A surface silicon-rich ZSM-5 molecular sieve and preparation method thereof
By pre-modifying the aluminum source during the synthesis of ZSM-5 molecular sieves, ZSM-5 molecular sieves with a surface rich in silicon and mesopores can be directly synthesized, solving the problems of decreased crystallinity and cumbersome processes in the existing technology, and achieving the effects of high silicon-to-aluminum ratio and abundant mesopores.
Patent Information
- Application Number
- CN202111183763.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-10-11
AI Technical Summary
In existing technologies, when adjusting the acid sites on the surface of ZSM-5 molecular sieves, post-treatment methods easily lead to a decrease in crystallinity, while direct methods are cumbersome and unstable, making it difficult to achieve molecular sieves with a surface rich in silica and mesoporous structure.
By pre-modifying the aluminum source during the synthesis of molecular sieves, using silane reagents to modify the aluminum source, and mixing it with silicon source, template agent and water, followed by aging, crystallization and calcination, ZSM-5 molecular sieves with silicon-rich surface and rich mesopores can be directly synthesized.
This method significantly improves the silicon-to-aluminum ratio on the molecular sieve surface, enriches the mesoporous structure, maintains the crystallinity and stability of the molecular sieve, and simplifies the preparation process.
Smart Images

Figure CN115959677B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of molecular sieve catalysts and preparation thereof, and more particularly to an MFI structure type molecular sieve and a preparation method thereof. Background Art
[0002] ZSM-5 molecular sieve is a type of molecular sieve with MFI structure, which has two sets of intersecting pore structures, one is an elliptical ten-membered ring straight pore, the size of which is about 0.54nm×0.56nm, and the other is a circular ten-membered ring Z-shaped pore, the size of which is about 0.52nm×0.58nm. Its unique pore type allows reactants and products to enter and exit smoothly, and because there is no cage structure, it reduces the accumulation of by-products in the pores, thus showing high selectivity and stability.
[0003] The aluminum acid sites in the molecular sieve are the active centers of the catalyst, and their distribution inside and outside the molecular sieve has a direct impact on the reaction products. For example, in the alkylation reaction of benzene or toluene with methanol, the composition of the three xylene isomers in the product varies significantly with the aluminum content on the molecular sieve surface. Therefore, the surface modification of molecular sieves has always been a topic of research by scholars. Generally, there are two methods: direct synthesis of molecular sieves to modify the surface and post-treatment modification of molecular sieves.
[0004] CN101857243A discloses a method for adjusting the surface pore size of a ZSM-5 molecular sieve by surface dealumination and siliconization. The molecular sieve is modified by ammonium fluorosilicate, and the surface skeleton aluminum is isomorphously replaced by silicon, thereby changing the surface silicon-aluminum ratio and adjusting the surface pore size.
[0005] CN110586174A discloses a method of modifying a ZSM-5 molecular sieve with silane ester or silane, thereby making the catalyst surface silicon-rich, effectively reducing the pore size, and effectively improving the selectivity of paraxylene in xylene.
[0006] CN105621434A discloses a direct method for synthesizing a molecular sieve with shape-selective properties. The template used in the method is selected from sodium fluoride, ammonia water, ethylamine, n-butylamine, tetraethylammonium hydroxide, etc. The molar ratio of the raw materials is: template / SiO2=0.02-15; SiO2 / Al2O3=30-800.
[0007] CN102259018A discloses a ZSM-5 composite structure molecular sieve and a preparation method thereof. The method comprises first preparing a P-ZSM-5 molecular sieve by an impregnation method, and then mixing the P-ZSM-5 molecular sieve with a silicon source, a template agent and water for secondary crystallization to obtain a composite molecular sieve with a Silicalite-1 outer shell and a P-ZSM-5 inner layer.
