A high speed steel drill bit and preparation method thereof

The high-speed steel drill bit with conformal cooling and debris channels addresses the inefficiency of traditional drill bits by integrating advanced manufacturing techniques, enhancing heat dissipation and durability for improved drilling performance.

CN115971544BActive Publication Date: 2024-12-03GUANGDONG INST OF NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211725280.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-12-03
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

Traditional high-speed steel drill bits have simple structures that rely on linear cooling channels, which are ineffective in dissipating heat generated during operation, limiting their performance and service life, especially in modern manufacturing applications requiring precision and complexity.

Method used

Design and manufacture a high-speed steel drill bit with an internal conformal cooling channel and external debris channel, utilizing a direct and spiral flow configuration, and employing laser additive manufacturing and surface laser quenching to create a wear-resistant surface and tough core, integrated with a debris outlet channel.

Benefits of technology

The integrated cooling and debris channels enhance drilling efficiency and service life by uniformly dissipating heat and guiding out debris, while the laser processing reduces residual stress and deformation, resulting in a high-performance drill bit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115971544B_ABST
    Figure CN115971544B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-speed steel drill bit, comprising a working part, a neck, a shank and a cooling channel; the cooling channel comprises a direct current channel and a spiral channel arranged around the direct current channel, the direct current channel and the spiral channel are connected, the spiral channel has a coolant inlet, the direct current channel has a coolant outlet, the cooling channel is used to allow coolant to enter from the coolant inlet, flow through the spiral channel and the direct current channel in sequence, and then flow out from the coolant outlet; the cooling channel structure can effectively take away the heat generated by the drill bit during operation, thereby improving the drilling efficiency. The present invention also discloses a method for preparing a high-speed steel drill bit, which adopts low-power, slow scanning speed laser forming and layer-by-layer laser remelting methods to achieve integrated forming of complex high-speed steel drill bits, and prepares a high-speed steel drill bit with a hard and wear-resistant surface and high strength and toughness in the core through heat treatment and surface laser quenching, thereby solving the deformation and cracking problems of high-speed steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of drill manufacturing, and relates to a high-speed steel drill with a cooling channel and a preparation method thereof. Background Art

[0002] High-speed steel has high hardness, high wear resistance, high heat resistance and good toughness. It is the preferred material for drilling tools, cutting tools and molds that are subject to impact and vibration. Because it contains more carbon and alloy elements, high-speed steel prepared by traditional melting and electroslag remelting often forms coarse primary eutectic carbides and network secondary carbides. Powder metallurgy can solve the problem of coarse and uneven distribution of carbides, but it is limited by the pressing mold, and the structure and shape of its high-speed steel products are relatively simple. With the continuous development of modern industry, high-speed steel tools and molds are developing in the direction of precision, complexity and miniaturization, and the demand for special-shaped and complex structural products is becoming increasingly strong. However, due to the limitations of pressing molds and processing tools, the existing high-speed steel drill bits have a simple structure and can usually only rely on drilling to produce linear cooling channels, which cannot effectively take away the heat generated by the high-speed steel drill bits during operation. Summary of the invention

[0003] The purpose of the present invention is to meet the urgent needs of modern manufacturing industry for high-performance drilling tools, and to invent and design a high-speed steel drill bit with an internal conformal cooling channel and an external debris channel. That is, the shape of the internal cooling channel changes with the shape of the high-speed steel drill bit, and a debris outlet channel is added on the outside, which can greatly improve the cooling efficiency and drilling efficiency of the high-speed steel drill bit, and solve the problem that the simple linear cooling channel of the traditional high-speed steel drill bit cannot dissipate heat quickly and evenly.

