A catalytic cracking catalyst with rich mesoporous structure and preparation method thereof

By using medium-macroporous alumina and other components of the pseudo-thin hydrolasite structure in the catalytic cracking catalyst, a rich mesoporous structure with a pore size of 5 to 100 nm was prepared, which solved the problem of insufficient pore size of traditional catalysts and improved the catalyst's Heavy oil conversion capability and coke selectivity, and enhance wear resistance.

CN115957798BActive Publication Date: 2024-11-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202111174446.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-09
Publication Date
2024-11-15
Estimated Expiration
2041-10-09

AI Technical Summary

Technical Problem

The pore size of the traditional catalytic cracking catalyst is less than 4nm, which cannot meet the demand for heavy oil cracking. Moreover, the catalyst strength is limited after the addition of medium-macro pore materials, resulting in less obvious increase in the medium-macro pore structure, affecting catalytic performance.

Method used

The medium-macroporous alumina with a phthalid structure is used to combine the first and second binders, molecular sieves and clay, and the catalyst is prepared by stirring, beating, spray drying and calcining to ensure that the pore size is 5 to 100 nm. Enrich the mesoporous structure and improve the catalyst's wear resistance and heavy oil conversion ability.

Benefits of technology

The rich mesoporous structure of the catalyst is realized, the heavy oil conversion capacity and coke selectivity are improved, the wear resistance of the catalyst is enhanced, and the coke selectivity and catalytic activity are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115957798B_ABST
    Figure CN115957798B_ABST
Patent Text Reader

Abstract

A catalytic cracking catalyst with rich mesoporous structure and a preparation method thereof. The catalyst comprises, on a dry basis, 10 to 35 weight percent of medium and macroporous alumina in terms of alumina, 5 to 30 weight percent of a first binder in terms of oxide, 2 to 20 weight percent of a second binder in terms of oxide, 20 to 60 weight percent of a molecular sieve and 5 to 50 weight percent of clay; the medium and macroporous alumina is alumina with a pseudo-boehmite structure, with a total pore volume of 0.5 to 2.0 mL / g, wherein the pore volume of 5 to 100 nm pores accounts for more than 80% of the total pore volume, the average pore diameter is 5 to 30 nm, and the specific surface area is 250 to 450 m 2 / g; the mass ratio of the first binder to the macroporous alumina is 0.5 to 1.0. The catalytic cracking catalyst of the present invention has a rich mesoporous structure. The total pore volume is not less than 0.200 mL / g as measured by the low-temperature nitrogen adsorption method. The volume of macropores of 2 to 100 nm accounts for more than 70% of the total pore volume, and the volume of mesopores of 4 to 50 nm accounts for more than 60% of the total pore volume. Therefore, the catalyst has good wear resistance, enhanced heavy oil conversion capacity, and significantly improved coke selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of oil refining catalysts, and in particular relates to a catalytic cracking catalyst with rich mesopore structure and a preparation method thereof. Background Art

[0002] The promulgation and implementation of carbon emission regulations and low-carbon fuel standards have had a great impact on my country's oil refining industry. As the main unit of my country's oil refining processing, the catalytic cracking unit has become a major emitter of carbon dioxide in the oil refining industry due to the regeneration of its catalyst charring. Therefore, reducing the coke yield is the most effective means to reduce carbon emissions from catalytic cracking units. However, with the increasing trend of heaviness and inferiority of raw materials, the coke yield of catalytic cracking catalysts remains high. Catalysts with medium and macropore structures are conducive to the rapid diffusion of reactant molecules and product molecules, reducing the formation of coke precursors, and are also conducive to improving the stripping performance of the catalyst and reducing strippable coke. Therefore, it is imperative to develop catalytic cracking catalysts with rich medium and macropore structures.

[0003] The diameter of heavy oil molecules is about 3 to 10 nm. In order to eliminate diffusion limitations, the optimal range of pore size of catalytic cracking catalysts is 2 to 6 times the diameter of heavy oil molecules, corresponding to a pore size range of 6 to 60 nm. However, the pore size of traditional catalytic cracking catalysts is less than 4 nm, which cannot meet the requirements of heavy oil cracking.