[0008] Among the methods for adjusting the surface acid sites of ZSM-5, the post-treatment method is reported to be dominant. Although this method can significantly increase the surface silicon-aluminum ratio of the molecular sieve and adjust the pore size, it will inevitably cause the molecular sieve crystallinity to decrease, and the treatment conditions are also demanding, which can easily cause adverse effects on the acid sites of the bulk molecular sieve. There are few reports on the direct method. The general idea is to coat a layer of Silicate during the synthesis of the molecular sieve to achieve the purpose of surface modification, but the process is cumbersome, and the layered structure is not stable and is easy to peel off. Summary of the invention
[0009] In view of the shortcomings of the prior art, the present invention discloses a surface silicon-rich ZSM-5 molecular sieve and a preparation method thereof. The ZSM-5 molecular sieve provided by the present invention is surface silicon-rich and rich in mesoporous structure.
[0010] The first aspect of the present invention provides a surface silicon-rich ZSM-5 molecular sieve, wherein the bulk silicon-aluminum ratio of the molecular sieve, i.e., the SiO2 / Al2O3 molar ratio, is 50-200, wherein the surface silicon-aluminum ratio is 40%-88% higher than the bulk silicon-aluminum ratio; the total specific surface area is 380-520m 2 / g, total pore volume 0.50-0.62cm 3 / g, of which the mesopore volume accounts for 70%-85% of the total pore volume.
[0011] Furthermore, the mesopores described in the present invention refer to pores with a pore diameter of 2 nm to 50 nm.
[0012] Furthermore, in the surface silicon-rich ZSM-5 molecular sieve, the bulk silicon-to-aluminum ratio, i.e., the SiO2 / Al2O3 molar ratio, of the molecular sieve is preferably 50-150, and the surface silicon-to-aluminum ratio, i.e., the SiO2 / Al2O3 molar ratio, is preferably 75-340.
[0013] Furthermore, the total specific surface area of the silicon-rich ZSM-5 molecular sieve is 400-480m 2 / g.
[0014] Furthermore, in the surface silicon-rich ZSM-5 molecular sieve, the mesopore distribution is as follows: the pore volume occupied by pores with a pore diameter of 2-10 nm is 58%-65% of the total mesopore volume, the pore volume occupied by pores with a pore diameter of 10-30 nm is 28%-33% of the total mesopore volume, and the pore volume occupied by pores with a pore diameter of 30-50 nm is 2%-14% of the total mesopore volume.
[0015] Furthermore, in the surface silicon-rich ZSM-5 molecular sieve, the surface silicon-aluminum ratio, i.e., the SiO2 / Al2O3 molar ratio, is 70-375.
[0016] Furthermore, in the surface silicon-rich ZSM-5 molecular sieve, the mesopore volume is 0.42-0.51 cm 3 / g.
[0017] The second aspect of the present invention provides a method for preparing the above-mentioned surface silicon-rich ZSM-5 molecular sieve, comprising the following steps:
[0018] (1) firstly dissolving the silane reagent in a solvent, then adding an aluminum source, heating under reflux conditions, and drying to obtain a modified aluminum source;
[0019] (2) mixing the modified aluminum source obtained in step (1) with water, optionally adding a mineralizer, the pH value of the mixture is 10.5-12.5, and then adding a template agent and a silicon source in sequence to obtain a ZSM-5 molecular sieve mother liquor;
[0020] (3) The ZSM-5 molecular sieve mother liquid obtained in step (2) is subjected to aging treatment, crystallization, and calcination to obtain the surface silicon-rich ZSM-5 molecular sieve.
[0021] Furthermore, the solvent in step (1) is selected from one or more of acetone, benzene, toluene, ether, and carbon tetrachloride. The silane reagent is n-octyltriethylsilane, and the aluminum source is pseudo-boehmite, wherein the mass content of aluminum oxide in the pseudo-boehmite is 60%-85%.
[0022] Furthermore, in step (1), the silane reagent is dissolved in a solvent, and the mass ratio of the solvent to the silane reagent is 50-300.
[0023] Furthermore, in step (1), the mass ratio of the aluminum source to the silane reagent is 7-40, wherein the aluminum source is calculated as Al2O3.
[0024] Furthermore, the temperature of the heating treatment in step (1) is 80°C-150°C, preferably 100°C-130°C; and the treatment time is 4-24h.
[0025] Furthermore, after the heating treatment in step (1), conventional treatment steps such as solid-liquid separation (such as filtration) and washing may be performed, and then drying may be performed.