[0004] One embodiment of the present invention provides a high-speed steel drill bit, comprising a working portion, a neck, a shank, and a cooling channel;

[0005] The working part includes a cutting part, a guide part and a debris channel; wherein the cutting part includes a cutting edge and a spiral groove, and the cutting part is used for drilling and cutting; the guide part includes an auxiliary cutting edge and a spiral groove, and the guide part is used to assist drilling and cutting and guide out cutting debris; the debris channel is located at the outer edges of the cutting part and the guide part, and is used to assist in guiding out cutting debris;

[0006] The cooling flow channel includes a direct flow channel located at the center of the high-speed steel drill bit and a spiral flow channel arranged around the direct flow channel. The direct flow channel and the spiral flow channel are connected and arranged. The spiral flow channel has a coolant inlet, and the direct flow channel has a coolant outlet. The cooling flow channel is used to allow coolant to enter from the coolant inlet, flow through the spiral flow channel and the direct flow channel in sequence, and then flow out from the coolant outlet.

[0007] In one of the embodiments, the chip channel includes two or more semi-arc channels, and the two or more semi-arc channels are symmetrically distributed along the central axis of the high-speed steel drill bit to assist in guiding out the cutting chips.

[0008] In one of the embodiments, the neck includes a circular chamfer, and the circular chamfer is used to avoid stress concentration.

[0009] In one of the embodiments, a threaded structure or a flat tail structure is provided at the end of the handle for fixing and transmitting force.

[0010] One embodiment of the present invention provides a method for preparing a high-speed steel drill bit, comprising the following steps:

[0011] Design and modeling steps: using 3D modeling software to design a 3D model of the high-speed steel drill bit as described in any one of the above embodiments, and performing layered slicing processing on the 3D model to obtain 3D model data of the high-speed steel drill bit;

[0012] Laser additive manufacturing steps: according to the three-dimensional model data of the high-speed steel drill bit, under the protection of an inert atmosphere, using a laser beam to heat and melt the pre-laid high-speed steel powder, allowing the high-speed steel to cool and deposit on a preheated substrate, and then using a laser beam to repeatedly melt and deposit layers; repeating the steps of laying high-speed steel powder, laser heating and melting high-speed steel powder, and laser repeatedly melting and depositing layers, to form a high-speed steel drill bit layer by layer;

[0013] Heat treatment and surface laser quenching treatment steps: after the high-speed steel drill bit is subjected to solid solution and oil quenching treatment, a fine-grained hardened layer is formed on the surface of the high-speed steel drill bit by laser quenching.

[0014] In one embodiment, in the process of using a laser beam to heat and melt the pre-laid high-speed steel powder, the laser forming parameters used include: laser power 100-190W, laser scanning speed 500-750mm / s, laser scanning spacing 50-100μm.

[0015] In one embodiment, in the process of repeatedly melting and depositing layers using a laser beam, the laser forming parameters used include: laser power of 100 to 190 W, laser scanning speed of 500 to 750 mm / s, and laser scanning spacing of 50 to 100 μm.

[0016] In one of the embodiments, during the process of repeatedly melting the deposited layer using a laser beam, the high-speed steel deposited layer is heated and melted 1-3 times to reduce the temperature gradient and residual stress and inhibit cracks.

[0017] In one of the embodiments, during the laser quenching process, a laser beam is used to quickly heat the surface of the high-speed steel drill bit, raising the surface temperature to 750-900°C, followed by air cooling to form a fine-grained hardened layer on the surface of the high-speed steel drill bit to obtain a wear-resistant surface and a tougher core.

[0018] The high-speed steel drill bit or the method for preparing the high-speed steel drill bit provided in the above embodiments has the following beneficial effects:

[0019] 1. A high-speed steel drill bit with an internal conformal cooling channel and an external debris channel is designed and manufactured to achieve structural and functional integration, greatly improving the drilling efficiency, cooling efficiency and service life of the drill bit. In particular, since the cooling channel includes a direct current channel located at the center of the high-speed steel drill bit and a spiral channel arranged around the direct current channel, and the direct current channel and the spiral channel are connected. When the high-speed steel drill bit is working, the coolant enters from the coolant inlet, flows through the spiral channel and the direct current channel in sequence, and then flows out from the coolant outlet. That is, the internal conformal cooling channel adopts an inner and outer surrounding structure to avoid mutual interference, that is, the coolant enters from the coolant inlet, flows through the conformal cooling channel that changes with the spiral shape of the high-speed steel drill bit, then passes through the direct current channel at the center of the high-speed steel drill bit, and finally flows out from the coolant outlet; the coolant flows through the internal conformal cooling channel to take away the heat generated when the drill bit is working, achieve uniform heat dissipation, and improve the drilling efficiency and service life of the drill bit.

