A colloidal gold-PS microsphere composite microsphere and preparation method thereof

Through the surface functional modification and covalent coupling assembly of colloidal gold-PS microsphere composite microspheres, a highly sensitive and stable solid phase carrier suitable for in vitro diagnosis is formed, which solves the problem of PS microspheres and colloidal gold in the existing technology. Problems such as difficult centrifugation, decolorization and low detection sensitivity in in vitro diagnostics.

CN115958193BActive Publication Date: 2024-10-25ZHENGZHOU LINGSI BIO-TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202211613856.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-15
Publication Date
2024-10-25
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

Existing colored PS microspheres have problems such as difficulty in centrifugation, easy decolorization, small particle size, and low detection sensitivity in in vitro diagnostics. In particular, the stability and detection sensitivity of colloidal gold as a nanocarrier are insufficient.

Method used

Colloidal gold-PS microsphere composite microspheres are used, and are assembled through surface functionalization modification and covalent coupling to form a covalent coupling of nano-microspheres and PS microspheres, combining the color development characteristics of colloidal gold and the chromogenic properties of PS microspheres. Bioconjugation ability, as a solid phase carrier for lateral chromatography.

Benefits of technology

It solves the problems of difficult centrifugation of PS microspheres, poor stability of colloidal gold and low detection sensitivity. It retains the color development properties of colloidal gold and improves the sensitivity and stability of detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115958193B_ABST
    Figure CN115958193B_ABST
Patent Text Reader

Abstract

The present invention discloses a colloidal gold-PS microsphere composite microsphere, comprising surface functionalized colloidal gold nano-microspheres and surface-energized PS microspheres, wherein the surface functional groups between the colloidal gold nano-microspheres and the PS microspheres are covalently coupled and assembled into composite microspheres, wherein the colloidal gold nano-microspheres are located on the surface of the PS microspheres. The present invention also discloses a method for preparing the colloidal gold-PS microsphere composite microsphere, comprising the following steps: protecting the surface of the colloidal gold nano-microspheres with a film; performing surface functionalization modification on the colloidal gold nano-microspheres with film protection; functionalization modification on the surface of the PS microspheres; and covalently coupling and assembling the surface functionalized colloidal gold nano-microspheres and PS microspheres into composite microspheres. The colloidal gold-PS microsphere composite microspheres provided by the present invention serve as the main solid phase carrier of lateral chromatography, which can not only solve the problem of difficult centrifugation of PS microspheres, but also retain the color development characteristics of colloidal gold and are not easy to cause decolorization, and can also solve the problems of poor stability and low sensitivity of colloidal gold.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to polystyrene microspheres (PS microspheres), and in particular to colloidal gold-PS microsphere composite microspheres and a preparation method thereof. Background Art

[0002] In the current in vitro diagnostic field, nanoparticles have been widely used as solid phase carriers to achieve the identification, capture, control and transportation of target molecules.

[0003] Colored PS microspheres are prepared by combining chromophores on a polystyrene matrix or surface. They have the characteristics of bright colors and narrow particle size distribution. They can also be surface modified to prepare PS microspheres with different functional groups, including PS carboxyl microspheres, PS amino microspheres and PS epoxy microspheres, to facilitate the coupling loading of biological living materials.

[0004] Colloidal gold, also known as gold sol, is a colloidal solution formed by the reduction of chloroauric acid into gold nanoparticles. Its color ranges from orange to purple. In 1971, Faulk and Taylor first used immunogold labeling technology to study the antigen components of Salmonella wall cells, combined colloidal gold with antibodies, and applied it to immunocytochemistry research at the electron microscope level. In 1974, Romano et al. used colloidal gold to label antiglobulin antibodies and established indirect immunogold staining. Since then, colloidal gold has developed rapidly as a new type of immunolabeling technology. As a new immunological method, immunocolloidal gold technology has the advantages of simplicity, rapidity, accuracy and non-pollution, and has been increasingly widely used in medicine, animal and plant quarantine, food safety supervision and other fields.

[0005] Although colored PS microspheres have been widely used, there are still some unavoidable problems, such as: low specific gravity makes centrifugation difficult and color bleaching is prone to occur.

[0006] In the IVD field, since colloidal gold is bound by physical adsorption, antigens / antibodies are easily detached from the surface of gold particles, resulting in unstable markers; colloidal gold is easily affected by environmental factors such as salt concentration and pH, which can cause aggregation; and colloidal gold products as nanocarriers also have disadvantages such as small particle size and low detection sensitivity. Summary of the invention

[0007] The purpose of the present invention is to provide a colloidal gold-PS microsphere composite microsphere, which is a solid phase carrier that can not only meet the requirements of lateral chromatography technology for qualitative and easy interpretation, but also improve the sensitivity of detection. The nano-microsphere material of the present invention meets the needs of market development and is suitable for promotion.

[0008] Specifically, the colloidal gold-PS microsphere composite microsphere includes surface functionalized colloidal gold nanospheres and surface energetic PS microspheres, and the surface functional groups between the colloidal gold nanospheres and the PS microspheres are covalently coupled to assemble into composite microspheres, wherein the colloidal gold nanospheres are located on the surface of the PS microspheres. The composite microspheres are covalently coupled nanospheres and PS microspheres, and their structure is that the colloidal gold sub-spheres are coupled to the PS mother spheres, that is, the colloidal gold nanospheres are coupled to the surface of the PS microspheres, and the color characteristics of the colloidal gold nanospheres are retained; at the same time, because the surfaces of the colloidal gold spheres and the PS microspheres have functional groups, there are modified groups distributed on the surface of the composite microspheres, which can be coupled with biological living materials, and can be used in the field of IVD as a solid phase carrier material for lateral chromatography.