[0004] CN1436835A discloses a catalytic cracking catalyst and its preparation method, wherein the catalyst contains 5-60 wt% of medium- and macro-porous alumina, 5-60 wt% of zeolite, 5-40 wt% of binder, and 5-85 wt% of clay, wherein the average pore diameter of the medium- and macro-porous alumina is not less than 3 nm, and the preparation method of the catalytic cracking catalyst is to mix the zeolite with the medium- and macro-porous alumina, binder, and clay uniformly, and then spray, roast, wash, and dry the mixture. However, the volume of pores with a diameter greater than 2 nm in the catalytic cracking catalyst is still less than 0.2 mL / g.

[0005] CN106179476A discloses a catalytic cracking catalyst and a preparation method and application thereof. The catalytic cracking catalyst contains 1-50% by weight of a mesoporous active material, wherein the mesoporous active material has a pseudo-boehmite crystal phase structure and an anhydrous chemical expression is: (0-0.2)Na2O·(40-85)Al2O3·(10-55)SiO2·(0.5-10)P2O5·(0.5-10)M x O y, wherein the metal M is selected from Mg, elements of Groups IIB, IIIB, IVB, VIIB of the periodic table, and one or more of lanthanide rare earth elements, y is the highest valence state of the metal M when it forms an oxide, and the values ​​of x and y balance the valence of M and O. It has lower coke selectivity and higher catalytic cracking activity in heavy oil catalytic cracking, and can obtain a higher diesel yield and a lower gasoline sulfur content, but the pore size of the prepared catalyst lacks a medium- and large-pore structure.

[0006] CN105688977A discloses a method for preparing a catalytic cracking catalyst containing pseudo-boehmite. The method comprises mixing and stirring part of the pseudo-boehmite with a silicon-containing solution for more than 15 minutes to prepare a modified pseudo-boehmite A, mixing and slurrying the modified pseudo-boehmite A, the remaining pseudo-boehmite B, and clay to prepare a matrix slurry containing pseudo-boehmite, mixing the matrix slurry and the molecular sieve slurry, homogenizing, forming and drying, and ion exchange to obtain a catalytic cracking catalyst. The catalyst prepared by the method has a high macropore volume, and the macropore diameter is mainly distributed above 100nm, lacking a 5-100nm medium-macropore structure.

[0007] However, due to the poor adhesion of mesoporous and macroporous materials, direct addition will affect the catalyst strength, which limits the amount of mesoporous and macroporous materials added, resulting in an insignificant increase in mesoporous and macroporous structures. Therefore, the preparation of catalytic cracking catalysts with rich mesoporous structures and good anti-wear properties is still a hot topic in research. Summary of the invention

[0008] In order to solve the above problems, the present invention provides a catalytic cracking catalyst with rich mesoporous structure and a preparation method thereof. The catalytic cracking catalyst has good anti-wear index, rich mesoporous structure, strong heavy oil conversion ability and good coke selectivity.

[0009] On the one hand, the present invention provides a catalytic cracking catalyst, which comprises, based on the dry weight of the catalyst, 10 to 35 weight percent of medium and macroporous alumina, 5 to 30 weight percent of a first binder, 2 to 20 weight percent of a second binder, 20 to 60 weight percent of a molecular sieve and 5 to 50 weight percent of clay, wherein the mass ratio of the first binder to the medium and macroporous alumina is 0.5 to 1.0; the medium and macroporous alumina is alumina with a pseudo-boehmite structure, and its total pore volume is 0.5 to 2.0 mL / g, wherein the pore volume of pores with a pore diameter of 5 to 100 nm accounts for more than 80% of the total pore volume, its average pore diameter is 5 to 30 nm, and its specific surface area is 250 to 450 m 2 / g.

[0010] In one embodiment, according to the catalytic cracking catalyst provided by the present invention, based on the dry weight of the catalyst, the catalytic cracking catalyst comprises: 10-30 wt% of medium- and macroporous alumina, 8-25 wt% of a first binder, 2-15 wt% of a second binder, 30-45 wt% of a molecular sieve and 10-40 wt% of clay, wherein the mass ratio of the first binder to the medium- and macroporous alumina is 0.5-0.8; the medium- and macroporous alumina is alumina with a pseudo-boehmite structure, and its total pore volume is 0.7-1.5 mL / g, wherein the pore volume of pores with a pore diameter of 5-100 nm accounts for 80%-95% of the total pore volume, its average pore diameter is 6-20 nm, and its specific surface area is 300-400 m 2 / g.

