A polypropylene composite film and its preparation method and application
The polypropylene composite film, with specific layer compositions and preparation methods, addresses the challenge of balancing optical, impact, and electrical insulation properties, achieving enhanced mechanical and electrical performance for packaging applications.
Patent Information
- Application Number
- CN202111221982.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-20
AI Technical Summary
Existing polypropylene films struggle to balance good optical properties, impact resistance, and electrical insulation simultaneously, often compromising on one or more of these properties due to issues with material dispersion and rheological differences in multi-layer co-extrusion methods.
A polypropylene composite film composed of layers A and B, where layer A contains polypropylene and an optional polyolefin elastomer, and layer B contains random polypropylene, a polyolefin elastomer, and a polypropylene graft derived from copolymerized polypropylene and an alkenyl-containing silane monomer, is prepared through extrusion and casting, ensuring even distribution and improved properties.
The composite film achieves high longitudinal tensile strength, low haze, excellent impact resistance, and superior electrical insulation with good heat sealing strength, meeting stringent requirements for packaging materials.
Smart Images

Figure BDA0003312942700000041 
Figure BDA0003312942700000131 
Figure BDA0003312942700000132
Abstract
Description
Technical Field
[0001] The invention belongs to the field of films, and in particular relates to a polypropylene composite film and a preparation method and application thereof. Background Art
[0002] As a simple-structured polymer plastic, polypropylene has excellent electrical insulation properties and a high melting point. Polypropylene film as an insulating film packaging material is expected to adapt to more stringent working environments. Polypropylene film can usually be produced by methods such as casting and biaxial stretching, but polypropylene film prepared from homopolymer polypropylene raw materials usually has low impact strength. To improve the impact performance of polypropylene film, block impact polypropylene can be used to prepare the film, or polyolefin elastomers can be added to polypropylene, but the films prepared by the above methods usually have a high haze. It is also possible to add a nucleating agent to the film at the same time to reduce the haze of the film by refining the crystals in the film, but this method will lead to a decrease in impact performance. At the same time, some types of nucleating agents will also reduce the electrical insulation properties of the material in high-temperature application environments.
[0003] In order to improve the impact resistance and toughness of the film, the film can also be prepared by a multi-layer co-extrusion method. For example, CN101913279A adopts a three-layer co-extrusion method to prepare a composite film. The middle layer of the film is an elastomer and PP blended in a ratio of 1:10-1:3, and the elastomer provides good impact resistance. However, this method may be difficult to disperse evenly when the elastomer content is high. In addition, in the process of multi-layer co-extrusion, the different rheological properties of the raw materials between the layers often affect the uniformity of the film, and then affect the optical and mechanical properties of the film.
[0004] Therefore, it is necessary to develop a film that combines electrical insulation, mechanical and optical properties. Summary of the invention
[0005] The purpose of the present invention is to overcome the problem that the existing polypropylene film is difficult to have good optical properties, impact resistance and electrical insulation properties at the same time, and to provide a polypropylene composite film and a preparation method thereof. The polypropylene film of the present invention has good impact resistance, optical properties, tensile properties and electrical insulation properties at the same time, and has good heat sealing strength at a relatively low heat sealing temperature.
[0006] The first aspect of the present invention provides a polypropylene composite film, which comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B, wherein the polypropylene composition A comprises polypropylene a and an optional polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, a polyolefin elastomer y and a polypropylene graft z; the polypropylene graft z comprises a structural unit derived from a copolymerized polypropylene and a structural unit derived from an alkenyl-containing silane monomer.
[0007] The second aspect of the present invention provides a method for preparing the polypropylene composite film, comprising: extruding and casting a raw material composition for forming each layer after an optional granulation process to form the composite film.
[0008] The third aspect of the present invention provides use of the polypropylene composite film in the field of packaging materials.
[0009] The polypropylene composite film prepared by the present invention has good electrical insulation performance, impact resistance, optical performance and tensile performance, and has good heat sealing strength at a relatively low heat sealing temperature. The longitudinal (MD) tensile strength of the film is ≥40MPa, preferably the longitudinal (MD) tensile strength is ≥55MPa; the film haze is ≤5.5%, preferably the film haze is ≤2.7%; the pendulum impact strength is ≥0.8J, preferably the pendulum impact strength is ≥1.8J; the heat sealing strength at 150°C is ≥17N / 15mm, preferably the heat sealing strength at 150°C is ≥20N / 15mm; the volume resistivity is ≥1.8×10 15 Ω·m, preferably volume resistivity ≥1.9×10 15 Ω·m.
