A hydrophilic silicone oil composition and preparation method thereof

By reacting polyethyleneimine and diorganopolysiloxane containing reactive functional groups in water, combined with a reaction catalyst, a simple and environmentally friendly preparation of hydrophilic silicone oil is achieved, which solves the problems of using organic solvents and heating in the existing technology. , a stable and reactive hydrophilic silicone oil composition was obtained.

CN115976838BActive Publication Date: 2024-10-29CHONGQING JIAOTONG UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310112956.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-14
Publication Date
2024-10-29
Estimated Expiration
2043-02-14

AI Technical Summary

Technical Problem

The existing method of preparing hydrophilic silicone oil through modification of hydrophilic polymers is not simple and environmentally friendly. It usually requires the use of organic solvents and heating, and requires additional separation and purification steps after the reaction.

Method used

The hydrophilic silicone oil composition can be obtained by reacting polyethyleneimine, diorganopolysiloxane containing reactive functional groups and reaction catalyst in water with rapid stirring at room temperature, avoiding organic solvents and heat treatment.

Benefits of technology

A simple and environmentally friendly preparation process is achieved, and the hydrophilic silicone oil composition obtained has excellent water dispersion system stability, silicone oil intrinsic hydrophobicity and subsequent reactivity, without adding surfactants or dispersants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115976838B_ABST
    Figure CN115976838B_ABST
Patent Text Reader

Abstract

The invention discloses a hydrophilic silicone oil composition and a preparation method thereof, and relates to the field of chemical technology. The present invention includes at least the following components: polyethyleneimine, a diorganopolysiloxane containing reactive functional groups, a reaction catalyst and water, the mass ratio of the polyethyleneimine to water is 1:9-7:3, and the mass ratio of the diorganopolysiloxane containing reactive functional groups to the mass ratio of polyethyleneimine is 0.0001-2. The preparation method of the present invention is simpler, environmentally friendly, and energy-saving. The preparation process only uses water as a solvent, rarely involves an organic solvent, and only needs to be carried out at room temperature, without additional heating and vacuuming and other separation and purification steps. The obtained hydrophilic silicone oil composition has excellent water dispersion system stability, silicone oil intrinsic hydrophobicity and subsequent reactivity at the same time, and no surfactant or dispersant is added in the hydrophilic silicone oil composition system, and can be mixed with water in any proportion, and the dispersion system stability is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical engineering, in particular to a hydrophilic silicone oil composition and a preparation method thereof. Background Art

[0002] Silicone oil generally refers to liquid linear polysiloxane products, which are difficult to disperse stably in water due to their hydrophobicity. Silicone oil mixtures with water as the dispersion medium have important application value in the textile industry, leather industry, coating industry, paper industry, daily chemicals and building materials.

[0003] At present, the preparation methods of silicone oil water dispersion system mainly include two categories. One is to disperse silicone oil or silicone oil precursor in water to form an emulsion with the help of surfactants or other dispersants, and the other is to hydrophilically modify silicone oil and introduce hydrophilic substances into silicone oil molecules to improve the dispersibility of silicone oil in water. Among them, the particle size of silicone oil obtained by the dispersion method using surfactants or dispersants is relatively large, and the long-term storage stability of the dispersion system is not as good as that of the dispersion system formed by hydrophilic modified silicone oil. In addition, the system contains a large amount of surfactants and other substances that are not covalently linked to the silicone oil, which affects subsequent use.

[0004] Hydrophilic modified silicone oil generally introduces hydrophilic groups or polymers into the silicone oil molecular structure by means of covalent bonds. Hydrophilic modified silicone oil generally can disperse spontaneously in water without additional additives. If the hydrophilic silicone oil in the current patent adopts the hydrophilic modification of the side groups on the silicone oil main chain, the hydrophobic properties of the silicone oil itself cannot be maintained if the modification ratio is too high, and the stability of its water dispersion system cannot be guaranteed if the modification ratio is too low. When the hydrophilic silicone oil obtained by water-soluble polyether modification lacks reactive functional groups in the molecular structure. Therefore, it is difficult for current hydrophilic silicone oil products to simultaneously achieve the stability of the water dispersion system, the intrinsic hydrophobicity of the silicone oil, and the subsequent reactivity.