[0011] In one embodiment, the catalytic cracking catalyst provided by the present invention has a rich mesoporous structure. The total pore volume measured by low-temperature nitrogen adsorption method is not less than 0.200 mL / g, preferably 0.200-0.300 mL / g, wherein the pore volume of mesopores with a pore diameter of 2-100 nm accounts for more than 70% of the total pore volume, preferably 75%-95%, and the pore volume of mesopores with a pore diameter of 4-50 nm accounts for more than 60% of the total pore volume, preferably 65%-85%.

[0012] In one embodiment, according to the catalytic cracking catalyst provided by the present invention, the first binder is one or more selected from aluminum sol, silica sol, and silica-alumina sol, preferably aluminum sol and silica sol, and the second binder is one or more selected from acidified pseudo-boehmite, silica sol, aluminum sol, silica-alumina sol, aluminum phosphate sol, and zirconium sol, preferably aluminum sol, silica sol, and acidified pseudo-boehmite; and the mass ratio of the first binder to the second binder is 0.5 to 5.0.

[0013] In one embodiment, according to the catalytic cracking catalyst provided by the present invention, the molecular sieve is selected from NaY type molecular sieve, high silicon-aluminum ratio Y zeolite obtained by modifying NaY type molecular sieve, such as HY, REY, REHY, USY, REUSY, MFI type zeolite, one or more of β zeolite.

[0014] In one embodiment, according to the catalytic cracking catalyst provided by the present invention, the clay is various clays such as kaolin, bentonite, montmorillonite, sepiolite, diatomaceous earth, etc. that can be used as catalyst components.

[0015] On the other hand, the present invention also provides a method for preparing the catalytic cracking catalyst, which comprises the following steps: (1) mixing medium- and macro-pore alumina, clay and a first binder and stirring them uniformly to obtain a first slurry; (2) adding a molecular sieve to the first slurry, mixing and stirring them uniformly to obtain a second slurry; (3) adding a second binder to the second slurry, mixing and stirring them, spray drying and calcining the obtained mixed slurry, thereby obtaining the catalytic cracking catalyst provided by the present invention.

[0016] In one embodiment, according to the preparation method provided by the present invention, in the step (1), based on the dry weight of the catalyst, 10-35 wt% of the medium- and macro-porous structured alumina, 5-50 wt% of the clay, and 5-30 wt% of the first binder are mixed and slurried with deionized water for a slurrying time of not less than 15 min to obtain a first slurry, and the solid content of the obtained first slurry is 15-40 wt%; in the step (2), 20-60 wt% of the molecular sieve is added to the first slurry, mixed and slurried for a slurrying time of not less than 15 min to obtain a second slurry, and the solid content of the obtained second slurry is 15-40 wt%; in the step (3), 2-20 wt% of the second binder is added to the second slurry, and the solid content of the obtained mixed slurry is 15-40 wt%.

[0017] Compared with the prior art, the present invention has the following advantages: on the one hand, the prior art acidifies the medium- and macroporous alumina to improve the catalyst wear performance, but the acidification will cause the original medium- and macroporous structure to disappear, and the catalyst heavy oil conversion capacity and coke selectivity will be reduced; on the other hand, the prior art directly adds the medium- and macroporous alumina material to the catalyst without acidification to increase the macropore volume, but this will cause the catalyst wear performance to deteriorate. In contrast, the preparation method of the catalytic cracking catalyst according to the present invention not only retains the medium- and macroporous structure of the medium- and macroporous alumina, improves the heavy oil conversion capacity and coke selectivity, but also overcomes the adverse effect of the medium- and macroporous alumina on the catalyst strength.

[0018] Therefore, compared with conventional catalysts, the catalytic cracking catalyst provided by the present invention has a rich 4-50 nm mesoporous structure, good wear resistance, enhanced catalyst heavy oil conversion ability, and significantly improved coke selectivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is the pore distribution diagram of the medium and macroporous alumina used in the present invention.