[0010] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0011] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0012] The present invention provides a polypropylene composite film, which comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B, wherein the polypropylene composition A comprises polypropylene a and an optional polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, a polyolefin elastomer y and a polypropylene graft z; the polypropylene graft z comprises a structural unit derived from copolymerized polypropylene and a structural unit derived from an olefin-containing silane monomer.
[0013] According to some embodiments of the present invention, the polypropylene composite film has at least one of the following characteristics: longitudinal (MD) tensile strength ≥40MPa, preferably longitudinal (MD) tensile strength ≥55MPa; film haze ≤5.5%, preferably film haze ≤2.7%; pendulum impact strength ≥0.8J, preferably pendulum impact strength ≥1.8J; heat sealing strength at 150°C ≥17N / 15mm, preferably heat sealing strength at 150°C ≥20N / 15mm; volume resistivity ≥1.8×10 15Ω·m, preferably volume resistivity ≥1.9×10 15 Ω·m.
[0014] According to some embodiments of the present invention, the polypropylene a may be homopolypropylene and / or polypropylene graft z. Preferably, the homopolypropylene a has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity of greater than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.0. Homopolypropylene meeting the above characteristics is commercially available. For example, homopolypropylene with a grade of PPH-FA03 of Qingdao Refining and Chemical. Alternatively, it may be prepared by conventional methods in the art.
[0015] According to a preferred embodiment of the present invention, based on the weight of the polypropylene graft z, the content of the structural unit derived from the alkenyl-containing silane monomer and in the grafted state in the polypropylene graft z is 0.2-6wt%, preferably 0.2-2.5wt%.
[0016] In the present invention, the "structural unit" means that it is a part of the polypropylene graft, and its form is not limited. Specifically, the "structural unit derived from copolymerized polypropylene" refers to the product formed by copolymerized polypropylene, which includes both the "group" form and the "polymer" form. The "structural unit derived from alkenyl-containing silane monomer" refers to the product formed by alkenyl-containing silane monomer, which includes both the "group" form and the "monomer" form, and also the "polymer" form. The "structural unit" can be a repeating unit or a non-repeating independent unit.
[0017] In the present invention, the structural unit derived from the alkenyl group-containing silane-based monomer "in a grafted state" refers to the structural unit derived from the alkenyl group-containing silane-based monomer that forms a covalent bond (graft) with the copolymerized polypropylene.
[0018] In the present invention, the meaning of "comonomer" of copolymerized polypropylene is well known to those skilled in the art, and refers to a monomer copolymerized with propylene.
[0019] According to a preferred embodiment of the present invention, the polypropylene grafted product z is prepared by solid phase grafting reaction of copolymerized polypropylene and alkenyl-containing silane monomers. The grafting reaction of the present invention is a free radical polymerization reaction, therefore, the "grafted state" refers to the state in which the reactant is connected with another reactant after free radical polymerization. The connection includes both direct connection and indirect connection.
[0020] During the grafting reaction, the alkenyl-containing silane monomers can polymerize to form a certain amount of ungrafted polymers. The polypropylene grafted product z of the present invention includes both the product (crude product) directly obtained by grafting copolymerization of polypropylene and alkenyl-containing silane monomers, and the pure grafted modified polypropylene obtained by further purifying the product.
[0021] According to a preferred embodiment of the present invention, the melt mass flow rate of the polypropylene graft z at 230°C and 2.16 kg load is 0.01-30 g / 10 min, preferably 0.05-20 g / 10 min, further preferably 0.1-10 g / 10 min, and more preferably 0.2-8 g / 10 min.
[0022] The alkenyl-containing silane monomer of the present invention may be any monomeric silane compound that can be polymerized by free radicals, and may be selected from at least one of the alkenyl-containing silane monomers selected from the monomers having the structure shown in Formula I,
[0023]
[0024] Among them, R 1 C 2 -C 12 The alkenyl group is preferably a monounsaturated alkenyl group; R 2 , R 3 , R 4 are each independently selected from substituted or unsubstituted C 1 -C 12 Straight chain alkyl, substituted or unsubstituted C 3 -C 12 Branched alkyl, substituted or unsubstituted C 1 -C 12 Alkoxy, substituted or unsubstituted C 1 -C 12 Preferably, R 1 C 2 -C 6 The alkenyl group is preferably a monounsaturated alkenyl group; R 2 , R 3 , R 4 are each independently selected from substituted or unsubstituted C 1 -C 6 Straight chain alkyl, substituted or unsubstituted C 3 -C 6 Branched alkyl, substituted or unsubstituted C 1 -C 6 Alkoxy, substituted or unsubstituted C 1 -C 6 The acyloxy group.