[0009] The colloidal gold-PS microsphere composite microspheres may have a diameter of 150-250 nm.

[0010] The surface functional groups of colloidal gold nanoparticles and PS microspheres can be carboxyl, amino, aldehyde, epoxy, sulfonic acid, chloromethyl, hydroxyl, and the like.

[0011] Another object of the present invention is to provide a method for preparing colloidal gold-PS microsphere composite microspheres.

[0012] Specifically, the preparation method of colloidal gold-PS microsphere composite microspheres comprises the following steps:

[0013] (1) Protecting the surface of colloidal gold nanoparticles with a film;

[0014] (2) Surface functionalization modification of the film-protected colloidal gold nanoparticles;

[0015] (3) Functionalization modification of the surface of PS microspheres;

[0016] (4) Surface functionalized colloidal gold nanospheres and PS microspheres were covalently coupled and assembled into composite microspheres.

[0017] In step (1), the colloidal gold nanospheres are coated with an amphiphilic polymer compound to protect the colloidal gold and other nanomaterials. While protecting the colloidal gold and other nanomaterials, the colloidal gold is given a stable structure and the spherical shape and structure of the protective material are protected. Specifically, the surface coating of the colloidal gold nanospheres can be, but is not limited to, a surface silicon shell treatment.

[0018] As an embodiment, in step (1), a colloidal gold solution of ≥1OD is taken, and a high molecular polymer aqueous solution with a mass volume ratio of 1:1 is added, mixed, and allowed to stand for reaction to obtain solution A, wherein the higher the concentration of colloidal gold, the higher the efficiency of the high molecular polymer film. Solution A is added with ammonia water-organic solvent with a volume ratio of 1:19 and stirred or shaken to obtain solution B; a silicate compound solution is added to solution B, and the reaction is carried out for 24 hours to obtain solution C; solution C is centrifuged to remove the supernatant, the solid matter is washed, redissolved and dispersed to obtain colloidal gold nanoparticles with silica shells on the surface.

[0019] The high molecular polymer may be PVP, PVA, poloxamer, etc. In the silicate compound solution, the volume ratio of the silicate compound to the organic solvent is 1:9. The organic solvent is methanol, ethanol or isopropanol. The centrifugal force is 10000g, and the solid is repeatedly washed 4-5 times with the organic solvent.

[0020] In step (2), the functionalization modification of the colloidal gold surface may be, but is not limited to, amino modification, and may include carboxylation, amino modification, aldehyde modification, epoxy modification, sulfonation, chloromethylation, hydroxylation, and the like.

[0021] As an embodiment, in step (2), the colloidal gold nanoparticles after film attachment, i.e., the colloidal gold nanoparticles with a silicon shell on the surface, react with a silane coupling agent solution containing amino groups. The aminosilane coupling agent can be any one of 3-aminopropyltriethoxysilane, γ-aminopropylmethyldiethoxysilane, and N-aminoethyl-γ-aminopropyltriethoxysilane; the solvent of the silane coupling agent solution is a 1:19 mixture of ammonia water-ethanol, ammonia water-methanol or ammonia water-isopropanol. The solvent should be consistent with the polarity of the surface-modified aminosilane coupling agent.

[0022] In step (3), the surface functionalization modification of the PS microspheres may be, but is not limited to, carboxylation modification, and may include carboxylation, amination, aldehyde modification, epoxylation, sulfonation, chloromethylation, hydroxylation, and the like.

[0023] As an embodiment, step (3) includes:

[0024] 1) Preparation of PS seeds: Add redistilled styrene monomer to an aqueous solution containing an emulsifier SDS (sodium dodecyl sulfate), pass N2 to remove O2 in the system, heat to 75°C, add initiator KPS (potassium persulfate) and polymerize for 8 hours to obtain solution F;

[0025] 2) Surface functionalization of PS microspheres: After obtaining solution F, take out a portion of solution F, add it to an aqueous solution containing an emulsifier, sodium dodecyl sulfate (SDS), add a certain amount of redistilled styrene monomer, add initiator KPS after passing N2, slowly heat to 75°C, react for 3 hours, add redistilled acrylic acid or methacrylic acid monomer, react for 10 hours to obtain solution G, which is the carboxylated PS microspheres.

[0026] In step (4), the coupling assembly method can be, but is not limited to, chemical connection between colloidal gold and PS microspheres through carboxyl and amino groups, amino groups and amino groups, hydroxyl and amino groups, hydroxyl and carboxyl groups, amino groups and epoxy groups, etc.

[0027] As an embodiment, step (4) includes:

[0028] 1) Wash the PS carboxyl microspheres three times with a 25 mM sodium chloride solution and then redisperse them in 25 mM sodium chloride to obtain solution H.

[0029] 2) Dispersing the amino-modified colloidal gold nanospheres in 25 mM sodium chloride to obtain solution I.

[0030] 3) Solution H was mixed with solution I, and then the mixture was rotated on a mixer for 30 minutes. After the rotation reaction, a sodium chloride solution containing an EDC / NHS activator was added to the reaction system, and the mixture was continued to react on the mixer for 4 hours. After the reaction was completed, the mixture was centrifuged and washed repeatedly with ethanol for 3 times to finally obtain colloidal gold-PS microsphere composite microspheres.

[0031] Beneficial effects:

[0032] The colloidal gold-PS microsphere composite microsphere provided by the present invention is used as the main solid phase carrier of lateral chromatography, which can not only solve the problem of difficult centrifugation of PS microspheres, but also retain the color development characteristics of colloidal gold and is not easy to cause decolorization, and also solve the problems of poor stability and low sensitivity of colloidal gold. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a TEM photograph of the colloidal gold-PS microsphere composite microsphere of the present invention.