[0005] Reference patent number CN1927910A is a preparation method of amino / epoxy co-modified hydrophilic silicone oil, which requires isopropanol as a solvent to dissolve isopropanol and hydrogen-containing silicone oil, and the reaction process needs to be heated to 90°C for more than 3 hours, and after the reaction is completed, vacuum treatment is required to obtain the desired product;

[0006] Reference patent number CN101497697A is a method for preparing a block water-soluble hydrophilic silicone oil. This method also requires a reaction in an organic solvent and requires different reaction treatments between 60°C and 90°C. Finally, vacuuming the organic solvent is still required to obtain the desired product.

[0007] Reference patent number CN112321834A is a method for preparing a hydrophilic silicone oil, using isooctyl alcohol as a reaction solvent, reacting at 70°C, and heating to volatilize and remove the organic solvent. In addition, an emulsifier needs to be added to obtain a silicone oil water dispersion system;

[0008] Reference patent number CN105111450A is a method for preparing hydrophilic silicone oil for leather treatment, which still uses an organic solvent as a reaction medium and needs to be heated to 80°C-120°C under nitrogen protection to promote the reaction;

[0009] Reference patent number CN109400885A is a method for preparing a hydrophilic amino silicone oil with a comb-like structure. Isopropyl alcohol is also used as a reaction solvent, and a multi-step reaction is carried out between 60°C and 120°C. Although the vacuum separation step is not mentioned in these two patents, the final products contain unseparated organic solvents.

[0010] By referring to the above patents, it can be seen that the existing method for preparing hydrophilic silicone oil by modifying hydrophilic polymers is not simple and environmentally friendly. Either an organic solvent needs to be used to solve the compatibility problem between the polymer and the silicone oil, or a surfactant needs to be added to the water to disperse the silicone oil in the water. In addition, heating is basically required to promote the reaction, and additional separation and purification steps are required after the reaction. Summary of the invention

[0011] The purpose of the present invention is to provide a hydrophilic silicone oil composition and a preparation method thereof to solve the existing problem: the existing preparation method of hydrophilic silicone oil by modifying a hydrophilic polymer is not simple and environmentally friendly, and either an organic solvent needs to be used to solve the compatibility problem between the polymer and the silicone oil, or a surfactant needs to be added to water to disperse the silicone oil in the water, and basically heating is required to promote the reaction, and additional separation and purification steps are required after the reaction.

[0012] To achieve the above object, the present invention provides the following technical solution: a hydrophilic silicone oil composition, comprising at least the following components: polyethyleneimine, diorganopolysiloxane containing reactive functional groups, a reaction catalyst and water.

[0013] Preferably, the mass ratio of the polyethyleneimine to water is 1:9-7:3, the mass ratio of the diorganopolysiloxane containing reactive functional groups to the polyethyleneimine is 0.0001-2, and the mass ratio of the reaction catalyst to the polyethyleneimine is 0-0.4.

[0014] Preferably, the polyethyleneimine includes at least one of linear polyethyleneimine and branched polyethyleneimine.

[0015] Preferably, the reaction catalyst includes an acid-base regulator and an alcohol regulator.

[0016] Preferably, the acid-base regulator includes at least one or more of acetic acid, ammonia water, triethylamine, sodium hydroxide, sodium bicarbonate, sodium carbonate, 4-dimethylaminopyridine and pyridine.

[0017] Preferably, the alcohol regulator includes at least one or more of ethanol, glycerol and isopropanol.

[0018] Preferably, the diorganopolysiloxane containing reactive functional groups has an average structural formula of:

[0019]

[0020] In the formula, A comprises a reactive functional group, and the reactive functional group comprises at least one or more of an epoxy group and a carbon-carbon double bond;

[0021] In the formula, R1 is at least one of an alkane group and an alkoxy group;

[0022] In the formula, R2 includes at least one or more of the same substance as the reactive functional group, an alkane group and an alkoxy group.

[0023] A method for preparing a hydrophilic silicone oil composition is used for the above content, comprising at least the following steps:

[0024] S1: dissolving polyethyleneimine in water to obtain a polyethyleneimine aqueous solution;

[0025] S2: mixing a reaction catalyst, a diorganopolysiloxane containing a reactive functional group and the above-mentioned polyethyleneimine aqueous solution;

[0026] S3: Rapidly stir at room temperature for more than 6 hours to obtain the aqueous silicone oil composition.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. The preparation method of the present invention is simpler, more environmentally friendly and energy-saving. The preparation process only uses water as a solvent and rarely involves organic solvents. At the same time, it only needs to be carried out at room temperature without additional heating and vacuuming and other separation and purification steps.