[0025] More preferably, the alkenyl-containing silane monomer is selected from at least one of vinyltriethoxysilane, vinyltrimethoxysilane, vinyltriisopropoxysilane, vinyltri-tert-butoxysilane, vinyltriacetoxysilane, methylvinyldimethoxysilane, ethylvinyldiethoxysilane, allyltriethoxysilane, allyltrimethoxysilane, allyltriisopropoxysilane, vinyltri(β-methoxyethoxy)silane, allyltri(β-methoxyethoxy)silane, allyltri-tert-butoxysilane, allyltriacetoxysilane, methylallyldimethoxysilane and ethylallyldiethoxysilane.
[0026] According to the present invention, the copolymerized polypropylene is a propylene copolymer containing ethylene or a higher α-olefin or a mixture thereof. Specifically, the comonomer of the copolymerized polypropylene is selected from C 2 -C 8 At least one of the α-olefins of 2 -C 8 The α-olefins include but are not limited to at least one of ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene and 1-octene, preferably ethylene and / or 1-butene. Further preferably, the copolymerized polypropylene consists of propylene and ethylene.
[0027] According to the present invention, in addition to the above-mentioned composition characteristics, the copolymerized polypropylene also has at least one of the following characteristics: a comonomer content of 0.5-30 mol%, preferably 4-25 mol%; a xylene soluble content of 2-80 wt%, preferably 18-75 wt%, and more preferably 30-70 wt%; a comonomer content in the solubles of 10-70 wt%, preferably 10-50 wt%, and more preferably 20-35 wt%; a ratio of the intrinsic viscosity of the solubles to the polypropylene of 0.3-5, preferably 0.5-3, and more preferably 0.8-1.3; a melt mass flow rate at 230°C and a load of 2.16 kg of 0.01-60 g / 10 min, preferably 0.05-35 g / 10 min, and more preferably 0.5-15 g / 10 min; a melting temperature Tm of 100°C or more, preferably 110-180°C, and more preferably 120-170°C; a weight average molecular weight of 20×10 4 -60×10 4 g / mol.
[0028] The copolymerized polypropylene of the present invention can be any commercially available polypropylene powder suitable for the present invention, or can be produced by a common polymerization process described in the literature, for example, by the methods described in CN101679557A and CN101058654A.
[0029] The polypropylene grafted product z of the present invention can be prepared by a method comprising the following steps: in the presence of an inert gas, a reaction mixture comprising copolymerized polypropylene and an alkenyl-containing silane monomer is subjected to a solid phase grafting reaction to obtain the polypropylene grafted product.
[0030] The solid phase grafting reaction of the present invention can be carried out by referring to various conventional methods in the art, such as forming active grafting sites on copolymerized polypropylene in the presence of grafting monomers, or first forming active grafting sites on copolymerized polypropylene and then treating with grafting monomers. The grafting sites can be formed by treating with free radical initiators, or by high energy ionizing radiation or microwave treatment. Free radicals generated in the polymer as a result of chemical or radiation treatment form grafting sites on the polymer and initiate polymerization of monomers at these sites.
[0031] Preferably, the grafting point is initiated by a free radical initiator and the grafting reaction is further carried out. In this case, the reaction mixture also includes a free radical initiator; further preferably, the free radical initiator is selected from a peroxide free radical initiator and / or an azo free radical initiator.
[0032] Among them, the peroxide free radical initiator is preferably selected from at least one of dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, lauroyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate, tert-butyl peroxy (2-ethylhexanoate) and dicyclohexyl peroxydicarbonate; the azo free radical initiator is preferably azobisisobutyronitrile and / or azobisisoheptylnitrile.
[0033] More preferably, the grafting point is initiated by a peroxide-based free radical initiator and the grafting reaction is further carried out.
[0034] In addition, the grafting reaction of the present invention can also be carried out by the methods described in CN106543369A, CN104499281A, CN102108112A, CN109251270A, CN1884326A and CN101492517B.