[0034] Figure 2 It is a schematic diagram of the preparation process of colloidal gold-PS microspheres according to Example 1 of the present invention.

[0035] Figure 3 It is a schematic diagram of the preparation process of colloidal gold-PS microspheres according to Example 2 of the present invention.

[0036] Figure 4 It is a schematic diagram of the preparation process of colloidal gold-PS microspheres according to Example 3 of the present invention.

[0037] Figure 5 Schematic diagram of the preparation process of colloidal gold-PS microspheres according to Example 4 of the present invention. DETAILED DESCRIPTION

[0038] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.

[0039] The specific implementation process involves a cleaning operation step, which includes centrifuging to discard the supernatant, then re-dissolving with a solvent, and re-centrifuging to remove the supernatant and then re-dissolving. This is a complete cleaning process.

[0040] (1) Surface coating protection of colloidal gold materials: Use amphiphilic polymers to coat colloidal gold. While protecting nanomaterials such as colloidal gold, it also gives colloidal gold a stable structure and protects the spherical shape and structure of the material.

[0041] In the specific implementation process, a high concentration colloidal gold solution (≥1OD) is taken and a high molecular polymer aqueous solution with a mass volume ratio of 1:1 is added. These high molecular materials can be PVP, PVA, poloxamer, etc. After the colloidal gold and the high molecular material are mixed, they are allowed to stand and react to obtain solution A. Among them, after repeated verification and confirmation, the higher the concentration of colloidal gold, the higher the efficiency of polymer film attachment.

[0042] After obtaining solution A, add ammonia water-ethanol, ammonia water-methanol or ammonia water-isopropanol solution with a volume ratio of 1:19, stir or shake to mix, and obtain solution B.

[0043] Add a silicate compound solution to solution B. The solvent here should be consistent with the solvent of solution B, and should be methanol, ethanol or isopropanol, etc.; further, the volume ratio of silicate to solvent is generally 1:9. React for 24 hours to obtain solution C.

[0044] Solution C is centrifuged to remove the supernatant at a centrifugal force of 10000 g, preferably washed repeatedly with a corresponding solvent for 4-5 times, then redissolved and dispersed to obtain colloidal gold nanoparticles with a silica shell on the surface.

[0045] (2) Surface modification of colloidal gold nanoparticles: The colloidal gold nanoparticles with silica shells on the surface are reacted with a silane coupling agent solution containing amino groups. The aminosilane coupling agent described herein can be any one of 3-aminopropyltriethoxysilane, γ-aminopropylmethyldiethoxysilane, and N-aminoethyl-γ-aminopropyltriethoxysilane; the solvent is a 1:19 mixture of ammonia water-ethanol, ammonia water-methanol, or ammonia water-isopropanol. Accordingly, the solvent should be consistent with the polarity of the surface-modified aminosilane coupling agent to obtain solution D.

[0046] Solution D is centrifuged at 10000 g, and after removing the supernatant, it is preferably re-dissolved in a corresponding solvent and washed 3-4 times under the same conditions. After the last re-dissolution, the suspension is dispersed by ultrasound to obtain a colloidal gold solution E with surface modified amino groups.

[0047] (3) Preparation of PS seeds: Add redistilled styrene monomer to an aqueous solution containing an emulsifier SDS (sodium dodecyl sulfate), pass N2 to remove O2 in the system, heat to 75°C, add initiator KPS (potassium persulfate) and polymerize for 8 hours to obtain solution F.

[0048] Functionalization modification of PS microsphere surface: take out a part of solution F, add it to the aqueous solution containing emulsifier sodium dodecyl sulfate (SDS), add a certain amount of redistilled styrene monomer, add initiator KPS after passing N2, slowly heat to 75°C, react for 3 hours, add redistilled acrylic acid or methacrylic acid monomer, react for 10 hours to obtain solution G, which is the carboxylated PS microspheres.

[0049] (4) Assembly of colloidal gold and PS microspheres: Solution G and solution D are mixed and reacted to obtain colloidal gold-PS microsphere composite microspheres.

[0050] Embodiment 1

[0051] (1) Take 500 μl of 200OD 40nm colloidal gold solution, add 10-100 μl (m / v) 50% PVP aqueous solution, mix well and let stand for reaction for 15 minutes; add 100 μl of ethanol solution containing 3-5% TEOS, mix well and add 5 μl ammonia water, shake and react for 24 hours; obtain the silicon-coated colloidal gold nanospheres, wash them 4 times by centrifugation with anhydrous ethanol (10000g, 10 min / time, ultrasonic dispersion); ultrasonically disperse them into 500 μl ethanol for later use.

[0052] (2) Add 30-60 μl of 1% 3-aminopropyltriethoxysilane ethanol solution dropwise to the silicon-coated colloidal gold nanospheres and stir at room temperature for 24 hours; discard the supernatant by centrifugation, wash with anhydrous ethanol by centrifugation 4 times (10,000 g, 10 min / time, ultrasonic dispersion), and finally dissolve with purified water to obtain amino-coated colloidal gold nanospheres.

[0053] (3) At room temperature, 100 ml of purified water, 100 mg of SDS, and 9 ml of redistilled styrene were added to a three-necked flask, mechanically stirred at 200 rpm, and nitrogen was passed through for 30 minutes. The temperature was raised to 75°C, 1 ml of a 30 mg / ml KPS aqueous solution was added, and the nitrogen atmosphere was maintained. The polymerization reaction was carried out for 8 hours to obtain PS seed microspheres.