[0026] Furthermore, the drying conditions in step (1) are as follows: the drying temperature is 90-180° C., and the drying time is 4-48 hours.
[0027] Furthermore, the mineralizer in step (2) is one or more of sodium hydroxide, potassium hydroxide, and ammonium hydroxide. The template is tetrapropylammonium hydroxide. The silicon source is one or more of white carbon black, silica sol, silica gel, methyl orthosilicate, and ethyl orthosilicate.
[0028] Furthermore, in step (2), the modified aluminum source is calculated as Al2O3, the silicon source is calculated as SiO2, the mineralizer is recorded as N, the template is recorded as M, and the molar ratio of the silicon source, the modified aluminum source, the mineralizer, the template and water is: SiO2:Al2O3:N:M:H2O=1:0.003-0.03:0-0.3:0.15-0.5:10-50, N is the mineralizer, and M is the template.
[0029] Furthermore, in step (3), the aging treatment is carried out at 10-30°C, and the aging time is 0.5-12h, preferably 1-6h.
[0030] Furthermore, in step (3), the crystallization temperature is 110°C-200°C, preferably 120°C-180°C, and the crystallization time is 1-96h, preferably 1-72h.
[0031] Furthermore, in step (3), after crystallization, conventional solid-liquid separation, washing, drying and other operations are performed, and then calcined to obtain the surface silicon-rich ZSM-5 molecular sieve. The solid-liquid separation, washing, drying, calcination and ion exchange processes are conventional and mature processes well known to professionals in the field, without any special limitation. As the separation method, for example, a method of filtering the obtained mixture can be cited. Here, the filtration, washing and drying can be carried out in any conventional manner known in the art. For example, as the filtration, for example, the obtained product mixture can be simply filtered. As the washing, for example, washing with deionized water and / or ethanol can be cited. As the drying temperature, for example, 40-250°C, preferably 60-150°C, can be cited, and as the drying time, for example, 4-30 hours, preferably 4-20 hours can be cited. The drying can be carried out under normal pressure or under reduced pressure. The calcination can be carried out in any conventional manner known in the art, such as a calcination temperature of 300-800°C, preferably 400-650°C, and a calcination time of 1-12 hours, preferably 2-8 hours. In addition, the calcination is generally carried out in an oxygen-containing atmosphere, such as air or oxygen atmosphere. In order to obtain HZSM-5 molecular sieve, an ion exchange method such as ammonium exchange can be used.
[0032] Further, the ammonium exchange can be carried out in any conventional manner known in the art, wherein the ammonium salt used can be at least one of ammonium nitrate, ammonium chloride, etc., the concentration of the ammonium salt solution is 0.1-1 mol / L, and the ammonium exchange can be carried out in batches, such as 2-6 times. The conditions for each ammonium exchange are as follows: temperature is 20-90°C, time is 1-4h, and solid-liquid (mass) ratio is 1: (4-10).
[0033] Compared with the prior art, the present invention has the following advantages:
[0034] (1) The present invention provides a ZSM-5 molecular sieve with surface silicon-rich, and the molecular sieve structure is rich in mesoporous structures.
[0035] (2) The preparation method provided by the present invention can directly synthesize ZSM-5 molecular sieves with a surface silicon-rich structure. The method of the present invention pre-modifies the aluminum source for molecular sieve synthesis, effectively guides it into the molecular sieve framework, achieves the effect of surface silicon-rich, and introduces long-chain carbon molecules during the preparation process, and produces a rich mesoporous structure inside the molecular sieve after preparation and calcination. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The XRD spectra of the ZSM-5 molecular sieves obtained in Examples 1-2 and Comparative Examples are shown. DETAILED DESCRIPTION
[0037] The specific embodiments of the present invention are described in detail below, but it should be pointed out that the protection scope of the present invention is not limited by these specific embodiments, but is determined by the claims.
[0038] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definitions in this specification shall prevail.
[0039] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.
[0040] It should be particularly noted that two or more aspects (or implementation methods) disclosed in the context of this specification can be arbitrarily combined with each other, and the technical solutions (such as methods or systems) thus formed are part of the original disclosure of this specification and also fall within the scope of protection of the present invention.
