A self-repairing coating on magnesium alloy surface and its preparation method and application

By forming a micro-arc oxidation coating on the surface of magnesium alloy and loading a phosphate corrosion inhibitor, the uncontrollable corrosion problem of magnesium alloy in biomedical applications is solved, and efficient self-repair and biosafety are achieved. It is suitable for medical magnesium alloy planting Protection from entering the body.

CN115948784BActive Publication Date: 2024-11-15NANJING INST OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310050477.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-01
Publication Date
2024-11-15
Estimated Expiration
2043-02-01

AI Technical Summary

Technical Problem

Magnesium alloys are limited in biomedical applications due to their uncontrollable corrosion problems. The existing microarc oxidation coatings are highly brittle and difficult to provide effective protection in force-coupling environments. The self-repair performance is insufficient, resulting in local corrosion and inability. Controlled degradation.

Method used

The microarc oxidation coating is prepared by the surface of magnesium alloy. The layered bimetal hydroxide is formed by reacting acidic manganese-containing aqueous solution and hydrothermal reaction, and the phosphate corrosion inhibitor is loaded in its interlayer structure. Combined with the pH response mechanism, it forms the Repair the coating to enhance protection.

Benefits of technology

It realizes the efficient and long-term self-repairing ability of the magnesium alloy surface, suppresses corrosion and cracks caused by force coupling, improves biosafety and corrosion resistance, and is suitable for the protection of medical magnesium alloy implants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115948784B_ABST
    Figure CN115948784B_ABST
Patent Text Reader

Abstract

The invention discloses a magnesium alloy surface self-repairing coating and a preparation method and application thereof, belonging to the technical field of magnesium alloy corrosion protection, and the preparation method comprises the following steps: S1, preparing a micro-arc oxidation coating on the magnesium alloy surface: after pretreatment, the magnesium alloy is placed in a micro-arc oxidation electrolyte for micro-arc oxidation treatment to obtain a micro-arc oxidation coating; S2, growing a layered double metal hydroxide on the micro-arc oxidation coating: placing a micro-arc oxidation coating sample in an acidic manganese-containing aqueous solution for immersion, and then placing the sample after immersion in the acidic manganese-containing aqueous solution in a Mg(NO3)2, Ca(NO3)2 or Zn(NO3)2 aqueous solution for hydrothermal reaction; S3, corrosion-inhibiting ion loading: placing the sample in a (NH4)2HPO4 aqueous solution for immersion to obtain a magnesium alloy surface self-repairing coating. The coating of the invention has good corrosion protection capability and rapid self-repairing functional characteristics, and is suitable for engineering and biomedical fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a magnesium alloy surface self-repairing coating and a preparation method and application thereof, belonging to the technical field of magnesium alloy corrosion protection. Background Art

[0002] The uncontrollable corrosion problem of magnesium alloys is the main factor limiting their biomedical use. Surface coating is an effective way to improve the corrosion problem of magnesium alloys. Micro-arc oxidation coating can effectively improve the corrosion resistance of magnesium alloys. The coating composition can meet the requirements of biomedical applications through the design of electrolyte composition. However, the porous structure of micro-arc oxidation coating is easy to serve as a permeation channel for physiological solutions. This causes defects such as cracks and shedding to appear on the surface coating during service. When the surface coating is partially damaged, the physiological solution will penetrate into the coating-substrate interface through the coating defects, causing local corrosion behavior, accompanied by local magnesium ion enrichment, alkaline microenvironment and hydrogen precipitation. Slightly soluble Mg(OH)2 will be formed at the coating interface and will be converted into soluble MgCl2 in the physiological solution. As the reaction continues, the magnesium alloy will fall into a vicious corrosion cycle.

[0003] Magnesium alloy implants are also in a load-chemical coupling environment during service. Due to the high brittleness of the micro-arc oxidation coating, the corrosion fatigue performance of magnesium alloy samples treated with micro-arc oxidation coating is even lower than that of uncoated samples; and the micro-arc oxidation coating has limited or no improvement on the stress corrosion resistance of magnesium alloys. Therefore, it is urgent to explore stable and efficient protective coatings on the surface of medical magnesium alloys.

[0004] In order to achieve controllable protective performance, self-healing coatings on the surface of magnesium alloys have received extensive attention, and a variety of self-healing coatings for industrial applications have been developed. However, self-healing coatings on the surface of engineering magnesium alloys often contain biotoxic corrosion inhibitors, and the design of self-healing coatings on the surface of medical magnesium alloys puts forward requirements for human safety and biocompatibility for the selection of coating components and corrosion inhibitors. In addition, in the complex physiological environment of force-chemical coupling, self-healing coatings need to have efficient and long-lasting self-healing behavior. In summary, it is urgent to develop new medical self-healing coatings that integrate safety and functionality to promote the clinical application of medical magnesium alloys. Summary of the invention

[0005] The present invention aims to provide a medical magnesium alloy surface self-repairing coating that integrates safety and functionality. The self-repairing coating not only meets the requirements of human safety and biocompatibility, but also has efficient and long-term self-repairing capabilities.