[0020] 2. Use low-power, slow scanning speed laser additive manufacturing process to reduce temperature gradient and residual stress during molding, and further combine laser remelting to solve the deformation and cracking problems of high-speed steel.

[0021] 3. Use surface laser quenching technology to produce high-performance high-speed steel drill bits with hard and wear-resistant surface and high strength and toughness in the core. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A schematic diagram of the structure of a high-speed steel drill bit provided in Example 1 of the present invention;

[0023] Figure 2 for Figure 1 Schematic diagram of cooling channel of high speed steel drill bit;

[0024] Figure 3 A schematic diagram of the structure of a high-speed steel drill bit provided in Example 2 of the present invention;

[0025] Figure 4 for Figure 2 Schematic diagram of cooling channel of high speed steel drill bit;

[0026] Figure 5This is a photo of a high-speed steel product prepared by the conventional powder metallurgy process provided in Comparative Example 1 of the present invention;

[0027] Figure 6 This is a photo of the high-speed steel product provided in Comparative Example 2 of the present invention that was prepared without the layer-by-layer laser remelting process. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. The specific embodiments described herein are only used to explain the present invention and cannot be interpreted as limiting the present invention.

[0029] One embodiment of the present invention provides a high-speed steel drill bit, comprising a working portion, a neck, a shank, and a cooling channel;

[0030] The working part includes a cutting part, a guide part and a debris channel; wherein the cutting part includes a cutting edge and a spiral groove, and the cutting part is used for drilling and cutting; the guide part includes an auxiliary cutting edge and a spiral groove, and the guide part is used to assist drilling and cutting and guide out cutting debris; the debris channel is located at the outer edges of the cutting part and the guide part, and is used to assist in guiding out cutting debris;

[0031] The cooling flow channel includes a direct flow channel located at the center of the high-speed steel drill bit and a spiral flow channel arranged around the direct flow channel. The direct flow channel and the spiral flow channel are connected and arranged. The spiral flow channel has a coolant inlet, and the direct flow channel has a coolant outlet. The cooling flow channel is used to allow coolant to enter from the coolant inlet, flow through the spiral flow channel and the direct flow channel in sequence, and then flow out from the coolant outlet.

[0032] In the high-speed steel drill bit provided in the above embodiment, by setting a conformal cooling channel inside the high-speed steel drill bit and setting a debris channel outside, the structure and function of the high-speed steel drill bit are integrated, which greatly improves the drilling efficiency, cooling efficiency and service life of the drill bit. In particular, since the cooling channel includes a direct current channel located at the center of the high-speed steel drill bit and a spiral channel arranged around the direct current channel, and the direct current channel and the spiral channel are connected. When the high-speed steel drill bit is working, the coolant enters from the coolant inlet, flows through the spiral channel and the direct current channel in sequence, and then flows out from the coolant outlet. That is, the internal conformal cooling channel adopts an inner and outer surrounding structure to avoid mutual interference, that is, the coolant enters from the coolant inlet, flows through the conformal cooling channel that changes with the spiral shape of the high-speed steel drill bit, then passes through the direct current channel at the center of the high-speed steel drill bit, and finally flows out from the coolant outlet; the coolant flows through the internal conformal cooling channel to take away the heat generated when the drill bit is working, achieve uniform heat dissipation, and improve the drilling efficiency and service life of the drill bit.

[0033] In one of the embodiments, the chip channel includes two or more semi-arc channels, and the two or more semi-arc channels are symmetrically distributed along the central axis of the high-speed steel drill bit to assist in guiding out the cutting chips.

[0034] In one of the embodiments, the neck includes a circular chamfer, and the circular chamfer is used to avoid stress concentration.

[0035] In one of the embodiments, a threaded structure or a flat tail structure is provided at the end of the handle for fixing and transmitting force.