[0041] Unless otherwise specified, all percentages, parts, ratios, etc. mentioned in this specification are based on weight, unless the weight basis does not conform to the common understanding of those skilled in the art.
[0042] In the present invention, the crystal phase of the molecular sieve is analyzed by using a Rigaku ultima IV X-ray powder diffractometer. Scanning and recording were performed with a nickel filter, a diffraction angle 2θ scanning range of 5-50°, an operating voltage of 35 kV, a current of 25 mA, and a scanning speed of 10° / min.
[0043] In the present invention, the specific surface area, pore volume and pore distribution of the ZSM-5 molecular sieve are measured by liquid nitrogen physical adsorption method, wherein the liquid nitrogen physical adsorption analysis measurement conditions are: American Micromeritics TriStar 3000 physical adsorption analyzer, analysis medium: N2, sample weight: 0.25g.
[0044] In the present invention, the ICP analysis (measuring bulk silicon-aluminum ratio) of the ZSM-5 molecular sieve is carried out on an IRIS XSP inductively coupled plasma atomic emission spectrometer of Thermo Company.
[0045] In the present invention, the ZSM-5 molecular sieve is subjected to XPS analysis (surface silicon-aluminum ratio measurement), and the test is carried out on an Axis DLD X-ray photoelectron spectrometer of Kratos Company.
[0046] [Example 1]
[0047] Preparation of modified aluminum source: Weigh 0.1 g of n-octyltriethoxysilane, disperse it in 8 g of toluene solvent, add 1 g of calcined pseudo-boehmite (alumina mass content is 70%), and reflux at 110° C. for 12 h. Centrifuge and wash the treated pseudo-boehmite, and dry it at 120° C. for 6 h.
[0048] Preparation of surface silicon-rich ZSM-5 molecular sieve: Weigh 0.22g of the above modified aluminum source and mix it with 50ml of deionized water, wherein the pH of the mixture is 11.5. Then add 15.0g of tetrapropylammonium hydroxide solution (mass content 25%), mix and stir evenly for 0.5h, then add 20g of ethyl orthosilicate (mass content of SiO2 is 28%), mix and stir evenly for 0.5h, continue to mix and stir evenly for 1h, then age for 1h, put it into a hydrothermal crystallization kettle, seal it and crystallize it at 180℃ for 2 days. After discharging, centrifuge the molecular sieve mother liquor, dry the obtained solid in an oven at 90℃ for 6h, and then roast it in a muffle furnace at 550℃ for 8h to obtain a hydrogen type molecular sieve.
[0049] The crystal structure of the hydrogen-type ZSM-5 molecular sieve obtained in Example 1 was characterized to obtain an XRD diffraction pattern, as shown in Figure 1 .
[0050] The hydrogen-type ZSM-5 molecular sieve obtained in Example 1 was subjected to physical adsorption analysis to obtain the specific surface area, total pore volume, mesopore volume and mesopore distribution. The results are shown in Table 1.
[0051] The bulk silicon-to-aluminum ratio of the hydrogen-type ZSM-5 molecular sieve obtained in Example 1 was measured by ICP analysis. The results are shown in Table 2.
[0052] The surface silicon-to-aluminum ratio of the hydrogen-type ZSM-5 molecular sieve obtained in Example 1 was measured by XPS analysis. The results are shown in Table 2.
[0053] [Example 2]
[0054] Preparation of modified aluminum source: Weigh 0.14 g of n-octyltriethoxysilane, disperse it in 20 g of toluene solvent, add 2 g of calcined pseudo-boehmite (alumina mass content is 70%), and reflux at 120° C. for 8 h. Centrifuge and wash the treated pseudo-boehmite, and dry it at 120° C. for 6 h.