[0020] Figure 2 This is the pore distribution diagram of the catalytic cracking catalyst prepared according to Example 1.

[0021] Figure 3 This is the pore distribution diagram of the catalytic cracking catalyst prepared according to Comparative Example 1. DETAILED DESCRIPTION

[0022] The present application is further described in detail below in conjunction with the accompanying drawings and embodiments. Through these descriptions, the features and advantages of the present application will become clearer and more explicit.

[0023] In addition, the technical features involved in different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.

[0024] The present invention provides a catalytic cracking catalyst, which contains, based on the dry weight of the catalyst, 10-35% by weight, preferably 10-30% by weight of medium- and macro-pore alumina, 5-30% by weight, preferably 8-25% by weight of a first binder, 2-20% by weight, preferably 2-15% by weight of a second binder, 20-60% by weight, preferably 30-45% by weight of a molecular sieve and 5-50% by weight, preferably 10-40% by weight of clay; the mass ratio of the first binder to the medium- and macro-pore alumina is 0.5-1.0, preferably 0.5-0.8. The medium- and macroporous alumina refers to alumina with a pseudo-boehmite structure, with a total pore volume of 0.5 to 2.0 mL / g, preferably 0.7 to 1.5 mL / g, wherein the pore volume of 5 to 100 nm pores accounts for more than 80% of the total pore volume, preferably 80% to 95%, the average pore diameter is 5 to 30 nm, preferably 6 to 20 nm, and the specific surface area is 250 to 450 m 2 / g, preferably 300-400m 2 / g.

[0025] The catalytic cracking catalyst provided by the present invention has a rich mesoporous structure. The total pore volume measured by a low-temperature nitrogen adsorption method is not less than 0.200 mL / g, preferably 0.200-0.300 mL / g, wherein the pore volume of mesopores with a size of 2-100 nm accounts for more than 70% of the total pore volume, preferably 75%-95%; the pore volume of mesopores with a size of 4-50 nm accounts for more than 60% of the total pore volume, preferably 65%-85%.

[0026] In the catalytic cracking catalyst according to the present invention, the alumina having a pseudo-boehmite structure can be prepared according to the methods provided in patents US4010116 and US4206085, the entire contents of which are incorporated herein by reference.

[0027] In the catalytic cracking catalyst according to the present invention, the first binder may be selected from one or more of aluminum sol, silica sol, and silica-alumina sol, preferably aluminum sol, and the second binder refers to one or more of acidified pseudo-boehmite, silica sol, aluminum sol, silica-alumina sol, aluminum phosphate sol, and zirconium sol, preferably acidified pseudo-boehmite.

[0028] In the catalytic cracking catalyst according to the present invention, the molecular sieve can be selected from NaY type molecular sieve, high silicon-aluminum ratio Y zeolite obtained by modifying NaY type molecular sieve, such as one or more of REY, HY, REHY, USY, REUSY, MFI type zeolite and Beta zeolite.

[0029] In the catalytic cracking catalyst according to the present invention, the clay refers to various clays that can be used as catalyst components, such as kaolin, bentonite, montmorillonite, sepiolite, diatomaceous earth, etc. These clays are well known to those skilled in the art.

[0030] The present invention also provides a method for preparing the catalytic cracking catalyst, which comprises the following steps:

[0031] (1) Mixing medium- and macro-porous alumina, clay and a first binder to obtain a first slurry; (2) Adding a molecular sieve to the first slurry, mixing and stirring to obtain a second slurry; (3) Adding a second binder to the second slurry, mixing and stirring, spray drying and calcining the obtained mixed slurry to obtain the catalytic cracking catalyst provided by the present invention.

[0032] In step (1) of the method for preparing a catalytic cracking catalyst according to the present invention, medium- and macro-porous alumina, clay, a first binder and deionized water are mixed and slurried for a period of not less than 15 minutes, preferably 20 to 60 minutes, and the solid content of the obtained first slurry is 15 to 40% by weight.

[0033] In step (2) of the method for preparing a catalytic cracking catalyst according to the present invention, a molecular sieve is added to the obtained first slurry, and the mixture is mixed and slurried for a period of not less than 15 minutes, preferably 20 to 60 minutes. The solid content of the obtained second slurry is 15 to 40% by weight.