[0036] In one of the embodiments, in the guide portion, the distance between the spiral flow channel and the central axis of the high-speed steel drill bit is greater than the distance between the bottom of the spiral groove of the guide portion and the central axis of the high-speed steel drill bit, and the distance between the spiral flow channel and the central axis of the high-speed steel drill bit is less than the distance between the bottom of the debris channel and the central axis of the high-speed steel drill bit.

[0037] Another embodiment of the present invention provides a method for preparing a high-speed steel drill bit, comprising the following steps:

[0038] Design and modeling steps: using 3D modeling software to design a 3D model of the high-speed steel drill bit as described in any one of the above embodiments, and performing layered slicing processing on the 3D model to obtain 3D model data of the high-speed steel drill bit;

[0039] Laser additive manufacturing steps: according to the three-dimensional model data of the high-speed steel drill bit, under the protection of an inert atmosphere, using a laser beam to heat and melt the pre-laid high-speed steel powder, allowing the high-speed steel to cool and deposit on a preheated substrate, and then using a laser beam to repeatedly melt and deposit layers; repeating the steps of laying high-speed steel powder, laser heating and melting high-speed steel powder, and laser repeatedly melting and depositing layers, to form a high-speed steel drill bit layer by layer;

[0040] Heat treatment and surface laser quenching treatment steps: after the high-speed steel drill bit is subjected to solid solution and oil quenching treatment, a fine-grained hardened layer is formed on the surface of the high-speed steel drill bit by laser quenching.

[0041] In the method for preparing the high-speed steel drill bit provided in the above embodiment, a low-power, slow scanning speed laser additive manufacturing process is used to reduce the temperature gradient and residual stress during molding, and further combined with laser remelting to solve the deformation and cracking problems of high-speed steel. In addition, surface laser quenching technology is used to prepare a high-performance high-speed steel drill bit with a hard and wear-resistant surface and a high-strength and high-toughness core.

[0042] Selective laser melting (SLM) technology uses a high-energy-density laser beam as a heat source to selectively melt the pre-laid metal powder layer by layer, and form a three-dimensional metal entity through metallurgical bonding between layers. The moldless, rapid and economical SLM technology can overcome the challenges of shape and structure complexity, performance complexity and functional complexity faced by traditional processing methods, and has unique advantages in the molding of difficult-to-process materials. The cooling rate during SLM molding is as high as 10 6 ~10 8 K / s is conducive to the formation of fine-grained structure and the fine-grained strengthening effect, which is expected to solve the problems of microstructure segregation and coarse carbides in high-speed steel. However, there are few reports on SLM manufacturing of high-speed steel. This is because high-carbon equivalent and high hardenability high-speed steel has poor welding performance and is prone to deformation and even cracking during SLM rapid melting-solidification molding.

[0043] In the method for preparing a high-speed steel drill bit provided in the above embodiment, a high-speed steel drill bit with integrated structure and function is designed and prepared by laser selective melting SLM technology, breaking through the limitation of traditional forming process on complex shapes, realizing integrated forming of complex internal and external structures, improving the cooling speed and cutting efficiency of the drill tool, and extending the service life. The layer-by-layer laser remelting method is adopted to reduce the temperature gradient and cooling speed, and solve the deformation and cracking problems of SLM-formed high-speed steel.

[0044] In one embodiment, in the process of using a laser beam to heat and melt the pre-laid high-speed steel powder, the laser forming parameters used include: laser power 100-190W, laser scanning speed 500-750mm / s, laser scanning spacing 50-100μm.

[0045] In one embodiment, in the process of repeatedly melting and depositing layers using a laser beam, the laser forming parameters used include: laser power of 100 to 190 W, laser scanning speed of 500 to 750 mm / s, and laser scanning spacing of 50 to 100 μm.

[0046] In one of the embodiments, during the process of repeatedly melting the deposited layer using a laser beam, the high-speed steel deposited layer is heated and melted 1-3 times to reduce the temperature gradient and residual stress and inhibit cracks.