[0035] Under the premise of meeting the above product characteristics, the present invention has no particular limitation on the amount of each component used in the grafting reaction. Specifically, the mass ratio of the free radical initiator to the alkenyl-containing silane monomer can be 0.1-10:100, preferably 0.5-6:100. The mass ratio of the alkenyl-containing silane monomer to the copolymerized polypropylene is 0.5-12:100, preferably 0.8-9:100, and more preferably 1-6:100.
[0036] The process conditions of the grafting reaction are not particularly limited in the present invention. Specifically, the temperature of the grafting reaction may be 30-130° C., preferably 60-120° C.; and the time may be 0.5-10 h, preferably 1-5 h.
[0037] In the present invention, the "reaction mixture" includes all materials added to the grafting reaction system. The materials can be added at once or at different stages of the reaction.
[0038] The reaction mixture of the present invention may further include a dispersant, which is preferably water or an aqueous solution of sodium chloride. The mass amount of the dispersant is preferably 50-300% of the mass of the copolymerized polypropylene.
[0039] The reaction mixture of the present invention may further include an interfacial agent, which is an organic solvent having a swelling effect on polyolefins, preferably at least one of the following organic solvents having a swelling effect on copolymerized polypropylene: ether solvents, ketone solvents, aromatic hydrocarbon solvents, and alkane solvents; more preferably at least one of the following organic solvents: chlorobenzene, polychlorinated benzene, C 6 Alkanes or cycloalkanes, benzene, C 1 -C 4 Alkyl substituted benzene, C 2 -C 6 Fatty ether, C 3 -C 6 Fatty ketones, decahydronaphthalene; more preferably at least one of the following organic solvents: benzene, toluene, xylene, chlorobenzene, tetrahydrofuran, ether, acetone, hexane, cyclohexane, decahydronaphthalene, heptane. The mass content of the interface agent is preferably 1-30% of the mass of the copolymerized polypropylene, and more preferably 10-25%.
[0040] The reaction mixture of the present invention may further include an organic solvent as a solvent for dissolving the solid free radical initiator, and the organic solvent preferably includes C 2 -C 5 Alcohols, C 2 -C 4 Ethers and C 3 -C 5 At least one of ketones, more preferably including C 2 -C 4 Alcohols, C 2 -C 3 Ethers and C 3 -C 5 At least one of ketones, most preferably at least one of ethanol, ether and acetone. The mass content of the organic solvent is preferably 1-35% of the mass of the copolymerized polypropylene.
[0041] As described above, the polypropylene grafted product z of the present invention includes both the product (crude product) directly obtained by grafting reaction of copolymerized polypropylene and grafted monomer, and the pure grafted modified polypropylene obtained by further purifying the product. Therefore, the preparation method of the present invention may optionally include a step of purifying the crude product. The purification may be carried out by various conventional methods in the art, such as extraction.
[0042] The present invention has no particular limitation on the grafting efficiency of the grafting reaction, but a higher grafting efficiency is more conducive to obtaining a polypropylene graft with desired properties through a one-step grafting reaction. Therefore, the grafting efficiency of the grafting reaction is preferably controlled to be 5-100%, and more preferably 5-60%. The concept of the grafting efficiency is well known to those skilled in the art, and refers to the amount of grafted monomers grafted / the total amount of grafted monomers fed into the reaction.
[0043] The inert gas of the present invention can be any inert gas commonly used in the art, including but not limited to nitrogen and argon.
[0044] According to some embodiments of the present invention, the polyolefin elastomer b is an elastomeric copolymer of ethylene and an alpha olefin, wherein the alpha olefin is preferably C 3 -C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.
[0045] According to some embodiments of the present invention, the polyolefin elastomer y is an elastomeric copolymer of ethylene and an alpha olefin, wherein the alpha olefin is preferably C 3 -C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.
[0046] The polyolefin elastomers meeting the above characteristics are commercially available, for example, polyolefin elastomers with the trademark of Exxon 6102, polyolefin elastomers with the trademark of Mitsui & Co., Ltd., and polyolefin elastomers with the trademark of Exxon EXACT 3139. Alternatively, they can be prepared by conventional methods in the art.
[0047] According to some embodiments of the present invention, the random polypropylene x is a copolymer of propylene and ethylene and / or butene, that is, at least one of a copolymer of propylene and ethylene, a copolymer of propylene and butene, and a copolymer of propylene and ethylene and butene, preferably selected from at least one of an ethylene-propylene-butene terpolymer, a propylene-ethylene binary random copolymer, and a propylene-butene binary random copolymer.