[0034] In step (3) of the method for preparing a catalytic cracking catalyst according to the present invention, a second binder is added to the obtained second slurry, and the solid content of the obtained mixed slurry is 15 to 40% by weight.

[0035] In the method for preparing the catalytic cracking catalyst provided by the present invention, the spray drying and calcination are carried out according to the existing methods, and the present invention has no special requirements. The method also includes washing, drying and other processes after the catalyst is calcined, which can be carried out according to the existing methods, and the present invention has no special requirements.

[0036] Example

[0037] The following examples will further illustrate the present invention and are intended to help readers better understand the essence of the present invention and the beneficial effects brought about, but should not be construed as any limitation on the practicable scope of the present invention.

[0038] The raw materials used to prepare the catalyst cracking catalyst in the following examples are as follows: the solid content of kaolin is 76% by weight; the alumina content in the aluminum sol is 21.5% by weight; the SiO2 content in the silica sol is 27.0% by weight; the properties of conventional pseudo-boehmite and medium- and macro-pore pseudo-boehmite are shown in Table 1; the solid content of the acidified pseudo-boehmite is 12.0% by weight, and the acidification is carried out with hydrochloric acid, and the molar ratio of acid (HCl) to alumina is 0.20; the solid content of the rare earth ultra-stable Y zeolite REUSY used is 85.0% by weight, and the unit cell constant is In terms of weight percentage, the content of Na2O is 1.6% and the content of RE2O3 is 12.0%. The medium- and macroporous alumina A to D are provided by Sinopec Catalyst Co., Ltd., and their properties are shown in Table 1.

[0039] The analysis and evaluation methods are described as follows:

[0040] Specific surface area and pore volume analysis: The ASAP 2405NV1.01 automatic adsorption instrument from Micromeritics, USA, was used, and the low temperature static nitrogen adsorption capacity method was used. The sample was heated to 1.33×10 -2 Pa, vacuum degassing at 300 ° C for 4 h, using N2 as the adsorption medium, and measuring the adsorption-desorption isotherm of the sample at 77.4 K. The specific surface area of ​​the sample was calculated according to the BET formula, and the volume of N2 adsorbed by the sample at a relative pressure of p / p0 = 0.98 was measured, and converted into liquid nitrogen volume, i.e., the total pore volume. The micropore volume was calculated according to the t-plot method, and the difference between the two was the volume of mesopores of 2 to 100 nm, among which the pore volumes of mesopores of 4 to 50 nm and mesopores of 5 to 100 nm were obtained by peak fitting.

[0041] Catalyst strength: put a certain amount of catalyst into a fixed device and blow it for 5 hours under a constant airflow. Except for the first hour, the average wear percentage in the last four hours is called the catalyst wear index, and the unit is % per hour. The method and standard are: air lift method Q / SYLS0518-2002.

[0042] Evaluation of catalytic cracking catalyst: The catalytic cracking catalyst was pre-aged in a fixed bed aging device at 800°C and 100% steam for 12 hours, and then evaluated on an ACE device. The properties of the reaction raw oil are shown in Table 8. The reaction temperature is 500°C, and the catalyst-oil weight ratio is 8.04. Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield, and coke selectivity = coke yield / conversion rate.

[0043] Example 1

[0044] 142 g of kaolin and 114 g of medium-macroporous alumina A were added to 291 g of water, and after stirring for 15 minutes, 279 g of aluminum sol was added, and stirring was continued for 60 minutes to obtain a first slurry; molecular sieve slurry (wherein the slurry contains 155 g of REUSY molecular sieve, and the solid content of the molecular sieve slurry is 35% by weight) was added to the first slurry, and stirring was continued for 30 minutes to obtain a second slurry; 93 g of aluminum sol was added to the second slurry, and stirring was continued for 30 minutes, and the obtained total slurry was spray-dried to form, and then calcined at 500°C for 2 hours to obtain the catalytic cracking catalyst C1 of the present invention. The pore distribution of the obtained catalyst C1 is as follows: Figure 2 shown.