[0054] Take 100ml purified water, 100mg SDS, 10ml PS seed microspheres, and 5ml styrene monomer and add them to a three-necked flask, stir mechanically at 200rpm, and pass nitrogen for 30 minutes; add 1ml 30mg / ml KPS aqueous solution, slowly heat to 75℃, and react for 3h. Take 500ul of acrylic acid (AA) and add it to the three-necked flask, and continue to react for 10h. After the reaction is completed, turn off the heating and cool it to room temperature, centrifuge the latex ball solution and remove the supernatant (10000g, 20min), wash it with anhydrous ethanol 2-3 times, and finally dissolve it with purified water to obtain carboxylated PS microspheres.

[0055] (4) Take 3 mg of PS carboxyl microspheres, wash them 2-3 times with 25 mM sodium chloride solution, and then redisperse them in 300 μl of 25 mM sodium chloride. Take 8 mg of amino-modified colloidal gold nanospheres and disperse them in 300 μl of 25 mM sodium chloride. Add the PS microspheres obtained in 1 dropwise to the colloidal gold solution obtained in 2, and then rotate the reaction on a mixer for 30 minutes. After the rotation reaction, add 10 mg of EDC / NHS to the reaction system, use 25 mM sodium chloride as solvent for EDC / NHS, and continue to react on the mixer for 4 hours. After the reaction is completed, centrifuge at 5000 g for 10 minutes, and wash repeatedly with ethanol 2-3 times to finally obtain colloidal gold-PS microsphere composite microspheres.

[0056] (5) Take 1 ml of 10 mg / ml colloidal gold-PS microsphere composite microspheres, add glutaraldehyde with a final concentration of 1%, activate for 1 hour, centrifuge at 1000g for 10 minutes, add a determined amount of the best HCG antibody protein to be labeled, shake well, and add 5% BSA to block nonspecific binding. Centrifuge at 5000 rpm at 4°C, aspirate the supernatant, and resuspend the precipitate in PBS buffer solution at pH 7.4 containing 1% BSA and 0.05% NaN3 to obtain a covalently bound composite microsphere antibody protein complex.

[0057] (6) The covalently bound composite microsphere-antibody-protein complex is evenly spread on glass fiber paper, dried overnight for 12 hours, and then cut into appropriate lengths to assemble into a reagent strip.

[0058] Embodiment 2

[0059] (1) Take 500 μl of 200OD 40nm colloidal gold solution, add 10-100 μl (m / v) 50% PVP aqueous solution, mix well and let stand for 15 minutes; add 100 μl of ethanol solution containing 3-5% TEOS, mix well and add 5 μl of ammonia water, shake and react for 24 hours; wash with anhydrous ethanol by centrifugation 4 times (10000g, 10 min / time, ultrasonic dispersion); ultrasonically disperse into 500 μl ethanol for later use.

[0060] (2) adding 30-60 μl of 1% γ-aminopropylmethyldiethoxysilane ethanol solution to the silicon-coated colloidal gold dropwise, stirring at room temperature for 24 hours; centrifuging and discarding the supernatant, washing with anhydrous ethanol by centrifugation for 4 times (10000 g, 10 min / time, ultrasonic dispersion), and finally re-dissolving with purified water to obtain amino-coated colloidal gold nanospheres;

[0061] (3) At room temperature, 100 ml of purified water, 100 mg of SDS, and 9 ml of redistilled styrene were added to a three-necked flask, mechanically stirred at 200 rpm, and nitrogen was passed through for 30 minutes. The temperature was raised to 75°C, 1 ml of a 30 mg / ml KPS aqueous solution was added, and the nitrogen atmosphere was maintained. The polymerization reaction was carried out for 8 hours to obtain PS seed microspheres.

[0062] Take 100ml purified water, 100mg SDS, 10ml PS seed microspheres, and 5ml styrene monomer and add them to a three-necked flask, stir mechanically at 200rpm, and pass nitrogen for 30 minutes. Add 1ml 30mg / ml KPS aqueous solution, slowly heat to 75℃, and react for 3h. Take 500ul of acrylic acid (AA) and add it to the three-necked flask, and continue to react for 10h. After the reaction is completed, turn off the heating and cool it to room temperature, centrifuge the latex ball solution and remove the supernatant (10000g, 20min), wash it with anhydrous ethanol 2-3 times, and finally dissolve it with purified water to obtain carboxylated PS microspheres.

[0063] (4) Take 3 mg of PS carboxyl microspheres, wash them 2-3 times with 25 mM sodium chloride solution, and then redisperse them in 300 μl of 25 mM sodium chloride. Take 8 mg of amino-modified colloidal gold nanospheres and disperse them in 300 μl of 25 mM sodium chloride. Add the PS microspheres obtained in 1 dropwise to the colloidal gold solution obtained in 2, and then rotate the reaction on a mixer for 30 minutes. After the rotation reaction, add 10 mg of EDC / NHS to the reaction system, use 25 mM sodium chloride as solvent for EDC / NHS, and continue to react on the mixer for 4 hours. After the reaction is completed, centrifuge at 5000 g for 10 minutes, and wash repeatedly with ethanol 2-3 times to finally obtain colloidal gold-PS microsphere composite microspheres.

[0064] (5) Take 1 ml of 10 mg / ml colloidal gold-PS microsphere composite microspheres, add glutaraldehyde to make the final concentration of the system 1%, activate for 1 hour, centrifuge at 1000g for 10 minutes, add a determined amount of the best HCG antibody protein to be labeled, shake well, and add 5% BSA to block nonspecific binding. Centrifuge at 5000 rpm at 4°C, aspirate the supernatant, and resuspend the precipitate in PBS buffer solution at pH 7.4 containing 1% BSA and 0.05% NaN3 to obtain a covalently bound composite microsphere antibody protein complex.