[0048] The melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is preferably 2-10 g / 10 min.
[0049] Random polypropylenes meeting the above characteristics are commercially available, such as Yanshan Petrochemical's F5006 random polypropylene, Shanghai Petrochemical's F500EPS random polypropylene, and Shanghai Petrochemical's F800EPS random polypropylene. Alternatively, they can be prepared by conventional methods in the art.
[0050] According to some embodiments of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-100 wt % of the polypropylene a and 0-50 wt % of the polyolefin elastomer b.
[0051] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 75-95 wt% of polypropylene a and 5-25 wt% of polyolefin elastomer b.
[0052] The elastomer or polypropylene graft in the composition contains a rubber phase, which provides good impact performance for the film. At the same time, since the macromolecular chain segments of the homopolymer phase of homopolypropylene are relatively regular, crystallization and orientation occur during the film preparation process, providing good mechanical properties for the film. According to the research of the inventors, according to the composition provided by the present invention, the rubber phase can be evenly distributed in the film, and the size of the rubber phase can meet the requirements of the refractive index, so a film with good optical properties can be obtained, so that the film has good impact performance and optical properties at the same time; at the same time, under this ratio, the film has good mechanical properties. The electrical insulation performance of the polypropylene graft is significantly improved due to the grafting modification, and it has excellent electrical insulation characteristics. With different processing aids, the film can have excellent electrical insulation or antistatic properties.
[0053] According to some embodiments of the present invention, based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 50-90 wt% of random polypropylene x, 5-40 wt% of polyolefin elastomer y and 2-40 wt% of polypropylene graft z.
[0054] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 60-85 wt% of random polypropylene x, 5-20 wt% of polyolefin elastomer y and 5-20 wt% of polypropylene graft z.
[0055] According to the research of the present inventors, when the polypropylene composition B adopts this ratio and the surface layer in the composite film is made of the polypropylene composition B, the impact resistance of the film can be greatly improved, and the optical properties can be further improved, and the film can also have good heat sealing properties.
[0056] According to some embodiments of the present invention, based on the total weight of the polypropylene composition A as 100 parts by weight, the weight of the polyolefin elastomer b is calculated as Wb, based on the total weight of the polypropylene composition B as 100 parts by weight, the weight of the polyolefin elastomer y is calculated as Wy, and the ratio of Wb to Wy is 6:1-1:4, for example, it can be 5.5:1, 5:1, 4.5:1, 4:1, 3.5:1, 3:1, 2.5:1, 2:1, 1.5:1, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5 and any value therebetween.
[0057] According to a preferred embodiment of the present invention, the ratio of Wb to Wy is 4:1-1:4.
[0058] According to the research conducted by the present inventors, when a double-layer or multi-layer film is co-extruded, when the ratio of Wb to Wy is within the range described in the present invention, the impact resistance and optical properties of the film can be further improved, and at the same time the extrusion process will be smoother.
[0059] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-10 g / 10 min, preferably 3-8 g / 10 min.
[0060] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 3-10 g / 10 min, preferably 4-8 g / 10 min.
[0061] When the melt mass flow rates of the polypropylene composition A and the polypropylene composition B are within the above range, the film preparation process can be made smoother, thereby ensuring that the film has better uniformity, mechanical properties and optical properties.
[0062] The composite film of the present invention may be a double-layer structure, or a three-layer or more film layer structure, and the other layers may have the same composition as the film layer A or the film layer B, or may have different compositions from the film layer A or the film layer B, or may be a mixture of a polypropylene composition A and a polypropylene composition B. When the polypropylene composite film has a structure of three or more layers, the film layer B is preferably used as a surface layer, such as a three-layer film including a film layer A, a film layer B, and a film layer C, and the B layer and the C layer may be located on both sides of the A layer, respectively.
[0063] According to some embodiments of the present invention, in the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-2:1, for example, it can be 1:4, 1:3.5, 1:3, 1:2.5, 1:2, 1:1.5, 1:1, 1.5:1, 2:1 and any value therebetween.
[0064] According to a preferred embodiment of the present invention, in the polypropylene composite film, the ratio of the sum of the thickness of other film layers to the thickness of the film layer A is 1:2-1:1. Under this ratio, the composite film has good mechanical properties.
[0065] In the present invention, in order to improve the performance of the composite film during processing, the composite film preferably further contains an antioxidant and / or a lubricant.