[0045] Example 2

[0046] 153 g of kaolin and 86 g of medium-macroporous alumina B were added to 440 g of water, and 186 g of aluminum sol was added after stirring for 30 minutes, and stirring was continued for 60 minutes to obtain a first slurry; molecular sieve slurry (wherein the slurry contained 169 g of REUSY molecular sieve and the solid content of the molecular sieve slurry was 38 wt%) was added to the first slurry, and stirring was continued for 40 minutes to obtain a second slurry; 333 g of acidified pseudo-boehmite was added to the second slurry, and stirring was continued for 60 minutes. The obtained total slurry was spray-dried to form, and then calcined at 500°C for 2 hours to obtain the catalytic cracking catalyst C2 of the present invention.

[0047] Example 3

[0048] Add 100 g of kaolin and 139 g of medium-macroporous alumina C to 578 g of water, stir for 20 minutes, then add 279 g of aluminum sol and 74 g of silica sol, continue stirring for 60 minutes to obtain a first slurry; add molecular sieve slurry (the slurry contains 141 g of REUSY molecular sieve and the solid content of the molecular sieve slurry is 38 wt%) to the first slurry, continue stirring for 60 minutes to obtain a second slurry; add 111 g of aluminum sol to the second slurry, continue stirring for 30 minutes, spray dry the obtained total slurry to form, and then calcine at 500°C for 2 hours to obtain the catalytic cracking catalyst C3 of the present invention.

[0049] Example 4

[0050] 153 g of kaolin, 56 g of medium-macroporous alumina D and 149 g of aluminum sol were added to 179 g of water, the mixture was stirred for 90 minutes to obtain a first slurry; molecular sieve slurry (the slurry contained 179 g of REUSY molecular sieve and the solid content of the molecular sieve slurry was 35 wt%) was added to the first slurry, and stirring was continued for 60 minutes to obtain a second slurry; 500 g of acidified pseudo-boehmite was added to the second slurry, and stirring was continued for 60 minutes, the obtained total slurry was spray-dried to form, and then calcined at 550°C for 1.5 hours to obtain the catalytic cracking catalyst C4 of the present invention.

[0051] Example 5

[0052] Add 63 grams of kaolin and 169 grams of medium-macroporous alumina D to 474 grams of water, stir for 45 minutes, then add 372 grams of aluminum sol, continue stirring for 60 minutes to obtain a first slurry; add molecular sieve slurry (the slurry contains 155 grams of REUSY molecular sieve, and the solid content of the molecular sieve slurry is 35 weight%) to the first slurry, continue stirring for 60 minutes to obtain a second slurry; add 74 grams of silica sol to the second slurry, continue stirring for 30 minutes, spray dry the obtained total slurry to form, and then calcine at 500°C for 2 hours to obtain the catalytic cracking catalyst C5 of the present invention.

[0053] Table 1 Properties of macroporous alumina

[0054]

[0055] Comparative Example 1

[0056] In this comparative example, the medium- and macroporous alumina was first acidified by a conventional acidification method, and then the catalytic cracking catalyst was prepared.

[0057] 114 g of medium-macroporous aluminum oxide A was added to 286 g of water, and after stirring for 15 minutes, 16 g of 36% hydrochloric acid was added for acidification (according to the acid-aluminum mass ratio of 0.20), and stirred for 60 minutes to obtain the first slurry; 142 g of kaolin was added to 138 g of water, stirred for 60 minutes, and then molecular sieve slurry (wherein the slurry contained 155 g of REUSY molecular sieve, and the solid content of the molecular sieve slurry was 35% by weight) was added, and stirring was continued for 30 minutes to obtain the second slurry; after the first slurry and the second slurry were mixed and stirred for 30 minutes, 372 g of aluminum sol was added, and mixed evenly for 60 minutes, the obtained slurry was spray-dried and formed, and then calcined at 500°C for 2 hours to obtain the comparative catalyst DC1. The pore distribution of the obtained catalyst DC1 is as follows: Figure 3 shown.

[0058] Comparative Example 2

[0059] In this comparative example, the medium- and macro-porous alumina is not mixed with the first binder in advance, but is directly used to prepare the catalytic cracking catalyst.