[0006] At the same time, the present invention provides a method for preparing a self-repairing coating on the surface of a magnesium alloy, which has the self-repairing function of layered double metal hydroxide interlayer anion exchange and pH-responsive dual controlled release corrosion inhibitor, and the corrosion inhibitor has strong dissolution ability and strong self-repairing ability.

[0007] At the same time, the present invention provides a magnesium alloy surface self-repairing coating for application in surface treatment of medical magnesium alloy implants.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0009] A method for preparing a self-repairing coating on a magnesium alloy surface comprises the following steps:

[0010] S1. Preparing a micro-arc oxidation coating on the surface of a magnesium alloy: After the magnesium alloy is pretreated, the pretreated magnesium alloy is placed in a micro-arc oxidation electrolyte for micro-arc oxidation treatment to obtain a micro-arc oxidation coating;

[0011] S2. Growth of layered double metal hydroxides from micro-arc oxidation coatings: soaking the micro-arc oxidation coating samples in an acidic manganese-containing aqueous solution, and then placing the samples soaked in the acidic manganese-containing aqueous solution in a Mg(NO3)2, Ca(NO3)2 or Zn(NO3)2 aqueous solution for hydrothermal reaction;

[0012] S3. Corrosion-inhibiting ion loading: The sample obtained in S2 is immersed in an aqueous solution of (NH4)2HPO4 to obtain a self-repairing coating on the surface of the magnesium alloy.

[0013] In S1, the pretreatment method includes grinding and polishing, and pickling and / or alkali washing are selected as needed.

[0014] In S1, the micro-arc oxidation electrolyte is a silicate system aqueous solution, and its electrolyte composition includes 20-30 g / L Na2SiO3·9H2O and 1-2 g / L NaOH; the micro-arc oxidation treatment process is: constant current mode: forward current is 10-20 A / dm 2 , negative current is 0~5A / dm 2 , frequency 500~1000Hz, duty cycle: 15~30%, termination voltage 400~450V.

[0015] In S2, the acidic manganese-containing aqueous solution is a 0.05-0.1 mol / L MnCl2 solution, the pH of which is adjusted to 4-5, the soaking water bath temperature is 20-50°C, and the soaking time is 6-9h.

[0016] In S2, the aqueous solution of Mg(NO3)2, Ca(NO3)2 or Zn(NO3)2 is 0.02-0.10 mol / L, the hydrothermal reaction time is 12-24 h, and the hydrothermal reaction temperature is 95-120°C.

[0017] In S3, the concentration of the (NH4)2HPO4 aqueous solution is 0.05-0.10 mol / L, the temperature is 50-80°C, the soaking time is 12-24 h, and the pH is 7.5-8.5.

[0018] The micro-arc oxidation coating prepared by S1 has a dense layer and a loose layer, and the thickness of the dense layer is not less than 3μm; after being immersed in an acidic manganese-containing aqueous solution in S2, a manganese-rich compound is deposited on the loose layer of the micro-arc oxidation coating for sealing the micro-arc oxidation coating; after being hydrothermally treated with an Mg(NO3)2 aqueous solution, the manganese-rich compound is in situ converted into a magnesium-manganese layered double metal hydroxide; after being hydrothermally treated with a Ca(NO3)2 aqueous solution, the manganese-rich compound is in situ converted into a calcium-manganese layered double metal hydroxide; after being hydrothermally treated with a Zn(NO3)2 aqueous solution, the manganese-rich compound is in situ converted into a calcium-manganese layered double metal hydroxide. The manganese-rich compounds are in situ converted into zinc-manganese layered double metal hydroxides; after S3 is treated with (NH4)2HPO4 aqueous solution, phosphate is intercalated into the interlayer structure of the layered double metal hydroxides and forms hydrogen phosphate compounds on the surface; the surface of the magnesium-manganese layered double metal hydroxide is MgHPO4 compound; the surface of the calcium-manganese layered double metal hydroxide is CaHPO4 compound and MgHPO4 compound; the surface of the zinc-manganese layered double metal hydroxide is ZnHPO4 compound and MgHPO4 compound.