[0066] In the present invention, the antioxidant may be any antioxidant commonly used in the art, without particular limitation. For example, it may be antioxidant 1076, antioxidant 1010, antioxidant 168, thioester antioxidants (such as DLTP, DSTP), etc. Based on the total amount of the polypropylene composition A or the polypropylene composition B as 100 parts by weight, the content of the antioxidant may be 0.1-0.8 parts by weight, preferably 0.2-0.4 parts by weight.
[0067] In the present invention, the lubricant is preferably a PEG lubricant and / or a monoglyceride lubricant. Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight, preferably 0.05-0.2 parts by weight.
[0068] According to the present invention, in order to improve other properties of the composite film (such as stability, antistatic property, etc.), the composite film preferably further contains a film-forming aid. The film-forming aid can be selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a filler, a lubricant, an anti-adhesive agent (anti-adhesive agent) and an antistatic agent. The specific type of the film-forming aid can be a conventional choice in the art, and the present invention is not particularly limited thereto.
[0069] In the present invention, based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid may be 0.01-0.5 parts by weight, preferably 0.05-0.3 parts by weight.
[0070] The present invention also provides a method for preparing the polypropylene composite film, comprising: extruding and casting the raw material composition for forming each layer after an optional granulation process to form the composite film.
[0071] In the preparation method of the present invention, the pelletizing process can generally include: uniformly mixing the components of the polypropylene composition and the optional antioxidant, lubricant and film-forming aid in a high-speed mixer, adding the uniformly mixed materials to a twin-screw extruder for melt mixing and uniform extrusion pelletization, and drying to obtain pellets. The processing temperature of the twin-screw extruder can be controlled to be 170-230°C.
[0072] According to some embodiments of the present invention, the pellets can be processed by extrusion casting. The process of the extrusion casting method may include sending the pellets of different compositions to multiple extruders respectively, and after the pellets are co-extruded and composited through the extruder die, they are sequentially passed through a casting roller, a traction roller, and then trimmed and rolled to obtain the composite film. Among them, the temperature of the extrusion casting can be controlled to 170-230°C, and the temperature of the casting roller can be 10-50°C. The specific process of preparing the film by the extrusion casting method is a commonly used choice in the art and will not be repeated here.
[0073] The obtained composite film can be stretched in a subsequent process, such as biaxial stretching, which can further improve the mechanical properties of the composite film.
[0074] According to one embodiment of the present invention, the polypropylene composition A and the polypropylene composition B are pelletized, extruded and cast, and optionally stretched to obtain the polypropylene composite film.
[0075] The polypropylene composite film of the present invention can be used in the field of packaging materials, such as in the field of high-end packaging that has high requirements for film impact resistance, optical properties and electrical insulation properties, including but not limited to battery packaging, electronic product packaging or food, especially high-end food packaging.
[0076] The specific embodiments of the present invention are described in detail below by way of examples. It should be understood that the examples described below are only used to illustrate and explain the present invention and are not used to limit the present invention.
[0077] In the following examples and comparative examples:
[0078] The film casting equipment was purchased from Swedish Labtech Company, model LCR400.
[0079] The polypropylene composition and film properties were tested according to the following method, and the film test results are shown in Table 1:
[0080] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, wherein the test temperature is 230°C and the load is 2.16 kg.
[0081] (2) Film tensile strength: measured according to the method specified in GB / T 1040.3-2006.
[0082] (3) Film pendulum impact strength: measured according to the method specified in GB / T 8809-2015.
[0083] (4) Film haze: measured according to the method specified in GB / T 2410-2008.
[0084] (5) Film heat seal strength: Measured according to the method specified in QB / T 2358. When preparing the sample, the heat seal temperature is 150°C, the heat seal pressure is 0.2 MPa, and the heat seal time is 3 s.
[0085] (6) Comonomer content in copolymerized polypropylene: The comonomer content was determined by quantitative Fourier transform infrared (FTIR) spectroscopy. The correlation of the determined comonomer content was calibrated by quantitative nuclear magnetic resonance (NMR) spectroscopy. 13 The calibration method of the results obtained by C-NMR spectrum was carried out according to the conventional method in the art.
[0086] (7) Xylene soluble content in copolymerized polypropylene, comonomer content in soluble matter, and intrinsic viscosity ratio of soluble matter to copolymerized polypropylene: Tested using the CRYST-EX instrument from Polymer Char. Trichlorobenzene solvent was used, the temperature was raised to 150°C for dissolution, the temperature was kept constant for 90 minutes, and a sample was taken for testing. The temperature was then lowered to 35°C, the temperature was kept constant for 70 minutes, and a sample was taken for testing.