[0047] In one of the embodiments, during the laser quenching process, a laser beam is used to quickly heat the surface of the high-speed steel drill bit, raising the surface temperature to 750-900°C, followed by air cooling to form a fine-grained hardened layer on the surface of the high-speed steel drill bit to obtain a wear-resistant surface and a tougher core.

[0048] The high-speed steel drill bit or the method for preparing the high-speed steel drill bit provided in the embodiments of the present invention will be described in detail with reference to specific embodiments below.

[0049] Example 1

[0050] (1) Structure of high-speed steel drill bit

[0051] Please also see Figure 1 and Figure 2The high-speed steel drill bit 100 provided in Example 1 of the present invention includes: a working part 110, a neck 120, a shank 130, and an internal conformal cooling channel 140 that changes with the shape of the drill bit. The working part 110 includes a cutting part 111, a guide part 112, and four outer chip channels 113. The cutting part 111 includes a cutting edge 1111 and a spiral groove 1112, and the cutting part 111 is used for drilling and cutting; the guide part 112 includes an auxiliary cutting edge 1121 and a spiral groove 1122, and the guide part 112 assists in drilling and cutting, and guides out the cutting chips; the outer side of the high-speed steel drill bit is designed with four semi-arc chip channels 113, and the four semi-arc chip channels 113 are symmetrically distributed along the central axis of the drill bit to assist in guiding out the cutting chips. The neck 120 is designed with an arc chamfer 121 to avoid stress concentration. There is a flat tail structure 131 at the end of the shank 130. The internal conformal cooling channel 140 adopts an inner and outer surrounding structure. That is, the cooling channel 140 includes a direct flow channel 141 located at the center of the high-speed steel drill bit and a spiral channel 142 arranged around the direct flow channel 141, and the direct flow channel 141 and the spiral flow channel 142 are arranged in communication. The spiral flow channel 142 has a coolant inlet 1421, and the direct flow channel 141 has a coolant outlet 1411. The coolant enters from the coolant inlet 1421, flows through the conformal cooling channel 140 that changes with the spiral shape of the high-speed steel drill bit, then passes through the direct flow channel 141 at the center of the high-speed steel drill bit, and finally flows out from the coolant outlet 1411, achieving a uniform heat dissipation effect.

[0052] (2) Integrated molding of high-speed steel drill bits

[0053] 1) Design and modeling steps

[0054] The high-speed steel drill bit model is designed using 3D modeling software. The model is sliced ​​and layered with a layer thickness of 30 μm to obtain the 3D model data of the high-speed steel drill bit;

[0055] 2) Laser additive manufacturing steps

[0056] Select CPM4V high-speed steel powder as the raw material, and lay a thin layer of high-speed steel powder on the substrate;

[0057] According to the three-dimensional model data of the high-speed steel drill bit, a laser beam is used to heat and melt the pre-laid thin layer of high-speed steel powder under the protection of an inert atmosphere, so that the high-speed steel is cooled and deposited on the preheated substrate. The laser forming parameters include: laser power 100W, laser scanning speed 500mm / s, laser scanning spacing 50μm;

[0058] Then, the high-speed steel deposited layer is heated and melted again using the same laser parameters as those used for laser forming, thereby reducing residual stress and crack density;

[0059] Repeating the steps of laying high-speed steel powder, laser heating and melting the high-speed steel powder, and laser repeatedly melting and depositing layers, the high-speed steel drill is integrally formed layer by layer;

[0060] 3) Heat treatment and surface laser quenching steps

[0061] The high speed steel drill bit is heated to 1150° C. and kept at this temperature for 1 hour for solution treatment, and then placed in quenching oil for rapid cooling;

[0062] A high-energy laser beam is used to heat the working part (110) of a high-speed steel drill bit, so that the surface temperature of the working part (110) rises to 750°C, and then air-cooled to form a fine-grained hardened layer on the surface of the high-speed steel drill bit, thereby achieving fine-grained strengthening and martensite strengthening effects, making the surface of the high-speed steel drill bit hard and wear-resistant, while the core still has high toughness.