[0065] (6) The covalently bound composite microsphere-antibody-protein complex is evenly spread on glass fiber paper, dried overnight for 12 hours, and then cut into appropriate lengths to assemble into a reagent strip.

[0066] Embodiment 3

[0067] (1) Take 500 μl of 200OD 40nm colloidal gold solution, add 10-100 μl (m / v) 50% PVP aqueous solution, mix well and let stand for 15 minutes; add 100 μl of ethanol solution containing 3-5% TEOS, mix well and add 5 μl of ammonia water, shake and react for 24 hours; wash with anhydrous ethanol by centrifugation 4 times (10000g, 10 min / time, ultrasonic dispersion); ultrasonically disperse into 500 μl ethanol for later use.

[0068] (2) adding 30-60 μl of 1% 3-aminopropyltriethoxysilane ethanol solution dropwise to the silicon-coated colloidal gold, stirring at room temperature for 24 hours; centrifuging to discard the supernatant, washing with anhydrous ethanol by centrifugation for 4 times (10000 g, 10 min / time, ultrasonic dispersion), and finally re-dissolving with purified water to obtain amino-coated colloidal gold nanospheres;

[0069] (3) At room temperature, 100 ml of purified water, 100 mg of SDS, and 9 ml of redistilled styrene were added to a three-necked flask, mechanically stirred at 200 rpm, and nitrogen was passed through for 30 minutes. The temperature was raised to 75°C, 1 ml of a 30 mg / ml KPS aqueous solution was added, and the nitrogen atmosphere was maintained. The polymerization reaction was carried out for 8 hours to obtain PS seed microspheres.

[0070] Take 100ml purified water, 100mg SDS, 10ml PS seed microspheres, and 5ml styrene monomer and add them to a three-necked flask, stir mechanically at 200rpm, and pass nitrogen for 30 minutes. Add 1ml 30mg / ml KPS aqueous solution, slowly heat to 75℃, and react for 3h. Take 500ul methacrylic acid (MAA) and add it to the three-necked flask, and continue to react for 10h. After the reaction is completed, turn off the heating and cool it to room temperature, centrifuge the latex ball solution and remove the supernatant (10000g, 20min), wash it with anhydrous ethanol 2-3 times, and finally dissolve it with purified water to obtain carboxylated PS microspheres.

[0071] (4) Take 3 mg of PS carboxyl microspheres, wash them 2-3 times with 25 mM sodium chloride solution, and then redisperse them in 300 μl of 25 mM sodium chloride. Take 8 mg of amino-modified colloidal gold nanospheres and disperse them in 300 μl of 25 mM sodium chloride. Add the PS microspheres obtained in 1 dropwise to the colloidal gold solution obtained in 2, and then rotate the reaction on a mixer for 30 minutes. After the rotation reaction, add 10 mg of EDC / NHS to the reaction system, use 25 mM sodium chloride as solvent for EDC / NHS, and continue to react on the mixer for 4 hours. After the reaction is completed, centrifuge at 5000g for 10 minutes, and wash repeatedly with ethanol 2-3 times to finally obtain colloidal gold-PS microsphere composite microspheres.

[0072] (5) Take 1 ml of 10 mg / ml colloidal gold-PS microsphere composite microspheres, add glutaraldehyde to make the final concentration of the system 1%, activate for 1 hour, centrifuge at 1000g for 10 minutes, add a determined amount of the best HCG antibody protein to be labeled, shake well, and add 5% BSA to block nonspecific binding. Centrifuge at 5000 rpm at 4°C, aspirate the supernatant, and resuspend the precipitate in PBS buffer solution at pH 7.4 containing 1% BSA and 0.05% NaN3 to obtain a covalently bound composite microsphere antibody protein complex.

[0073] (6) The covalently bound composite microsphere-antibody-protein complex is evenly spread on glass fiber paper, dried overnight for 12 hours, and then cut into appropriate lengths to assemble into a reagent strip.

[0074] Embodiment 4

[0075] (1) Take 500 μl of 200OD 40nm colloidal gold solution, add 10-100 μl (m / v) 50% PVP aqueous solution, mix well and let stand for 15 minutes; add 100 μl of ethanol solution containing 3-5% TEOS, mix well and add 5 μl of ammonia water, shake and react for 24 hours; wash with anhydrous ethanol by centrifugation 4 times (10000g, 10 min / time, ultrasonic dispersion); ultrasonically disperse into 500 μl ethanol for later use.

[0076] (2) Add 30-60 μl of 1% γ-aminopropylmethyldiethoxysilane ethanol solution dropwise to the silicon-coated colloidal gold and stir at room temperature for 24 hours; discard the supernatant by centrifugation, wash with anhydrous ethanol by centrifugation 4 times (10000 g, 10 min / time, ultrasonic dispersion), and finally dissolve with purified water to obtain amino-coated colloidal gold nanospheres.

[0077] (3) At room temperature, 100 ml of purified water, 100 mg of SDS, and 9 ml of redistilled styrene were added to a three-necked flask, mechanically stirred at 200 rpm, and nitrogen was passed through for 30 minutes. The temperature was raised to 75°C, 1 ml of a 30 mg / ml KPS aqueous solution was added, and the nitrogen atmosphere was maintained. The polymerization reaction was carried out for 8 hours to obtain PS seed microspheres.