[0060] 114 g of medium-macroporous alumina A and 142 g of kaolin were added to 811 g of water and stirred for 60 minutes to obtain a first slurry; then, molecular sieve slurry (the slurry contained 155 g of REUSY molecular sieve and the solid content of the molecular sieve slurry was 35 wt%) was added and stirred for 30 minutes to obtain a second slurry; 372 g of aluminum sol was added and mixed evenly for 30 minutes. The obtained total slurry was spray dried to form, and then calcined at 500°C for 2 hours to obtain a comparative catalyst DC2.

[0061] Comparative Example 3

[0062] The catalytic cracking catalyst was prepared according to the method of Example 1 of CN1436835A.

[0063] 615 g of medium-macroporous alumina A, 1555 g of REUSY molecular sieve, 1628 g of aluminum sol, 2093 g of kaolin and 9000 g of deionized water were fully mixed and stirred for 2 hours. After homogenization, the mixture was spray-dried and formed. The obtained microspheres were calcined at 450°C for 0.5 hour to obtain a comparative catalyst DC3.

[0064] Table 2 Catalyst composition and physical properties

[0065]

[0066] Catalysts C1-C5 prepared in Examples 1-5 and catalysts DC1-DC3 prepared in Comparative Examples 1-3 were pre-aged in a fixed bed aging device at 800°C and 100% steam for 12 hours, and then evaluated on an ACE device. The properties of the reaction raw oil are shown in Table 3. The reaction temperature is 500°C, and the catalyst-oil weight ratio is 8.02. Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield; total liquid yield = liquefied gas yield + gasoline yield + diesel yield; coke selectivity = coke yield / conversion rate. The evaluation results are shown in Table 4.

[0067] Table 3 Raw oil properties

[0068]

[0069] Table 4 Evaluation results

[0070]

[0071] As shown in Table 2 and the accompanying drawings, compared with Comparative Examples 1 to 3, the total pore volume and the proportion of large and medium pores in Examples 1 to 5 are significantly increased, while still maintaining good wear resistance. The results in Table 4 show that, accordingly, compared with the catalysts DC1 to DC3 prepared in Comparative Examples 1 to 3, the catalysts C1 to C5 prepared in the examples of the present invention have lower heavy oil yields, increased total liquid yields, reduced coke yields, and significantly improved coke selectivity. It can be seen that the catalytic cracking catalyst prepared by the present invention has a rich large and medium pore structure, which brings excellent heavy oil cracking ability and good coke selectivity, and at the same time has good catalyst strength.

[0072] The present application has been described above in conjunction with preferred embodiments, but these embodiments are only exemplary and serve only as an illustration. On this basis, various replacements and improvements may be made to the present application, all of which fall within the scope of protection of the present application.

Claims

1. A catalytic cracking catalyst, based on the dry weight of the catalyst, comprising: 10-35 wt% of medium- and macroporous alumina, 5-30 wt% of a first binder, 2-20 wt% of a second binder, 20-60 wt% of a molecular sieve and 5-50 wt% of clay, wherein the mass ratio of the first binder to the medium- and macroporous alumina is 0.5-1.0; the medium- and macroporous alumina is alumina having a pseudo-boehmite structure, wherein the total pore volume is 0.5-2.0 mL / g, wherein the pore volume of pores of 5-100 nm accounts for more than 80% of the total pore volume, the average pore diameter is 5-30 nm, and the specific surface area is 250-450 m 2 / g; The total pore volume of the catalytic cracking catalyst is not less than 0.200 mL / g as measured by a low-temperature nitrogen adsorption method, wherein the pore volume of mesopores with a pore diameter of 2 to 100 nm accounts for more than 70% of the total pore volume, and the pore volume of mesopores with a pore diameter of 4 to 50 nm accounts for more than 60% of the total pore volume.

2. The catalytic cracking catalyst according to claim 1, characterized in that The catalytic cracking catalyst comprises, based on the dry weight of the catalyst, 10-30 wt% of medium- and macroporous alumina, 8-25 wt% of a first binder, 2-15 wt% of a second binder, 30-45 wt% of a molecular sieve and 10-40 wt% of clay, wherein the mass ratio of the first binder to the medium- and macroporous alumina is 0.5-0.8; the medium- and macroporous alumina is alumina with a pseudo-boehmite structure, wherein the total pore volume is 0.7-1.5 mL / g, wherein the pore volume of 5-100 nm pores accounts for 80%-95% of the total pore volume, the average pore diameter is 6-20 nm, and the specific surface area is 300-400 m 2 / g.