[0019] The magnesium alloy surface self-repairing coating obtained by the preparation method of the present invention comprises a micro-arc oxidation layer, the surface layer of the micro-arc oxidation layer is sealed by a manganese-rich compound, the sealed manganese-rich compound is in-situ grown into a layered double metal hydroxide layer, a phosphate corrosion inhibitor is loaded in the interlayer structure of the layered double metal hydroxide, and a hydrogen phosphate compound layer is in-situ formed on the surface of the layered double metal hydroxide.

[0020] Magnesium alloy surface self-repairing coating is used in surface treatment of medical magnesium alloy implants.

[0021] Application of magnesium alloy surface self-repairing coating on medical magnesium alloy implants.

[0022] A self-repairing coating on the surface of a magnesium alloy comprises a micro-arc oxidation layer, the surface layer of the micro-arc oxidation layer is sealed by a manganese-rich compound, the sealed manganese-rich compound is in-situ grown into a layered double metal hydroxide layer, a phosphate corrosion inhibitor is loaded in the interlayer structure of the layered double metal hydroxide, and a hydrogen phosphate compound layer is in-situ formed on the surface of the layered double metal hydroxide.

[0023] A medical magnesium alloy implant comprises a magnesium alloy surface self-repairing coating obtained by the preparation method of the invention.

[0024] The present invention provides a magnesium alloy surface self-repairing coating and a preparation method and application thereof, including the steps of preparing a micro-arc oxidation coating on the magnesium alloy surface, growing a layered double metal hydroxide from the micro-arc oxidation coating, and loading corrosion-inhibiting ions, thereby obtaining a self-repairing coating with excellent corrosion resistance, rapid self-repairing, and biosafety. The magnesium alloy surface self-repairing coating obtained by the present invention is suitable for the surface protection of medical magnesium alloys, and can effectively inhibit the local corrosion and uncontrollable degradation of magnesium alloy materials caused by cracks and local shedding of the coating caused by mechanical-chemical coupling.

[0025] The beneficial effects of the present invention are:

[0026] 1. The present invention relates to a self-repairing coating on the surface of a magnesium alloy, and a preparation method and application thereof. The silicate system micro-arc oxidation coating is composed of a dense layer and a porous layer, and has good corrosion protection function; the layered double metal hydroxide is distributed in the microporous structure and surface of the micro-arc oxidation coating, and plays a role in micro-arc oxidation sealing treatment; the micro-arc oxidation coating after sealing treatment can inhibit the release of magnesium ions during the hydrothermal reaction, and the composition of the layered double metal hydroxide is regulated by adding divalent metal ions in the hydrothermal treatment aqueous solution, so as to realize the preparation of layered double metal hydroxide containing magnesium / calcium / zinc on the surface of the magnesium alloy; (NH4)2HPO4 aqueous solution treatment not only introduces phosphate into the intercalation structure of the layered double metal hydroxide through anion exchange, but also can form a hydrogen phosphate compound coating on the surface of the layered double metal hydroxide.

[0027] 2. Phosphate is loaded in the layered double hydroxide in the form of interlayer anions and can be stably loaded in the coating; although a small amount of calcium hydroxide and magnesium hydroxide with poor corrosion resistance will be formed in the coating when the layered double hydroxide is prepared by hydrothermal reaction, the subsequent (NH4)2HPO4 aqueous solution can reduce the calcium hydroxide and magnesium hydroxide in the coating and convert them into calcium hydrogen phosphate / magnesium hydrogen phosphate / zinc hydrogen phosphate, and the bonding strength between the surface hydrogen phosphate compounds and the coating is good.

[0028] 3. The (NH4)2HPO4 aqueous solution is weakly alkaline at the initial stage of immersion. At this time, the phosphate corrosion inhibitor is mainly loaded between the layered double hydroxide layers. As the immersion time increases, the (NH4)2HPO4 solution becomes weakly alkaline due to the escape of NH3. The pH of the solution gradually decreases, and the hydroxyl groups on the surface of the layered double hydroxide adsorb phosphate and react with the hydroxide to form calcium hydrogen phosphate / magnesium hydrogen phosphate / zinc hydrogen phosphate ( M=Mg / Ca / Zn); the pH of the (NH4)2HPO4 aqueous solution gradually decreases, and the process is controllable, which helps to maintain the structural integrity of the layered double hydroxide and the synchronous loading of the hydrogen phosphate compound.