[0029] 2. The hydrophilic silicone oil composition obtained by the present invention has excellent water dispersion system stability, intrinsic hydrophobicity of silicone oil and subsequent reactivity. No surfactant or dispersant is added to the hydrophilic silicone oil composition system, and it can be mixed with water in any proportion. The dispersion system has excellent stability and there is no stratification or precipitation within one year of storage at room temperature. The hydrophilic silicone oil retains the original hydrophobicity of the silicone oil molecules while introducing a large number of amino groups for subsequent reactions. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0031] Figure 1 is an average structural formula representation of the diorganopolysiloxane containing reactive functional groups of the present invention as a whole;

[0032] Figure 2 This is a schematic diagram of the appearance of the hydrophilic silicone oil composition of the present invention;

[0033] Figure 3 Schematic diagram of the contact angle of cotton fabric after being treated with hydrophilic silicone oil of the present invention;

[0034] picture 4 Schematic diagram of the surface morphology and elemental analysis of cotton fabric after treatment with hydrophilic silicone oil of the present invention. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0036] See also Figure 1-4 , a hydrophilic silicone oil composition, comprising at least the following components: polyethyleneimine, diorganopolysiloxane containing reactive functional groups, a reaction catalyst and water.

[0037] The aqueous dispersion system formed after the polyethyleneimine and the silicone oil containing reactive functional groups react in water, the hydrophilic silicone oil composition can be spontaneously dispersed in water in any proportion without adding any surfactant or dispersant, and the dispersion system is stable for a long time, has a small dispersed particle size, and has functional groups that can be subsequently reacted.

[0038] The mass ratio of polyethyleneimine to water is 1:9-7:3, preferably 3:7-6:4.

[0039] The mass ratio of the diorganopolysiloxane containing reactive functional groups to the polyethyleneimine is 0.0001-2, preferably 0.1-0.5.

[0040] The mass ratio of the reaction catalyst to the mass of polyethyleneimine is 0-0.4.

[0041] The polyethyleneimine includes at least one of linear polyethyleneimine and branched polyethyleneimine;

[0042] The reaction catalyst includes an acid-base regulator and an alcohol regulator;

[0043] The acid-base regulator includes at least one or more of acetic acid, ammonia water, triethylamine, sodium hydroxide, sodium bicarbonate, sodium carbonate, 4-dimethylaminopyridine and pyridine;

[0044] The alcohol regulator includes at least one or more of ethanol, glycerol and isopropanol;

[0045] The diorganopolysiloxane containing reactive functional groups has an average structural formula of Figure 1 As shown, wherein A is a reactive functional group, the reactive functional group includes at least one or more of an epoxy group and a carbon-carbon double bond, preferably an epoxy group, wherein, wherein, R1 is at least one of an alkane group and an alkoxy group, wherein, R2 includes at least one or more of the same substance as the reactive functional group, an alkane group and an alkoxy group;

[0046] A method for preparing a hydrophilic silicone oil composition is used for the above content, comprising at least the following steps:

[0047] S1: dissolving polyethyleneimine in water to obtain a polyethyleneimine aqueous solution;

[0048] S2: mixing a reaction catalyst, a diorganopolysiloxane containing a reactive functional group and the above-mentioned polyethyleneimine aqueous solution;

[0049] S3: Rapidly stir at room temperature for more than 6 hours to obtain an aqueous silicone oil composition.

[0050] The reaction temperature is within the normal room temperature range and no additional heating is required.

[0051] In order to enable those skilled in the art to more clearly understand the technical solution of the present disclosure, the technical solution of the present disclosure will be described in detail below in combination with specific embodiments and comparative examples.

[0052] Embodiment 1:

[0053] Weigh 10 g of polyethyleneimine with an average molecular weight of 10,000 Da, add it into 10 g of deionized water, and stir to dissolve evenly.

[0054] 0.6 g of triethylamine and 5 g of polydimethylsiloxane having an average molecular weight of 5000 Da and a single-terminal epoxy group were added to the above solution.