[0055] Preparation of surface silicon-rich ZSM-5 molecular sieve: weigh 0.4g of the above modified aluminum source and 0.8g of sodium hydroxide and 100ml of deionized water, mix and stir evenly for 1h, wherein the pH of the mixture is 12.0, then add 36.2g of tetrapropylammonium hydroxide solution (mass content 25%), mix and stir evenly, add 45g of silica sol (mass content of SiO2 is 30%), mix and stir evenly for 1h, continue to mix and stir evenly for 1h, then age for 1h, put into a hydrothermal crystallization kettle, seal and crystallize at 180℃ for 2 days. After discharging, centrifuge the molecular sieve mother liquor, dry the obtained solid at 90℃ in an oven for 6h, and then roast at 550℃ in a muffle furnace for 8h to obtain the sodium type molecular sieve raw powder. The molecular sieve raw powder is ion exchanged with ammonium chloride solution to obtain the hydrogen type molecular sieve raw powder. The specific ion exchange conditions are: solid-liquid mass ratio: 1:6, exchange temperature: 90℃, exchange time: 2h, exchange times: 3 times.
[0056] The hydrogen-type ZSM-5 molecular sieve obtained in Example 2 was subjected to XRD crystal phase analysis, physical adsorption, ICP analysis, and XPS analysis under the same conditions as in Example 1. The results are shown in Figure 1 , Table 1-2.
[0057] [Example 3]
[0058] Preparation of modified aluminum source: Weigh 0.12g of n-octyltriethoxysilane, disperse it in 30g of solvent benzene, add 2g of pseudo-boehmite (alumina content 70%), and reflux for 12h at 110°C. Centrifuge and wash the treated pseudo-boehmite, and dry it at 120°C for 6h.
[0059] Secondly, prepare the surface silicon-rich ZSM-5 molecular sieve: weigh 0.3g of the above-mentioned modified aluminum source and 1.3g of sodium hydroxide and mix with 100 ml of deionized water, wherein the pH of the mixture is 11.3, then add 54.2g of tetrapropylammonium hydroxide solution (mass content 25%), mix and stir evenly for 1h, add 20g of white carbon black (mass content of SiO2 is 100%), 100g of deionized water, continue to mix and stir evenly for 1h, then age for 1h, put into a hydrothermal crystallization kettle, seal and crystallize at 180℃ for 2 days. After discharging, centrifuge the molecular sieve mother liquor, dry the obtained solid at 90℃ in an oven for 6h, and then roast at 550℃ in a muffle furnace for 8h to obtain the sodium type molecular sieve raw powder. The molecular sieve raw powder is ion exchanged with ammonium chloride solution to obtain the hydrogen type molecular sieve raw powder. The specific ion exchange conditions are: solid-liquid mass ratio: 1:6, exchange temperature: 90℃, exchange time: 2h, exchange times: 3 times.
[0060] The XRD pattern of the hydrogen-type ZSM-5 molecular sieve obtained in Example 3 is similar to that of Example 1, and has typical ZSM-5 characteristic peaks.
[0061] The hydrogen-type ZSM-5 molecular sieve obtained in Example 3 was subjected to physical adsorption, ICP analysis, and XPS analysis under the same conditions as in Example 1. The results are shown in Table 1-2.
[0062] [Comparative Example]
[0063] The preparation was carried out according to the preparation process of Example 1, except that the aluminum source was not modified.
[0064] The ZSM-5 molecular sieve obtained in the comparative example was subjected to XRD crystal phase analysis, physical adsorption, ICP analysis, and XPS analysis under the same conditions as in Example 1. Figure 1 , Table 1-2.
[0065] Table 1
[0066]
[0067] Table 2
[0068]
Claims
1. A surface silicon-rich ZSM-5 molecular sieve, in, The bulk silicon-aluminum ratio of the molecular sieve is SiO 2 / Al 2 O 3 The molar ratio is 50-200, of which the surface silicon-aluminum ratio is 40%-88% higher than the bulk silicon-aluminum ratio; the total specific surface area is 380-520m 2 / g, total pore volume 0.50-0.62cm 3 / g, of which the mesopore volume accounts for 70%-85% of the total pore volume.
2. The molecular sieve according to claim 1, It is characterized in that The bulk silicon-aluminum ratio of the molecular sieve is SiO 2 / Al 2 O 3 The molar ratio is 50-150, and the surface silicon-aluminum ratio is SiO 2 / Al 2 O 3 The molar ratio is 70-375.
3. The molecular sieve according to claim 1, It is characterized in that The total specific surface area of the molecular sieve is 400-480m 2 / g.