[0029] 4. The magnesium alloy surface self-repairing coating involved in the present invention is suitable for serving in a force-chemical coupling environment. Force-chemical coupling damage will cause coating damage, and micro-arc oxidation porous defects will act as crack sources. The present invention uses sealing treatment to reduce the stress corrosion cracking sensitivity of the micro-arc oxidation coating; when the phosphate-loaded layered double metal hydroxide at the microporous structure contacts the physiological solution, it can exchange anions with the anions in the environment, and trap the corrosive ions in the physiological solution in the interlayer structure of the layered double metal hydroxide, thereby hindering the further penetration of the corrosive ions; the phosphate loading form is firm and the loading amount is rich, and the surface hydrogen phosphate compound can quickly release a large amount of phosphate corrosion inhibitor, which is used to repair the local corrosion behavior caused by coating damage.

[0030] 5. The magnesium alloy surface self-repairing coating of the present invention has phosphate ions loaded in the coating in the form of hydrogen phosphate compounds and layered double hydroxide interlayer anions, and the phosphate corrosion inhibitor loading in the coating is large. The calcium hydrogen phosphate / magnesium hydrogen phosphate / zinc hydrogen phosphate on the composite coating has pH-responsive self-repairing functional characteristics (MHPO4+OH - →M 2+ +PO4 3- +H2O, M=Mg / Ca / Zn); the layered double hydroxide in the middle layer of the composite coating has an anion exchange effect. The pH effect and anion exchange, on the one hand, serve as an efficient self-repair response mechanism, and on the other hand, can consume the hydroxide and chloride ions in the local corrosion area, which can not only achieve efficient self-repair, but also inhibit the corrosive ions at the residual interface. The composite coating has efficient self-repair functional characteristics, and can quickly and actively repair coating defects caused by mechanical-chemical coupled physiological environments, overcoming the problem that a single micro-arc oxidation coating cannot improve the uncontrollable degradation of medical magnesium alloys under biomechanical conditions.

[0031] 6. The main cations in the layered double hydroxide are calcium / zinc / magnesium ions and manganese ions. The silicate system micro-arc oxidation coating has good chemical stability, which inhibits the dissolution of magnesium ions in the coating and the substrate during the hydrothermal reaction to a certain extent, and contributes to the successful preparation of calcium / zinc-containing layered double hydroxides. When the coating is damaged, the dissolved calcium / zinc ions will preferentially react with phosphate ions to form corrosion-resistant and biocompatible calcium-phosphorus deposition products, which contributes to efficient self-repair. In comparison, the thermodynamic driving force of the deposition reaction of magnesium ions and phosphate ions is weaker than that of calcium ions and phosphate ions.

[0032] 7. The present invention relates to a self-repairing coating on the surface of a magnesium alloy, which is composed of magnesium, manganese, phosphorus, oxygen, silicon, or zinc and calcium elements, all of which are nutrient elements required by the human body; the layered double metal hydroxide presents a nano-sheet structure, and the hydrogen phosphate compound presents a micron-sheet structure. The surface of the micro-nano-sized coating has good hydrophilic properties, which is conducive to cell adhesion, growth and proliferation.

[0033] The present invention discloses a magnesium alloy surface self-repairing coating and a preparation method and application thereof, and relates to magnesium alloy corrosion protection technology. The preparation method comprises the following steps: S1, preparing a micro-arc oxidation coating on the surface of the magnesium alloy; S2, growing a layered double metal hydroxide on the micro-arc oxidation coating; S3, loading corrosion-inhibiting ions. The present invention utilizes a layered double metal hydroxide for micro-arc oxidation coating pore sealing and corrosion-inhibiting ion loading, and loads a pH-sensitive hydrogen phosphate compound on the surface of the layered double metal hydroxide. The composite coating has good corrosion protection capability and rapid self-repairing functional characteristics, and can be adapted to engineering and biomedical fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The cross-sectional morphology and elemental analysis of the magnesium alloy surface self-repairing coating prepared in Example 1 of the present invention;

[0035] Figure 2 This is a surface morphology of the self-repairing coating on the magnesium alloy surface prepared in Example 1 of the present invention;

[0036] Figure 3 This is a surface morphology of the magnesium alloy surface self-repairing coating prepared in Example 1 of the present invention after being immersed in a 0.9wt.% NaCl solution for 7 days. DETAILED DESCRIPTION

[0037] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. The following embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0038] Example 1

[0039] A method for preparing a self-repairing coating on a magnesium alloy surface comprises the following steps:

[0040] S1. Preparing a micro-arc oxidation coating on the surface of a magnesium alloy: After the magnesium alloy is pre-treated by grinding, polishing, pickling and alkali washing in sequence, the pre-treated magnesium alloy is placed in a micro-arc oxidation electrolyte for micro-arc oxidation treatment to obtain a micro-arc oxidation coating;