[0078] Take 100ml purified water, 100mg SDS, 10ml PS seed microspheres, and 5ml styrene monomer and add them to a three-necked flask, stir mechanically at 200rpm, and pass nitrogen for 30 minutes. Add 1ml 30mg / ml KPS aqueous solution, slowly heat to 75℃, and react for 3h. Take 500ul methacrylic acid (MAA) and add it to the three-necked flask, and continue to react for 10h. After the reaction is completed, turn off the heating and cool it to room temperature, centrifuge the latex ball solution and remove the supernatant (10000g, 20min), wash it with anhydrous ethanol 2-3 times, and finally dissolve it with purified water to obtain carboxylated PS microspheres.

[0079] (4) Take 3 mg of PS carboxyl microspheres, wash them 2-3 times with 25 mM sodium chloride solution, and then redisperse them in 300 μl of 25 mM sodium chloride. Take 8 mg of amino-modified colloidal gold nanospheres and disperse them in 300 μl of 25 mM sodium chloride. Add the PS microspheres obtained in 1 dropwise to the colloidal gold solution obtained in 2, and then rotate the reaction on a mixer for 30 minutes. After the rotation reaction, add 10 mg of EDC / NHS to the reaction system, use 25 mM sodium chloride as solvent for EDC / NHS, and continue to react on the mixer for 4 hours. After the reaction is completed, centrifuge at 5000 g for 10 minutes, and wash repeatedly with ethanol 2-3 times to finally obtain colloidal gold-PS microsphere composite microspheres.

[0080] (5) Take 1 ml of 10 mg / ml colloidal gold-PS microsphere composite microspheres, add glutaraldehyde to make the final concentration of the system 1%, activate for 1 hour, centrifuge at 1000g for 10 minutes, add a determined amount of the best HCG antibody protein to be labeled, shake well, and add 5% BSA to block nonspecific binding. Centrifuge at 5000 rpm at 4°C, aspirate the supernatant, and resuspend the precipitate in PBS buffer solution at pH 7.4 containing 1% BSA and 0.05% NaN3 to obtain a covalently bound composite microsphere antibody protein complex.

[0081] (6) The covalently bound composite microsphere-antibody-protein complex is evenly spread on glass fiber paper, dried overnight for 12 hours, and then cut into appropriate lengths to assemble into a reagent strip.

[0082] Assembly of colloidal gold test strips:

[0083] The sample pad, the glass fiber paper coated with the covalently bound composite microsphere antibody protein complex, the nitrocellulose NC membrane and the absorbent paper are overlapped and pasted in sequence to form a test strip, and the test strip is cut into test strips of appropriate width by a cutting machine, which can be used for rapid detection of clinical samples.

[0084] The three gold-labeled test strips with different labeling methods were tested with HCG reference products to compare the sensitivity and stability. The comparison data are as follows:

[0085] Comparison of sensitivity

[0086] Table 1:

[0087] 0mIU / mL 0.4mIU / mL 0.9mIU / mL 2.5mIU / mL 5mIU / mL 10mIU / mL 20mIU / mL Traditional colloidal gold labeling method - - - - ± + ++ Embodiment 1 - - - ± + ++ ++ Embodiment 2 - - ± + ++ ++ ++ Embodiment 3 - - - ± ++ ++ ++ Embodiment 4 - ± + ++ ++ ++ ++

[0088] Note: “-” negative; “+” positive, the more “+” means the darker the color, the stronger the positive; “±” weakly positive, vaguely visible to the naked eye.

[0089] In the above embodiments, various processes and methods not described in detail are conventional methods well known in the art.

[0090] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that for ordinary technical users in the field, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. Colloidal gold-PS microsphere composite microspheres, characterized in that: It comprises surface functionalized colloidal gold nano-microspheres and surface functionalized PS microspheres, wherein the surface functional groups of the colloidal gold nano-microspheres and the PS microspheres are covalently coupled to assemble into composite microspheres, wherein the colloidal gold nano-microspheres are located on the surface of the PS microspheres; The surface functionalized colloidal gold nanoparticles are amino-modified colloidal gold nanoparticles, whose surface functional groups are from γ-aminopropylmethyldiethoxysilane; the surface functionalized PS microparticles are carboxylated PS microparticles; It is prepared by: (1) Take 500 μl of 200OD 40nm colloidal gold solution, add 10-100 μl of 50% PVP aqueous solution by mass volume ratio, mix well and let stand for 15 minutes; add 100 μl of ethanol solution containing 3-5% TEOS, mix well and add 5 μl of ammonia water, shake and react for 24 hours; wash with anhydrous ethanol 10000g centrifugation 4 times, 10 min / time, and ultrasonically disperse into 500 μl ethanol for later use; (2) adding 30-60 μl of 1% γ-aminopropylmethyldiethoxysilane ethanol solution to the silicon-coated colloidal gold dropwise, stirring at room temperature for 24 hours; centrifuging and discarding the supernatant, washing with anhydrous ethanol at 10,000 g for 4 times, 10 min / time, ultrasonically dispersing, and finally re-dissolving with purified water to obtain amino-coated colloidal gold nanospheres; (3) At room temperature, 100 ml of purified water, 100 mg of SDS, and 9 ml of redistilled styrene were added to a three-necked flask, mechanically stirred at 200 rpm, and nitrogen was passed through for 30 minutes. The temperature was raised to 75°C, and 1 ml of a 30 mg / ml KPS aqueous solution was added. The nitrogen atmosphere was maintained and the polymerization reaction was carried out for 8 hours to obtain PS seed microspheres. 100 ml of purified water, 100 mg of SDS, 10 ml of the PS seed microspheres, and 5 ml of styrene monomer were added to a three-necked flask, mechanically stirred at 200 rpm, and nitrogen was passed through for 30 minutes. 1 ml of a 30 mg / ml KPS aqueous solution was added and the temperature was raised to 75° C. The reaction was continued for 3 hours. 500 ul of acrylic acid was added to the three-necked flask and the reaction was continued for 10 hours. After the reaction was completed, the heating was turned off and the solution was cooled to room temperature. The latex ball solution was centrifuged at 10,000 g for 20 minutes and the supernatant was removed. The solution was washed with anhydrous ethanol for 2-3 times and finally redissolved with purified water to obtain carboxylated PS microspheres. (4) 3 mg of the carboxylated PS microspheres were washed 2-3 times with a 25 mM sodium chloride solution and then redispersed in 300 μl of 25 mM sodium chloride. 8 mg of the amino-modified colloidal gold nanospheres were dispersed in 300 μl of 25 mM sodium chloride. The PS microspheres obtained in step (1) were added dropwise to the colloidal gold solution obtained in step (2), and then rotated on a mixer for 30 minutes. After the rotation reaction, 10 mg of EDC / NHS were added to the reaction system, and 25 mM sodium chloride was used as a solvent for EDC / NHS. The reaction was continued on the mixer for 4 hours. After the reaction was completed, the colloidal gold-PS microsphere composite microspheres were centrifuged at 5000 g for 10 minutes, and washed repeatedly with ethanol for 2-3 times to finally obtain colloidal gold-PS microsphere composite microspheres.