[0063] Example 2

[0064] (1) High-speed steel drill bit structure

[0065] Please also see Figure 3 and Figure 4 The high-speed steel drill bit 200 provided in Example 4 of the present invention includes a high-speed steel drill bit including: a working portion 210, a neck portion 220, a shank portion 230, and an internal conformal cooling channel 240 that changes with the shape of the drill bit.

[0066] The working part 210 includes a cutting part 211, a guide part 212, and five chip channels 213 on the outside. The cutting part 211 includes a cutting edge 2111 and a spiral groove 2112, and the cutting part 211 is used for drilling and cutting. The guide part 212 includes an auxiliary cutting edge 2121 and a spiral groove 2122, and the guide part 212 is used to assist drilling and cutting, and to guide out cutting chips. Five semi-arc chip channels 213 are designed on the outside of the high-speed steel drill bit. The five semi-arc chip channels 213 are symmetrically distributed along the center axis of the drill bit to assist in guiding out cutting chips. The neck 220 is designed with an arc-shaped chamfer 221, and the arc-shaped chamfer 221 is used to avoid stress concentration. A threaded structure 231 is designed at the end of the shank 230. The internal conformal cooling channel 240 adopts an inner and outer surrounding structure. That is, the cooling channel 240 includes a direct flow channel 241 located at the center of the high-speed steel drill bit and a spiral channel 242 arranged around the direct flow channel 241, and the direct flow channel 241 and the spiral flow channel 242 are arranged in communication. The spiral flow channel 242 has a coolant inlet 2421, and the direct flow channel 241 has a coolant outlet 2411. The coolant enters from the coolant inlet 2421, flows through the conformal cooling channel 240 that changes with the spiral shape of the high-speed steel drill bit, then passes through the direct flow channel 241 at the center of the high-speed steel drill bit, and finally flows out from the coolant outlet 2411, achieving a uniform heat dissipation effect.

[0067] (2) Integrated molding of high-speed steel drill bits

[0068] 1) Design and modeling steps

[0069] The high-speed steel drill bit model is designed using 3D modeling software. The model is sliced ​​and layered with a layer thickness of 50 μm to obtain the 3D model data of the high-speed steel drill bit;

[0070] 2) Laser additive manufacturing steps

[0071] Select M2 high-speed steel powder as the raw material and lay a thin layer of high-speed steel powder on the substrate;

[0072] According to the three-dimensional model data of the high-speed steel drill bit, a laser beam is used to heat and melt the pre-laid thin layer of high-speed steel powder under the protection of an inert atmosphere, so that the high-speed steel is cooled and deposited on the preheated substrate. The laser forming parameters include: laser power 190W, laser scanning speed 750mm / s, laser scanning spacing 100μm;

[0073] Then, the high-speed steel deposited layer was heated and melted twice using the same laser parameters as those for laser forming to reduce residual stress and crack density;

[0074] Repeating the steps of laying high-speed steel powder, laser heating and melting the high-speed steel powder, and laser repeatedly melting and depositing layers, the high-speed steel drill is integrally formed layer by layer;

[0075] 3) Heat treatment and surface laser quenching steps

[0076] The high speed steel drill bit is heated to 1050°C and kept at this temperature for 2 hours for solution treatment, and then placed in quenching oil for rapid cooling;

[0077] The working part 210 of the high-speed steel drill bit is heated by a high-energy laser beam, so that the surface temperature of the working part 210 rises to 900°C, and then air-cooled to form a fine-grained hardened layer on the surface of the high-speed steel drill bit, thereby achieving fine-grain strengthening and martensite strengthening effects, making the surface of the high-speed steel drill bit hard and wear-resistant, while the core still has high strength and toughness.

[0078] Comparative Example 1

[0079] Powder metallurgy technology solves the common network carbide problem of traditional cast high-speed steel. The carbide particles in the prepared high-speed steel are very fine and evenly distributed, which significantly improves its toughness. However, the powder metallurgy process relies on the mold to press the high-speed steel powder into shape, resulting in a simple appearance and structure of the high-speed steel product, such as Figure 5 The spiral structure of the drill bit often requires subsequent machining, and it is impossible to realize the internal conformal cooling channel.

