stirring of the hydrothermal reaction and proton exchange to obtain Comparative Sample 1; Comparative Sample 1 is applied to the negative electrode of a sodium ion battery, assembled into a sodium ion battery, and its electrochemical sodium storage performance is tested: at a current density of 100 mA / g for charging and discharging, the first charging capacity is 50 mA h / g, and after 100 cycles, the capacity retention rate is 80%. Comparative Example 1 is compared with Example 3, and it can be seen that Example 3 is conducive to the formation of a heterogeneous structure through in-situ stirring during the hydrothermal process, and reduces the grain size of titanium dioxide, thereby increasing the capacity of the sodium battery, which is the process technology advantage of the present application.

[0062] Comparative Example 2:

[0063] The difference between Comparative Example 2 and Example 3 is that Comparative Example 2 does not undergo proton exchange treatment, and directly uses ferric oxide and titanate composite precursors as the negative electrode of the sodium ion battery, assembles a sodium ion battery, and tests its electrochemical sodium storage performance: at a current density of 100mA / g charge and discharge, the first charge capacity is 150mA h / g, and after 100 cycles, the capacity retention rate is 50%. Compared with Example 3, it can be seen that in the example, the excess alkali ion components in the precursor are removed, the content of titanium dioxide in the product is increased, the cycle stability of the sodium battery is enhanced, and the irreversible capacity is reduced.

[0064] In addition, from Figure 1-Figure 4 Analysis shows that: Figure 1 This is a scanning electron microscope photo of the composite precursor of ferric oxide and titanate in Example 1 of the present invention, which is magnified 50,000 times. Figure 1 Analysis shows that the product is a nanosheet structure with a particle size of 50 to 200 nm; Figure 2 This is a scanning electron microscope photo of the iron oxide quantum dots / titanium dioxide heterogeneous nanosheets in Example 1 of the present invention, with a magnification of 10,000 times. Figure 2 Analysis shows that the heterogeneous nanosheets are in a crystalline state, and the particle size of the titanium silicon oxide microspheres is 50 to 200 nm; Figure 3 This is a scanning electron microscope photo of the iron oxide quantum dots / titanium dioxide heterogeneous nanosheets in Example 3 of the present invention. The magnification in the figure is 150,000 times. Figure 3The analysis shows that there are holes on the surface of the Fe2O3 quantum dots / TiO2 heterogeneous nanosheets prepared by the present invention; Figure 4 This is a transmission electron microscope photo of the iron oxide quantum dots / titanium dioxide heterogeneous nanosheets in Example 2 of the present invention. Figure 4 The magnification is 200,000 times. Among them, the size distribution of ferric oxide quantum dots is 2 to 10 nm, and the sodium battery capacity is higher than that in Example 1; the nanosheets in Example 3 collapse, the ferric oxide agglomerates, and the sodium battery capacity is lower than that in Examples 1 and 2. In general, the higher the calcination temperature, the less the proportion of anatase TiO2, and the higher the proportion of rutile phase TiO2, the ferric oxide quantum dots will gradually agglomerate, and the sodium battery capacity will decrease with increasing temperature. Therefore, the ratio of anatase phase to rutile phase and the size distribution of quantum dots can be controlled by controlling the temperature, thereby obtaining a nanomaterial with better capacity and stability.

[0065] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0066] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a high surface active material, characterized in that: The following steps are involved: Ferric chloride and titanium dioxide P25 nanoparticles are dispersed in a sodium hydroxide solution, stirred in situ and subjected to hydrothermal treatment, and the parameters of the in situ stirring and hydrothermal treatment are: an in situ stirring rate of 100 r / min to 600 r / min; a hydrothermal treatment temperature of 100°C to 200°C, and a hydrothermal treatment time of 10 h to 48 h, to obtain a composite precursor of ferric oxide and titanate; wherein the titanium dioxide P25 nanoparticles are a mixture of anatase phase and rutile phase; and the mass ratio of the titanium dioxide P25 nanoparticles to the ferric chloride is 1:1 to 1:10; The ferric oxide and titanate composite precursor are subjected to proton exchange in a hydrochloric acid solution for 1 to 10 hours, and the temperature of the heat preservation treatment is 25 to 100° C., to obtain iron-doped metatitanate nanosheets; The iron-doped metatitanate nanosheets are subjected to heat treatment in air to obtain a high surface activity material, wherein the heat treatment temperature is 300 to 1000° C. and the heat treatment time is 3 min to 150 min.

2. The preparation method according to claim 1, characterized in that: The concentration of the sodium hydroxide solution is 1 mol / L to 10 mol / L.

3. The preparation method according to claim 1, characterized in that: The surface of the high surface activity material is a nano-heterogeneous structure with a specific surface area of ​​50 m 2 / g ~ 200 m 2 / g, and the particle size distribution is 2nm~50nm.

Citation Information

Patent Citations

  • Transition metal doped titanium dioxide catalyst, preparation method and application thereof and device for producing hydrogen peroxide through electrochemical water oxidation

    CN115261925A