[0041] The micro-arc oxidation electrolyte is a silicate system, and its electrolyte composition is 20g / L Na2SiO3·9H2O and 1g / LNaOH; constant current mode: forward current is 10A / dm 2 , negative current is 0A / dm 2 , frequency 500Hz, duty cycle: 15%, termination voltage 400V;

[0042] S2. Growth of layered double metal hydroxides from micro-arc oxidation coatings: The micro-arc oxidation coating samples were immersed in an acidic manganese-containing aqueous solution, the acidic manganese-containing aqueous solution was a 0.05 mol / L MnCl2 solution, the pH of which was adjusted to 4, the immersion water bath temperature was 20°C, and the immersion time was 6 hours; the samples immersed in the acidic manganese-containing aqueous solution were then placed in a Mg(NO3)2 aqueous solution for hydrothermal reaction, the Mg(NO3)2 solution was 0.02 mol / L, the hydrothermal reaction time was 12 hours, and the hydrothermal temperature was 95°C;

[0043] S3. Corrosion-inhibiting ion loading: The sample obtained in S2 was immersed in an (NH4)2HPO4 aqueous solution with a concentration of 0.05 mol / L, a temperature of 50°C, a time of 12 h, and a pH of 7.5 to obtain a self-repairing coating on the surface of the magnesium alloy.

[0044] The micro-arc oxidation coating prepared by S1 has a dense layer and a loose layer, and the thickness of the dense layer is not less than 3μm; after being immersed in an acidic manganese-containing aqueous solution in S2, manganese-rich compounds are deposited on the loose layer of the micro-arc oxidation coating for sealing the micro-arc oxidation coating; after being hydrothermally treated with an Mg(NO3)2 aqueous solution, the manganese-rich compounds are in situ converted into magnesium-manganese layered double metal hydroxides; after being treated with an (NH4)2HPO4 aqueous solution in S3, phosphates are intercalated into the interlayer structure of the layered double metal hydroxides, and hydrogen phosphate compounds are formed on the surface, and the surface of the magnesium-manganese layered double metal hydroxide is a MgHPO4 compound.

[0045] The magnesium alloy surface self-repairing coating obtained by the preparation method of this embodiment includes a micro-arc oxidation layer, the surface layer of the micro-arc oxidation layer is sealed with a manganese-rich compound, the sealed manganese-rich compound is in-situ grown into a magnesium-manganese layered double metal hydroxide layer, the interlayer structure of the magnesium-manganese layered double metal hydroxide is loaded with a phosphate corrosion inhibitor, and a MgHPO4 compound is in-situ formed on the surface of the magnesium-manganese layered double metal hydroxide.

[0046] Magnesium alloy surface self-repairing coating is used in surface treatment of medical magnesium alloy implants.

[0047] A medical magnesium alloy implant comprises a magnesium alloy surface self-repairing coating obtained by the preparation method of this embodiment.

[0048] Example 2

[0049] A method for preparing a self-repairing coating on a magnesium alloy surface comprises the following steps:

[0050] S1. Preparing a micro-arc oxidation coating on the surface of a magnesium alloy: After the magnesium alloy is pre-treated by grinding, polishing, pickling and alkali washing in sequence, the pre-treated magnesium alloy is placed in a micro-arc oxidation electrolyte for micro-arc oxidation treatment to obtain a micro-arc oxidation coating;

[0051] The micro-arc oxidation electrolyte is a silicate system, and its electrolyte composition is 30g / L Na2SiO3·9H2O and 2g / LNaOH; constant current mode: forward current is 20A / dm 2 , negative current is 5A / dm 2 , frequency 1000Hz, duty cycle: 30%, termination voltage 450V;

[0052] S2. Growth of layered double metal hydroxides from micro-arc oxidation coatings: The micro-arc oxidation coating samples were immersed in an acidic manganese-containing aqueous solution, the acidic manganese-containing aqueous solution was a 0.1 mol / L MnCl2 solution, the pH of which was adjusted to 5, the immersion water bath temperature was 50°C, and the immersion time was 9 hours; the samples immersed in the acidic manganese-containing aqueous solution were then placed in a Ca(NO3)2 aqueous solution for hydrothermal reaction, the Ca(NO3)2 solution was 0.10 mol / L, the hydrothermal reaction time was 24 hours, and the hydrothermal temperature was 120°C;

[0053] S3. Corrosion-inhibiting ion loading: The sample obtained in S2 was immersed in an (NH4)2HPO4 aqueous solution with a concentration of 0.10 mol / L, a temperature of 80°C, a time of 24 h, and a pH of 8.5 to obtain a self-repairing coating on the surface of the magnesium alloy.