[0087] (8) Weight average molecular weight of copolymerized polypropylene: Determined by high temperature GPC, using PL-GPC 220 gel permeation chromatograph from Polymer Laboratory, the sample was dissolved in 1,2,4-trichlorobenzene at a concentration of 1.0 mg / ml. The test temperature was 150°C and the solution flow rate was 1.0 ml / min. The molecular weight of polystyrene was used as an internal reference to develop a standard curve, and the molecular weight and molecular weight distribution of the sample were calculated based on the elution time.
[0088] (9) Melting temperature Tm: Differential scanning calorimetry is used to analyze the melting and crystallization processes of the material. The specific operation is: Under nitrogen protection, 5-10 mg of sample is measured from 20°C to 200°C using a three-stage temperature rise and fall measurement method. The change in heat flow reflects the melting and crystallization process of the material, and the melting temperature Tm is calculated.
[0089] (10) Grafting efficiency GE, parameter M1: 2-4 g of the grafted product was placed in a Soxhlet extractor and extracted with acetone for 24 h to remove unreacted monomers and homopolymers to obtain a pure grafted product. The product was dried and weighed to calculate the parameter M1 and grafting efficiency GE.
[0090] The parameter M1 represents the content of the structural unit derived from the alkenyl-containing silane monomer in the polypropylene graft z. In the present invention, the calculation formulas of M1 and GE are as follows:
[0091]
[0092]
[0093] In the above formula, w 0 is the mass of the PP matrix; w 1 is the mass of the grafted product before extraction; w 2 is the mass of the grafted product after extraction; w 3 It is the mass of added olefin-containing silane monomer.
[0094] (11) Volume resistivity: measured according to the method specified in GB / T 1410-2006.
[0095] (12) Isoregularity: Pass 13 C NMR measurement: The nuclear magnetic resonance spectrometer (NMR) of 400 MHz propylene polymer was measured using the AVANCE III nuclear magnetic resonance spectrometer (NMR) of Bruker Company, Switzerland. 13 C-NMR), where the solvent is deuterated o-dichlorobenzene and the sample concentration is 250 mg sample / 2.5 mL solvent. To prevent oxidative degradation of the sample during dissolution and data collection, 2 mg of 2,6-di-tert-butyl-4-methylphenol antioxidant (BHT) was added to the sample. The sample was dissolved at 140°C and collected. 13 C-NMR, test temperature 125°C, probe size 10 mm, 90° pulse, sampling time AQ 5 s, delay time D1 1 s, scan number 6000 times. The content of diad isotacticity [mm] is taken as the isotacticity.
[0096] (13) Molecular weight distribution (Mw / Mn): Determined by gel permeation chromatography (GPC), using a PL-GPC 220 gel permeation chromatograph produced by Polymer Laboratories, UK, in combination with an IR5 infrared detector. The chromatographic column in the gel permeation chromatograph consisted of three Plgel 10 μm MIXED-B columns connected in series. The solvent and mobile phase were both 1,2,4-trichlorobenzene (containing 0.3 g / 1000 mL of the antioxidant 2,6-di-tert-butyl-p-cresol). The column temperature was 150 °C, and the flow rate was 1.0 mL / min. EasiCal PS-1 narrow distribution polystyrene standard produced by PL was used for universal calibration.
[0097] Preparation Example 1
[0098] The basic copolymer polypropylene powder with the following characteristics was selected: the ethylene content of the comonomer was 18.1wt%, the xylene soluble content was 48.7wt%, the comonomer content in the solubles was 31.9wt%, the soluble / copolymer polypropylene intrinsic viscosity ratio was 0.89, and the weight average molecular weight was 34.3×10 4g / mol, MFR at 230℃ and 2.16kg load is 1.21g / 10min, Tm=143.4℃, sieve to remove fine powder less than 40 mesh. Weigh 2.0kg of the above basic copolymer polypropylene powder, add it to a 10L reactor with mechanical stirring, close the reaction system, and replace with nitrogen for deoxygenation. Add 2.5g of lauroyl peroxide and 50g of vinyltriethoxysilane, stir and mix for 30min, swell at 40℃ for 1 hour, heat to 90℃, and react for 4 hours. After the reaction is completed, nitrogen is purged and cooled to obtain polypropylene-g-vinyltriethoxysilane C1, whose melt mass flow rate is 1.15g / 10min, M1 is 1.03%, and grafting efficiency is 42%.