[0080] Comparative Example 2

[0081] The same high-speed steel material and laser additive manufacturing parameters as in Example 1 were used, but no layer-by-layer laser remelting was performed. Due to the high carbon and high alloy content in the high-speed steel, the high cooling rate and periodic thermal effect during the laser additive manufacturing process produced a brittle microstructure and high residual thermal stress, which did not cause the CMP4V high-speed steel to crack. Figure 6 shown.

[0082] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a high-speed steel drill bit, characterized in that: The following steps are involved: Design and modeling steps: design a three-dimensional model of a high-speed steel drill bit using three-dimensional modeling software, perform layered slicing processing on the three-dimensional model, and obtain three-dimensional model data of the high-speed steel drill bit; the high-speed steel drill bit includes a working part, a neck, a shank, and a cooling channel; the working part includes a cutting part, a guide part, and a chip channel; wherein the cutting part includes a cutting edge and a spiral groove, and the cutting part is used for drilling and cutting; the guide part includes an auxiliary cutting edge and a spiral groove, and the guide part is used for assisting drilling and cutting and exporting cutting chips; the chip channel is located between the cutting part and the The outer edge of the guide part includes two or more semi-arc channels, and the two or more semi-arc channels are symmetrically distributed along the central axis of the high-speed steel drill bit, and are used to assist in guiding out cutting debris; the cooling flow channel includes a direct flow channel located at the center of the high-speed steel drill bit and a spiral flow channel arranged around the direct flow channel, the direct flow channel and the spiral flow channel are connected, the spiral flow channel has a coolant inlet, and the direct flow channel has a coolant outlet, and the cooling flow channel is used to allow coolant to enter from the coolant inlet, flow through the spiral flow channel and the direct flow channel in sequence, and then flow out from the coolant outlet; Laser additive manufacturing steps: according to the three-dimensional model data of the high-speed steel drill bit, under the protection of an inert atmosphere, using a laser beam to heat and melt the pre-laid high-speed steel powder, allowing the high-speed steel to cool and deposit on a preheated substrate, and then using a laser beam to repeatedly melt and deposit layers; repeating the steps of laying high-speed steel powder, laser heating and melting high-speed steel powder, and laser repeatedly melting and depositing layers, to form a high-speed steel drill bit layer by layer; Heat treatment and surface laser quenching treatment steps: after the high-speed steel drill bit is subjected to solid solution and oil quenching treatment, a fine-grained hardened layer is formed on the surface of the high-speed steel drill bit by laser quenching.

2. The method for preparing a high speed steel drill bit according to claim 1, characterized in that: In the process of using a laser beam to heat and melt the pre-laid high-speed steel powder, the laser forming parameters used include: laser power 100-190W, laser scanning speed 500-750mm / s, laser scanning spacing 50-100μm.

3. The method for preparing a high speed steel drill bit according to claim 2, characterized in that: In the process of repeatedly melting and depositing layers using a laser beam, the laser forming parameters used include: laser power 100~190W, laser scanning speed 500~ 750mm / s, laser scanning interval 50~100μm.

4. The method for preparing a high speed steel drill bit according to claim 3, characterized in that: In the process of repeatedly melting the deposited layer using a laser beam, the high-speed steel deposited layer is heated and melted 1-3 times to reduce the temperature gradient and residual stress and inhibit cracks.

5. The method for preparing a high speed steel drill bit according to claim 1, characterized in that: During the laser quenching process, a laser beam is used to quickly heat the surface of the high-speed steel drill bit, raising its surface temperature to 750-900°C, followed by air cooling to form a fine-grained hardened layer on the surface of the high-speed steel drill bit to obtain a wear-resistant surface and a tougher core.

6. The method for preparing a high speed steel drill bit according to claim 1, characterized in that: The cooling channel is a conformal cooling channel.

7. The method for preparing a high speed steel drill bit according to claim 1, characterized in that: The neck includes an arc-shaped chamfer, and the arc-shaped chamfer is used to avoid stress concentration.