[0054] The micro-arc oxidation coating prepared by S1 has a dense layer and a loose layer, and the thickness of the dense layer is not less than 3μm; after being immersed in an acidic manganese-containing aqueous solution in S2, manganese-rich compounds are deposited on the loose layer of the micro-arc oxidation coating for sealing the micro-arc oxidation coating; after being hydrothermally treated with a Ca(NO3)2 aqueous solution, the manganese-rich compounds are in situ converted into calcium-manganese layered double metal hydroxides; after being treated with a (NH4)2HPO4 aqueous solution in S3, phosphates are intercalated into the interlayer structure of the layered double metal hydroxides, and hydrogen phosphate compounds are formed on the surface; the surface of the calcium-manganese layered double metal hydroxide is CaHPO4 compound and MgHPO4 compound.

[0055] The magnesium alloy surface self-repairing coating obtained by the preparation method of this embodiment includes a micro-arc oxidation layer, the surface layer of the micro-arc oxidation layer is sealed with a manganese-rich compound, the sealed manganese-rich compound is in-situ grown into a calcium-manganese layered double metal hydroxide layer, the interlayer structure of the calcium-manganese layered double metal hydroxide is loaded with a phosphate corrosion inhibitor, and CaHPO4 compounds and MgHPO4 compounds are in-situ formed on the surface of the calcium-manganese layered double metal hydroxide.

[0056] Magnesium alloy surface self-repairing coating is used in surface treatment of medical magnesium alloy implants.

[0057] A medical magnesium alloy implant comprises a magnesium alloy surface self-repairing coating obtained by the preparation method of this embodiment.

[0058] Example 3

[0059] A method for preparing a self-repairing coating on a magnesium alloy surface comprises the following steps:

[0060] S1. Preparing a micro-arc oxidation coating on the surface of a magnesium alloy: After the magnesium alloy is pre-treated by grinding, polishing, pickling and alkali washing in sequence, the pre-treated magnesium alloy is placed in a micro-arc oxidation electrolyte for micro-arc oxidation treatment to obtain a micro-arc oxidation coating;

[0061] The micro-arc oxidation electrolyte is a silicate system, and its electrolyte composition is 25g / L Na2SiO3·9H2O and 1.2g / LNaOH; constant current mode: forward current is 12A / dm 2 , negative current is 1A / dm 2 , frequency 600Hz, duty cycle: 20%, termination voltage 425V;

[0062] S2. Growth of layered double metal hydroxides by micro-arc oxidation coating: The micro-arc oxidation coating sample was immersed in an acidic manganese-containing aqueous solution, the acidic manganese-containing aqueous solution was a 0.06 mol / L MnCl2 solution, the pH of which was adjusted to 4.5, the immersion water bath temperature was 30°C, and the immersion time was 8 hours; then the sample immersed in the acidic manganese-containing aqueous solution was placed in a Zn(NO3)2 aqueous solution for hydrothermal reaction, the Zn(NO3)2 solution was 0.06 mol / L, the hydrothermal reaction time was 18 hours, and the hydrothermal temperature was 100°C;

[0063] S3. Corrosion-inhibiting ion loading: The sample obtained in S2 was immersed in an (NH4)2HPO4 aqueous solution with a concentration of 0.08 mol / L, a temperature of 70°C, a time of 18 h, and a pH of 8.0 to obtain a self-repairing coating on the surface of the magnesium alloy.

[0064] The micro-arc oxidation coating prepared by S1 has a dense layer and a loose layer, and the thickness of the dense layer is not less than 3μm; after being immersed in an acidic manganese-containing aqueous solution in S2, manganese-rich compounds are deposited on the loose layer of the micro-arc oxidation coating for sealing the micro-arc oxidation coating; after hydrothermal treatment with a Zn(NO3)2 aqueous solution, the manganese-rich compounds are in situ converted into zinc-manganese layered double metal hydroxides; after being treated with a (NH4)2HPO4 aqueous solution in S3, phosphates are intercalated into the interlayer structure of the layered double metal hydroxides, and hydrogen phosphate compounds are formed on the surface, and the surface of the zinc-manganese layered double metal hydroxide is ZnHPO4 compounds and MgHPO4 compounds.

[0065] The magnesium alloy surface self-repairing coating obtained by the preparation method of this embodiment includes a micro-arc oxidation layer, the surface layer of the micro-arc oxidation layer is sealed with a manganese-rich compound, the sealed manganese-rich compound is in-situ grown into a zinc-manganese layered double metal hydroxide layer, the interlayer structure of the zinc-manganese layered double metal hydroxide is loaded with a phosphate corrosion inhibitor, and ZnHPO4 compounds and MgHPO4 compounds are in-situ formed on the surface of the zinc-manganese layered double metal hydroxide.