2. The method for preparing colloidal gold-PS microsphere composite microspheres according to claim 1, characterized in that: The following steps are involved: (1) Take 500 μl of 200OD 40nm colloidal gold solution, add 10-100 μl of 50% PVP aqueous solution by mass volume ratio, mix well and let stand for 15 minutes; add 100 μl of ethanol solution containing 3-5% TEOS, mix well and add 5 μl of ammonia water, shake and react for 24 hours; wash with anhydrous ethanol 10000g centrifugation 4 times, 10 min / time, and ultrasonically disperse into 500 μl ethanol for later use; (2) adding 30-60 μl of 1% γ-aminopropylmethyldiethoxysilane ethanol solution to the silicon-coated colloidal gold dropwise, stirring at room temperature for 24 hours; centrifuging and discarding the supernatant, washing with anhydrous ethanol at 10,000 g for 4 times, 10 min / time, ultrasonically dispersing, and finally re-dissolving with purified water to obtain amino-coated colloidal gold nanospheres; (3) At room temperature, 100 ml of purified water, 100 mg of SDS, and 9 ml of redistilled styrene were added to a three-necked flask, mechanically stirred at 200 rpm, and nitrogen was passed through for 30 minutes. The temperature was raised to 75°C, and 1 ml of a 30 mg / ml KPS aqueous solution was added. The nitrogen atmosphere was maintained and the polymerization reaction was carried out for 8 hours to obtain PS seed microspheres. 100 ml of purified water, 100 mg of SDS, 10 ml of the PS seed microspheres, and 5 ml of styrene monomer were added to a three-necked flask, mechanically stirred at 200 rpm, and nitrogen was passed for 30 minutes, 1 ml of 30 mg / ml KPS aqueous solution was added, the temperature was raised to 75° C., and the reaction was continued for 3 hours, 500 ul of acrylic acid was added to the three-necked flask, and the reaction was continued for 10 hours. After the reaction was completed, the heating was turned off and cooled to room temperature, the latex ball solution was centrifuged at 10000 g for 20 minutes, the supernatant was removed, and the solution was washed with anhydrous ethanol for 2-3 times, and finally re-dissolved with purified water to obtain carboxylated PS microspheres; (4) Take 3 mg of PS carboxyl microspheres, wash them with 25 mM sodium chloride solution for 2-3 times, and then redisperse them in 300 μl of 25 mM sodium chloride. Take 8 mg of amino-modified colloidal gold nanospheres, disperse them in 300 μl of 25 mM sodium chloride, add the PS microspheres obtained in step (1) dropwise to the colloidal gold solution obtained in step (2), and then rotate the mixture on a mixer for 30 minutes. After the rotation reaction, add 10 mg of EDC / NHS to the reaction system, using 25 mM sodium chloride as solvent for EDC / NHS, and continue to react on the mixer for 4 hours. After the reaction, centrifuge at 5000 g for 10 minutes, and wash repeatedly with ethanol for 2-3 times to finally obtain colloidal gold-PS microsphere composite microspheres.