[0055] The above system was rapidly stirred at room temperature for 48 hours and then the reaction was stopped.

[0056] Embodiment 2:

[0057] Weigh 10 g of polyethyleneimine with an average molecular weight of 10,000 Da and add it to 15 g of deionized water, stirring to dissolve evenly;

[0058] Add 0.6 g of triethylamine and 5 g of polydimethylsiloxane having an average molecular weight of 5000 Da and a single-terminal epoxy group into the above solution;

[0059] The above system was rapidly stirred at room temperature for 48 hours and then the reaction was stopped.

[0060] Embodiment 3:

[0061] Weigh 10 g of polyethyleneimine with an average molecular weight of 10,000 Da and add it to 20 g of deionized water, stirring to dissolve evenly;

[0062] Add 0.6 g of triethylamine and 5 g of polydimethylsiloxane having an average molecular weight of 5000 Da and a single-terminal epoxy group into the above solution;

[0063] The above system was rapidly stirred at room temperature for 48 hours and then the reaction was stopped.

[0064] Embodiment 4:

[0065] Weigh 10 g of polyethyleneimine with an average molecular weight of 25,000 Da, add it to 20 g of deionized water, and stir to dissolve evenly;

[0066] Add 0.6 g of triethylamine and 5 g of polydimethylsiloxane having an average molecular weight of 5000 Da and a single-terminal epoxy group into the above solution;

[0067] The above system was rapidly stirred at room temperature for 48 hours and then the reaction was stopped.

[0068] Embodiment 5:

[0069] Weigh 10 g of polyethyleneimine with an average molecular weight of 25,000 Da, add it to 20 g of deionized water, and stir to dissolve evenly;

[0070] Add 0.6 g of triethylamine and 2 g of polydimethylsiloxane having an average molecular weight of 5000 Da and a single-terminal epoxy group into the above solution;

[0071] The above system was rapidly stirred at room temperature for 48 hours and then the reaction was stopped.

[0072] Embodiment 6:

[0073] Weigh 10 g of polyethyleneimine with an average molecular weight of 25,000 Da, add it to 20 g of deionized water, and stir to dissolve evenly;

[0074] Add 0.6 g of triethylamine and 3 g of polydimethylsiloxane having an average molecular weight of 5000 Da and a single-terminal epoxy group into the above solution;

[0075] The above system was rapidly stirred at room temperature for 48 hours and then the reaction was stopped.

[0076] Embodiment 7:

[0077] Weigh 10 g of polyethyleneimine with an average molecular weight of 25,000 Da, add it to 20 g of deionized water, and stir to dissolve evenly;

[0078] Add 0.3 g of triethylamine and 3 g of polydimethylsiloxane having an average molecular weight of 5000 Da and a single-terminal epoxy group into the above solution;

[0079] The above system was rapidly stirred at room temperature for 48 hours and then the reaction was stopped.

[0080] Embodiment 8:

[0081] Weigh 10 g of polyethyleneimine with an average molecular weight of 25,000 Da, add it to 20 g of deionized water, and stir to dissolve evenly;

[0082] Add 0.8 g of triethylamine and 3 g of polydimethylsiloxane having an average molecular weight of 5000 Da and a single-terminal epoxy group into the above solution;

[0083] The above system was rapidly stirred at room temperature for 48 hours and then the reaction was stopped.

[0084] Embodiment 9:

[0085] Weigh 10 g of polyethyleneimine with an average molecular weight of 10,000 Da and add it to 20 g of deionized water, stirring to dissolve evenly;

[0086] Add 0.4 g of triethylamine and 2 g of polydimethylsiloxane with an average molecular weight of 2000 Da and a carbon-carbon double bond at one end to the above solution;

[0087] The above system was rapidly stirred at room temperature for 48 hours and then the reaction was stopped.

[0088] Embodiment 10:

[0089] Weigh 10 g of polyethyleneimine with an average molecular weight of 25,000 Da, add it to 20 g of deionized water, and stir to dissolve evenly;

[0090] Add 0.4 g of triethylamine and 2 g of polydimethylsiloxane with an average molecular weight of 2000 Da and a carbon-carbon double bond at one end to the above solution;

[0091] The above system was rapidly stirred at room temperature for 48 hours and then the reaction was stopped.