3. The catalytic cracking catalyst according to claim 1, characterized in that The total pore volume of the catalytic cracking catalyst is measured by low temperature nitrogen adsorption method and is 0.200-0.300 mL / g.

4. The catalytic cracking catalyst according to claim 1, characterized in that The pore volume of medium and large pores with a pore diameter of 2 to 100 nm accounts for 75% to 95% of the total pore volume.

5. The catalytic cracking catalyst according to claim 1, characterized in that The pore volume of 4-50 nm mesopores accounts for 65%-85% of the total pore volume.

6. The catalytic cracking catalyst according to claim 1, characterized in that The first binder is one or more selected from aluminum sol, silica sol, and silica-alumina sol, and the second binder is one or more selected from acidified pseudo-boehmite, silica sol, aluminum sol, silica-alumina sol, aluminum phosphate sol, and zirconium sol, and the mass ratio of the first binder to the second binder is 0.5~5.

0.

7. The catalytic cracking catalyst according to claim 6, characterized in that The first binder is aluminum sol, and the second binder is acidified pseudo-boehmite.

8. The catalytic cracking catalyst according to claim 1, characterized in that The clay is one or more selected from kaolin, bentonite, montmorillonite, sepiolite and diatomaceous earth.

9. The catalytic cracking catalyst according to claim 1, characterized in that The molecular sieve is one or more selected from NaY molecular sieve, high silicon-aluminum ratio Y zeolite obtained by modifying NaY molecular sieve, MFI type zeolite, and beta zeolite.

10. The catalytic cracking catalyst according to claim 9, characterized in that The high silicon-aluminum ratio Y zeolite obtained after the modification of the NaY molecular sieve is HY, REY, REHY, USY or REUSY.

11. A method for preparing a catalytic cracking catalyst according to any one of the preceding claims, comprising the following steps: (1) Mixing medium- and macro-porous alumina, clay, a first binder and deionized water to obtain a first slurry; (2) Adding molecular sieve to the first slurry, mixing and stirring to obtain a second slurry; (3) Adding a second binder to the second slurry, mixing and stirring, spray drying and calcining the obtained mixed slurry to obtain the catalytic cracking catalyst according to any of the preceding claims.

12. The preparation method according to claim 11, characterized in that: Based on the dry weight of the catalyst, in the step (1), 10-35 wt % of the medium- and macro-pore structured alumina, 5-50 wt % of the clay, and 5-30 wt % of the first binder are mixed with deionized water and beaten for a beating time of not less than 15 min to obtain a first slurry, and the solid content of the obtained first slurry is 15-40 wt %; in the step (2), 20-60 wt % of the molecular sieve is added to the first slurry, mixed and beaten for a beating time of not less than 15 min to obtain a second slurry, and the solid content of the obtained second slurry is 15-40 wt %; in the step (3), 2-20 wt % of the second binder is added to the second slurry, and the solid content of the obtained mixed slurry is 15-40 wt %.

13. The preparation method according to claim 11 or 12, characterized in that: The medium- and macro-pore structured alumina is alumina with a pseudo-boehmite structure, the first binder is one or more selected from aluminum sol, silica sol, and silica-alumina gel, the second binder is one or more selected from acidified pseudo-boehmite, silica sol, aluminum sol, silica-alumina gel, aluminum phosphate sol, and zirconium sol, the clay is one or more selected from kaolin, bentonite, montmorillonite, sepiolite, and diatomaceous earth, and the molecular sieve is one or more selected from NaY molecular sieve, high silicon-aluminum ratio Y zeolite obtained by modifying NaY molecular sieve, MFI type zeolite, and β zeolite.

Citation Information

Patent Citations

  • Method for preparing catalytic cracking catalyst containing pseudo-boehmite

    CN105688977A

  • Catalytic cracking catalyst as well as preparation method and application thereof

    CN106179476A

  • Catalytic cracking catalyst and its prepn

    CN1436835A

  • Fluid cracking catalysts