4. The molecular sieve according to claim 1, It is characterized in that The mesopore distribution of the molecular sieve is as follows: the pore volume occupied by pores with a pore diameter of 2-10 nm is 58%-65% of the total mesopore volume, the pore volume occupied by pores with a pore diameter of 10-30 nm is 28%-33% of the total mesopore volume, and the pore volume occupied by pores with a pore diameter of 30-50 nm is 2%-14% of the total mesopore volume.
5. The molecular sieve according to any one of claims 1 to 4, It is characterized in that In the molecular sieve, the surface silicon-aluminum ratio is SiO 2 / Al 2 O 3 The molar ratio is 75-340, and / or the mesopore volume is 0.42-0.51cm 3 / g.
6. A method for preparing the surface silicon-rich ZSM-5 molecular sieve according to any one of claims 1 to 5, comprising the following steps: (1) First, the silane reagent is dissolved in a solvent, then an aluminum source is added, heated under reflux conditions, and dried to obtain a modified aluminum source; (2) mixing the modified aluminum source obtained in step (1) with water, wherein the pH value of the mixture is 10.5-12.5, and then adding a template agent and a silicon source in sequence to obtain a ZSM-5 molecular sieve mother liquor; (3) The ZSM-5 molecular sieve mother liquor obtained in step (2) is subjected to aging treatment, crystallization, and calcination to obtain the surface silicon-rich ZSM-5 molecular sieve.
7. The preparation method according to claim 6, It is characterized in that In step (2), the modified aluminum source obtained in step (1) is mixed with water, and a mineralizer is added, and the pH value of the mixture is 10.5-12.
5.
8. The preparation method according to claim 6 or 7, It is characterized in that The solvent in step (1) is selected from one or more of acetone, benzene, toluene, ether, and carbon tetrachloride; the silane reagent is n-octyltriethylsilane, and the aluminum source is pseudo-boehmite, wherein the mass content of aluminum oxide in the pseudo-boehmite is 60%-85%; And / or, the template is tetrapropylammonium hydroxide; the silicon source is selected from one or more of white carbon black, silica sol, silica gel, methyl orthosilicate, and ethyl orthosilicate.
9. The preparation method according to claim 7, It is characterized in that The mineralizer in step (2) is one or more of sodium hydroxide, potassium hydroxide and ammonium hydroxide.
10. The preparation method according to claim 6 or 7, It is characterized in that In step (1), the silane reagent is dissolved in a solvent, and the mass ratio of the solvent to the silane reagent is 50-300; and / or, the mass ratio of the aluminum source to the silane reagent in step (1) is 7-40, wherein the aluminum source is Al 2 O 3 count.
11. The preparation method according to claim 6 or 7, It is characterized in that The heating treatment temperature in step (1) is 80°C-150°C; the treatment time is 4-24h; the drying conditions are as follows: the drying temperature is 90-180°C, and the drying time is 4-48h.
12. The preparation method according to claim 6 or 7, It is characterized in that The temperature of the heating treatment in step (1) is 100°C-130°C.
13. The preparation method according to claim 6, It is characterized in that In step (2), the aluminum source is modified to Al 2 O 3 The silicon source is SiO 2 The template is recorded as M, and the molar ratio of silicon source, modified aluminum source, template and water is: SiO 2 :Al 2 O 3 :M:H 2 O=1:0.003-0.03:0.15-0.5:10-50.
14. The preparation method according to claim 7, It is characterized in that In step (2), the aluminum source is modified to Al 2 O 3 The silicon source is SiO 2 The mineralizer is recorded as N, the template is recorded as M, and the molar ratio of silicon source, modified aluminum source, mineralizer, template and water is: SiO 2 :Al 2 O 3 :N:M:H 2 O=1: 0.003-0.03: 0-0.3: 0.15-0.5: 10-50, where the amount of N is not 0.
15. The preparation method according to claim 6 or 7, It is characterized in that The aging treatment in step (3) is carried out at 10-30°C for 0.5-12h; and / or the crystallization temperature is 110°C-200°C for 1-96h.
16. The preparation method according to claim 6 or 7, It is characterized in that The aging treatment in step (3) is carried out at 10-30°C for 1-6 hours; and / or the crystallization temperature is 120°C-180°C for 1-72 hours.