[0092] Figure 2The appearance of the hydrophilic silicone oil composition after being placed for one year is given in FIG. 1 . It can be found that the hydrophilic composition is transparent as a whole, without stratification and precipitation, indicating the excellent stability of the hydrophilic composition.

[0093] To further illustrate the properties of the hydrophilic silicone oil composition, it was used in a hydrophobic modified cotton fabric experiment. The cotton fabric was immersed in the hydrophilic silicone oil composition prepared in the above example for 2 hours, then treated at 110° C. for 2 hours, and then the unreacted substances remaining on the cotton fabric were washed with clean water and ethanol. Figure 3 The contact angle of the cotton fabric after washing shows that the originally absorbent cotton fabric becomes hydrophobic, which illustrates the hydrophobicity and reactivity of the hydrophilic silicone oil.

[0094] Figure 4 Figure 3 shows the morphological characterization and elemental analysis of hydrophilic silicone oil modified cotton fabric. The surface of the cotton fabric is covered with silicon elements, which further proves that the hydrophilic silicone oil is chemically bonded to the cotton fabric.

[0095] Table 1 presents the water contact angle data of cotton fabrics treated with hydrophilic silicone oil in various embodiments. It can be found that the treatment with hydrophilic silicone oil greatly improves the hydrophobicity of cotton fabrics, thereby proving the hydrophobicity and reactivity of the hydrophilic silicone oil.

[0096] Table 1: Water contact angle of cotton fabric treated with hydrophilic silicone oil composition

[0097] sample Water contact angle Blank cotton fabric Water absorption, unable to measure contact angle Example 1 140° Example 2 142° Example 3 139° Example 4 141° Example 5 135° Example 6 136° Example 7 137° Example 8 136° Example 9 134° Example 10 133°

[0098] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a hydrophilic silicone oil composition, characterized in that: At least the following steps are included: S1: dissolving polyethyleneimine in water to obtain a polyethyleneimine aqueous solution; S2: mixing a reaction catalyst, a diorganopolysiloxane containing a reactive functional group and the above-mentioned polyethyleneimine aqueous solution; The mass ratio of the polyethyleneimine to water is 1:9-7:3, the mass ratio of the diorganopolysiloxane containing reactive functional groups to the polyethyleneimine is 0.0001-2, and the mass ratio of the reaction catalyst to the polyethyleneimine is 0-0.4; The polyethyleneimine comprises at least one of linear polyethyleneimine and branched polyethyleneimine; The reaction catalyst includes an acid-base regulator and an alcohol regulator; The acid-base regulator includes at least one or more of acetic acid, ammonia water, triethylamine, sodium hydroxide, sodium bicarbonate, sodium carbonate, 4-dimethylaminopyridine and pyridine; The alcohol regulator includes at least one or more of ethanol, glycerol and isopropanol; S3: Rapidly stir at room temperature for more than 6 hours to obtain the aqueous silicone oil composition.

2. The method for preparing a hydrophilic silicone oil composition according to claim 1, characterized in that: The diorganopolysiloxane containing reactive functional groups has an average structural formula of: In the formula, A comprises a reactive functional group, and the reactive functional group comprises at least one or more of an epoxy group and a carbon-carbon double bond; In the formula, R1 is at least one of an alkane group and an alkoxy group; In the formula, R2 includes at least one or more of the same substance as the reactive functional group, an alkane group and an alkoxy group.

3. A hydrophilic silicone oil composition, prepared according to the method for preparing a hydrophilic silicone oil composition according to any one of claims 1 to 2, characterized in that: The invention comprises at least the following components: polyethyleneimine, diorganopolysiloxane containing reactive functional groups, a reaction catalyst and water, wherein the mass ratio of the polyethyleneimine to water is 1:9-7:3, the mass ratio of the diorganopolysiloxane containing reactive functional groups to the polyethyleneimine is 0.0001-2, and the mass ratio of the reaction catalyst to the polyethyleneimine is 0-0.4.

Citation Information

Patent Citations

  • Preparation of block water-soluble silicon oil

    CN101497697A

  • Synthesis method of water-soluble silicone oil used for treating leather

    CN105111450A

  • Preparation method of hydrophilic amino silicon oil of comb structure

    CN109400885A

  • Preparation method of hydrophilic silicone oil

    CN112321834A

  • Preparation method of amino / epoxy co-modified hydrophilic silicone oil

    CN1927910A