[0066] Magnesium alloy surface self-repairing coating is used in surface treatment of medical magnesium alloy implants.

[0067] A medical magnesium alloy implant comprises a magnesium alloy surface self-repairing coating obtained by the preparation method of this embodiment.

[0068] Comparative Example 1

[0069] The difference between this comparative example and Example 1 is that in this comparative example S2, Mg(NO3)2 aqueous solution is not selected for hydrothermal reaction, but deionized water is selected as the hydrothermal reaction solution medium.

[0070] Comparative Example 2

[0071] The difference between this comparative example and Example 1 is that in this comparative example S2, Mg(NO3)2 aqueous solution is not selected for hydrothermal reaction, but NaNO3 is selected as the hydrothermal reaction solution medium.

[0072] Comparative Example 3

[0073] The difference between this comparative example and Example 1 is that in this comparative example S3, (NH4)2HPO4 is replaced by Na2HPO4.

[0074] Comparative Example 4

[0075] The difference between this comparative example and Example 1 is that in this comparative example S3, the temperature is 100° C., the time is 36 h, and the pH is 7.0.

[0076] Characterization results

[0077] The coatings prepared by Examples 1 to 3 and Comparative Examples 1 to 4 were subjected to phase evaluation and self-healing ability analysis, and the results are shown in Table 1. The coatings prepared by Examples 1 to 3 of the present invention contain LDH (P) and hydrogen phosphate compounds, and have the self-healing functions of LDH (LDH is a layered double metal hydroxide) interlayer anion exchange and pH-responsive dual controlled release corrosion inhibitor. In Comparative Examples 1, 2 and 4, LDH (P) could not be obtained or LDH (P) was destroyed during the preparation process, and in Comparative Example 3, only LDH (P) was obtained, and pH-responsive hydrogen phosphate compounds could not be formed on the surface.

[0078] Figure 1The cross-sectional morphology and composition analysis of the coating prepared in Example 1 include Mg2SiO4, LDH(P) and MgHPO4. Figure 2 This is the surface morphology of the coating prepared in Example 1, and the upper layer of MgHPO4 is a micron-layer structure. Figure 3 This is the surface morphology of the coating prepared in Example 1 after being soaked in physiological saline. Since the physiological saline does not have corrosion-inhibiting ions, the pH of the physiological saline rises rapidly after soaking, the upper layer of MgHPO4 partially dissolves, and the exposed area is the middle layer of LDH (P) nanosheets.

[0079] LDH is a material with anion exchange function. In the present invention, the interlayer anion of LDH is phosphate. When it comes into contact with the external corrosive medium, it will exchange the chlorine or carbonate ions in the corrosive environment to the interlayer. At this time, the interlayer anion of LDH is converted from phosphate to Cl- / CO3 2- , which is manifested by the release of phosphate ions from the LDH interlayer and the exchange of anions in the service environment to the LDH interlayer, i.e. LDH(P)+Cl- / CO3 2- Converted to LDH(Cl- / CO3 2- )+P, P is phosphate; the hydrogen phosphate compounds on the surface have pH-responsive self-repairing function and can easily dissolve phosphate ions in an alkaline environment.

[0080] Table 1 shows the physical phase and self-repairing function (self-repairing ability (i.e., corrosion inhibitor dissolution ability): ***>**>*, LDH (P) refers to the layered double hydroxide of interlayer phosphate ions) of the magnesium alloy surface film layer obtained by the above-mentioned preparation process of the present invention.

[0081] Table 1 Performance of self-repairing coating on magnesium alloy surface

[0082]

[0083] It should be understood that in order to streamline the present disclosure and aid in understanding one or more of the various inventive aspects, in the above description of exemplary embodiments of the present invention, various features of the present invention are sometimes grouped together into a single embodiment, figure, or description thereof. However, this disclosed method should not be interpreted as reflecting the intention that the claimed invention requires more features than those expressly recited in each claim. Rather, as reflected in the claims, inventive aspects lie in less than all of the features of the previously disclosed embodiments. Therefore, the claims that follow the detailed description are hereby expressly incorporated into the detailed description, with each claim itself serving as a separate embodiment of the present invention.

[0084] Although the present invention has been described according to a limited number of embodiments, it will be apparent to those skilled in the art, with the benefit of the above description, that other embodiments may be envisioned within the scope of the invention thus described. In addition, it should be noted that the language used in this specification is selected primarily for readability and didactic purposes, rather than for explaining or defining the subject matter of the present invention. Therefore, many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the appended claims. The disclosure of the present invention is illustrative, not restrictive, with respect to the scope of the present invention, which is defined by the appended claims.