3. Colloidal gold-PS microsphere composite microspheres, characterized in that: It comprises surface functionalized colloidal gold nano-microspheres and surface functionalized PS microspheres, wherein the surface functional groups of the colloidal gold nano-microspheres and the PS microspheres are covalently coupled to assemble into composite microspheres, wherein the colloidal gold nano-microspheres are located on the surface of the PS microspheres; The surface functionalized colloidal gold nanoparticles are amino-modified colloidal gold nanoparticles, whose surface functional groups are from γ-aminopropylmethyldiethoxysilane; the surface functionalized PS microparticles are carboxylated PS microparticles; It is prepared by: (1) Take 500 μl of 200OD 40nm colloidal gold solution, add 10-100 μl of 50% PVP aqueous solution by mass volume ratio, mix well and let stand for 15 minutes; add 100 μl of 3-5% TEOS ethanol solution, mix well and add 5 μl ammonia water, shake and react for 24 hours; wash with anhydrous ethanol 10000g centrifugation 4 times, 10 min / time; ultrasonically disperse into 500 μl ethanol for later use; (2) adding 30-60 μl of 1% γ-aminopropylmethyldiethoxysilane ethanol solution to the silicon-coated colloidal gold dropwise, stirring at room temperature for 24 hours; centrifuging and discarding the supernatant, washing with anhydrous ethanol at 10,000 g for 4 times, 10 min / time, ultrasonically dispersing, and finally re-dissolving with purified water to obtain amino-coated colloidal gold nanospheres; (3) At room temperature, 100 ml of purified water, 100 mg of SDS, and 9 ml of redistilled styrene were added to a three-necked flask, mechanically stirred at 200 rpm, and nitrogen was passed through for 30 minutes. The temperature was raised to 75°C, and 1 ml of a 30 mg / ml KPS aqueous solution was added. The nitrogen atmosphere was maintained and the polymerization reaction was carried out for 8 hours to obtain PS seed microspheres. 100 ml of purified water, 100 mg of SDS, 10 ml of the PS seed microspheres, and 5 ml of styrene monomer were added to a three-necked flask, mechanically stirred at 200 rpm, and nitrogen was passed for 30 minutes, 1 ml of 30 mg / ml KPS aqueous solution was added, the temperature was raised to 75° C., and the reaction was continued for 3 hours, 500 ul of methacrylic acid was added to the three-necked flask, and the reaction was continued for 10 hours. After the reaction was completed, the heating was turned off and cooled to room temperature, the latex ball solution was centrifuged at 10000 g for 20 minutes, the supernatant was removed, and the solution was washed with anhydrous ethanol for 2-3 times, and finally re-dissolved with purified water to obtain carboxylated PS microspheres; (4) Take 3 mg of PS carboxyl microspheres, wash them with 25 mM sodium chloride solution for 2-3 times, and then redisperse them in 300 μl of 25 mM sodium chloride. Take 8 mg of amino-modified colloidal gold nanospheres, disperse them in 300 μl of 25 mM sodium chloride, add the PS microspheres obtained in step (1) dropwise to the colloidal gold solution obtained in step (2), and then rotate the reaction on a mixer for 30 minutes. After the rotation reaction, add 10 mg of EDC / NHS to the reaction system, using 25 mM sodium chloride as solvent. Continue to react on the mixer for 4 hours. After the reaction, centrifuge at 5000 g for 10 minutes, and repeatedly wash with ethanol 2-3 times to finally obtain colloidal gold-PS microsphere composite microspheres.

4. The method for preparing colloidal gold-PS microsphere composite microspheres according to claim 3, characterized in that: The following steps are involved: (1) Take 500 μl of 200OD 40nm colloidal gold solution, add 10-100 μl of 50% PVP aqueous solution by mass volume ratio, mix well and let stand for 15 minutes; add 100 μl of 3-5% TEOS ethanol solution, mix well and add 5 μl ammonia water, shake and react for 24 hours; wash with anhydrous ethanol 10000g centrifugation 4 times, 10 min / time; ultrasonically disperse into 500 μl ethanol for later use; (2) adding 30-60 μl of 1% γ-aminopropylmethyldiethoxysilane ethanol solution to the silicon-coated colloidal gold dropwise, stirring at room temperature for 24 hours; centrifuging and discarding the supernatant, washing with anhydrous ethanol at 10,000 g for 4 times, 10 min / time, ultrasonically dispersing, and finally re-dissolving with purified water to obtain amino-coated colloidal gold nanospheres; (3) At room temperature, 100 ml of purified water, 100 mg of SDS, and 9 ml of redistilled styrene were added to a three-necked flask, mechanically stirred at 200 rpm, and nitrogen was passed through for 30 minutes. The temperature was raised to 75°C, and 1 ml of a 30 mg / ml KPS aqueous solution was added. The nitrogen atmosphere was maintained and the polymerization reaction was carried out for 8 hours to obtain PS seed microspheres. 100 ml of purified water, 100 mg of SDS, 10 ml of PS seed microspheres, and 5 ml of styrene monomer were added to a three-necked flask, mechanically stirred at 200 rpm, and nitrogen was passed through for 30 minutes. 1 ml of 30 mg / ml KPS aqueous solution was added, the temperature was raised to 75 ° C, and the reaction was continued for 3 hours. 500 ul of methacrylic acid was added to the three-necked flask, and the reaction was continued for 10 hours. After the reaction was completed, the heating was turned off and cooled to room temperature. The latex ball solution was centrifuged at 10000g for 20 minutes and the supernatant was removed. It was washed with anhydrous ethanol 2-3 times and finally re-dissolved with purified water to obtain carboxylated PS microspheres. (4) Take 3 mg of PS carboxyl microspheres, wash them with 25 mM sodium chloride solution for 2-3 times, and then redisperse them in 300 μl of 25 mM sodium chloride. Take 8 mg of amino-modified colloidal gold nanospheres, disperse them in 300 μl of 25 mM sodium chloride, add the PS microspheres obtained in step (1) dropwise to the colloidal gold solution obtained in step (2), and then rotate the reaction on a mixer for 30 minutes. After the rotation reaction, add 10 mg of EDC / NHS to the reaction system, using 25 mM sodium chloride as solvent. Continue to react on the mixer for 4 hours. After the reaction, centrifuge at 5000 g for 10 minutes, and repeatedly wash with ethanol 2-3 times to finally obtain colloidal gold-PS microsphere composite microspheres.

Citation Information

Patent Citations

  • Method for preparing inorganic / organic composite microspheres

    CN102008925A

  • Preparation method of polystyrene / gold composite microspheres

    CN102358783A

  • Dual-enhanced chemiluminescent immunoassay method based on metal enhanced luminescence and nano particle labelled amplification

    CN104280542A

  • Immunofluorescence colloidal gold nanoparticle material

    CN113376372A

  • Nucleic acid carrier microsphere and preparation method thereof

    CN114350656A