[0085] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a self-repairing coating on a magnesium alloy surface, characterized in that: The following steps are involved: S1. Preparing a micro-arc oxidation coating on the surface of a magnesium alloy: After the magnesium alloy is pretreated, the pretreated magnesium alloy is placed in a micro-arc oxidation electrolyte for micro-arc oxidation treatment to obtain a micro-arc oxidation coating; S2. Growth of layered double metal hydroxides from micro-arc oxidation coatings: soaking the micro-arc oxidation coating sample in an acidic manganese-containing aqueous solution, and then placing the sample soaked in the acidic manganese-containing aqueous solution in an aqueous solution for hydrothermal reaction, wherein the aqueous solution is any one of Mg(NO3)2, Ca(NO3)2, and Zn(NO3)2; S3. Corrosion-inhibiting ion loading: The sample obtained in S2 is immersed in an (NH4)2HPO4 aqueous solution to obtain a self-repairing coating on the surface of the magnesium alloy, wherein the concentration of the (NH4)2HPO4 aqueous solution is 0.05-0.10 mol / L, the temperature is 50-80°C, the immersion time is 12-24 h, and the pH is 7.5-8.

5.

2. The preparation method according to claim 1, characterized in that: In S1, the micro-arc oxidation electrolyte is a silicate system aqueous solution, and its electrolyte composition includes 20-30 g / L Na2SiO3·9H2O and 1-2 g / L NaOH; the micro-arc oxidation treatment process is: constant current mode: forward current is 10-20 A / dm 2 , negative current is 0~5A / dm 2 , frequency 500~1000Hz, duty cycle: 15~30%, termination voltage 400~450V.

3. The preparation method according to claim 1, characterized in that: In S2, the acidic manganese-containing aqueous solution is a 0.05-0.1 mol / L MnCl2 solution, the pH of which is adjusted to 4-5, the soaking water bath temperature is 20-50°C, and the soaking time is 6-9h.

4. The preparation method according to claim 1, characterized in that: In S2, the aqueous solution of Mg(NO3)2, Ca(NO3)2 or Zn(NO3)2 is 0.02-0.10 mol / L, the hydrothermal reaction time is 12-24 h, and the hydrothermal reaction temperature is 95-120°C.

5. The preparation method according to claim 1, characterized in that: The micro-arc oxidation coating prepared by S1 has a dense layer and a loose layer, and the thickness of the dense layer is not less than 3μm; after being immersed in an acidic manganese-containing aqueous solution in S2, a manganese-rich compound is deposited on the loose layer of the micro-arc oxidation coating, which is used for sealing the micro-arc oxidation coating; when the aqueous solution is Mg(NO3)2, after hydrothermal treatment with the Mg(NO3)2 aqueous solution, the manganese-rich compound is in situ converted into a magnesium-manganese layered double metal hydroxide; when the aqueous solution is Ca(NO3)2, after hydrothermal treatment with the Ca(NO3)2 aqueous solution, the manganese-rich compound is in situ converted into a calcium-manganese layered double metal hydroxide; when the aqueous solution is Zn When (NO3)2 is used, the manganese-rich compound is hydrothermally treated with an aqueous Zn(NO3)2 solution, and the manganese-rich compound is in situ converted into a zinc-manganese layered double hydroxide. After S3 is treated with an aqueous (NH4)2HPO4 solution, phosphate is intercalated into the interlayer structure of the layered double hydroxide, and a hydrogen phosphate compound is formed on the surface. The surface of the magnesium-manganese layered double hydroxide is a MgHPO4 compound; the surface of the calcium-manganese layered double hydroxide is a CaHPO4 compound and a MgHPO4 compound; the surface of the zinc-manganese layered double hydroxide is a ZnHPO4 compound and a MgHPO4 compound.

6. The magnesium alloy surface self-repairing coating obtained by the preparation method according to any one of claims 1 to 5, characterized in that: The invention comprises a micro-arc oxidation layer, the surface layer of the micro-arc oxidation layer is sealed by a manganese-rich compound, the sealed manganese-rich compound is in-situ grown into a layered double metal hydroxide layer, a phosphate corrosion inhibitor is loaded in the interlayer structure of the layered double metal hydroxide, and a hydrogen phosphate compound layer is in-situ formed on the surface of the layered double metal hydroxide.

7. The magnesium alloy surface self-repairing coating according to claim 6 is applied to the surface treatment of medical magnesium alloy implants.

8. A medical magnesium alloy implant, characterized in that: It comprises a magnesium alloy surface self-repairing coating obtained according to the preparation method according to any one of claims 1 to 5.