[0099] Preparation Example 2
[0100] The basic copolymer polypropylene powder with the following characteristics was selected: 4.8wt% ethylene content of the comonomer, 19.2wt% xylene soluble content, 17.6wt% comonomer content in the solubles, 1.04 soluble / copolymer polypropylene intrinsic viscosity ratio, and a weight average molecular weight of 29.2×10 4 g / mol, MFR at 230℃ and 2.16kg load is 5.37g / 10min, Tm=163.3℃, sieve to remove fine powder less than 40 mesh. Weigh 2.0kg of the above basic copolymerized polypropylene powder, add it to a 10L reactor with mechanical stirring, close the reaction system, and replace with nitrogen for deoxygenation. Dissolve 3.7g of lauroyl peroxide in 70g of acetone, add the resulting acetone solution to the reaction system, heat to 40℃, purge with nitrogen for 30min to remove acetone, then add 75g of vinyl triethoxysilane, stir and mix for 30min, heat to 85℃, and react for 4 hours. After the reaction is completed, purge with nitrogen, cool and cool to obtain polypropylene-g-vinyl triethoxysilane C2, whose melt mass flow rate is 4.77g / 10min, M1 is 1.24%, and grafting efficiency is 34%.
[0101] Preparation Example 3
[0102] The basic copolymer polypropylene powder with the following characteristics was selected: ethylene content of comonomer 9.3wt%, xylene soluble content 21.0wt%, comonomer content in soluble matter 35.4wt%, soluble matter / copolymer polypropylene intrinsic viscosity ratio 1.68, weight average molecular weight 30.4×10 4g / mol, MFR at 230°C and 2.16kg load is 5.69g / 10min, Tm=163.0°C, and fine powder less than 40 mesh is removed by sieving. Weigh 2.0kg of the above-mentioned basic copolymer polypropylene powder, add it to a 10L reactor with mechanical stirring, close the reaction system, and replace with nitrogen for deoxygenation. Add 4.5g of tert-butyl peroxide (2-ethylhexanoate) and 120g of vinyl triisopropoxy silane, stir and mix for 60min, heat to 100°C, and react for 1.5 hours. After the reaction is completed, nitrogen is purged and cooled to obtain polypropylene-g-vinyl triisopropoxy silane C3, whose melt mass flow rate is 8.51g / 10min, M1 is 2.11%, and the grafting efficiency is 37%.
[0103] Preparation Example 4
[0104] The basic copolymer polypropylene powder with the following characteristics was selected: the ethylene content of the comonomer was 12.6 wt%, the xylene soluble content was 30.6 wt%, the comonomer content in the solubles was 43.6 wt%, the soluble / copolymer polypropylene intrinsic viscosity ratio was 1.84, and the weight average molecular weight was 27.1×10 4 g / mol, MFR at 230℃ and 2.16kg load is 8.46g / 10min, Tm=162.0℃, sieve to remove fine powder less than 40 mesh. Weigh 2.0kg of the above basic copolymer polypropylene powder, add it to a 10L reactor with mechanical stirring, close the reaction system, and replace with nitrogen for deoxygenation. Dissolve 5.0g of lauroyl peroxide in 100g of vinyltrimethoxysilane and 50g of toluene as an interface agent to form a solution, stir and mix the solution for 30min, heat to 95℃, add 4kg of dispersant water at 95℃, and react for 0.75 hours. After the reaction is completed, cool and filter to remove the dispersant water, vacuum dry at 70℃ for 10 hours to obtain polypropylene-g-vinyltrimethoxysilane C4, whose melt mass flow rate is 8.31g / 10min, M1 is 1.42%, and grafting efficiency is 29%.
[0105] Example 1
[0106] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0107] (1) Preparation of polypropylene composition A:
[0108] Component a is homopolypropylene with the brand name PPH-FA03, purchased from Qingdao Refining and Chemical, with a melt mass flow rate of 3.1 g / 10 min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.7; component b is polyolefin elastomer with the brand name 6102, purchased from Exxon, and is an ethylene-propylene copolymer with an ethylene structural unit content of 16 wt%. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the masses of the above-mentioned component a and component b being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain pellets of a polypropylene composition A. The melt mass flow rate MFR thereof is tested. A =3.5g / 10min.
[0109] (2) Preparation of polypropylene composition B:
[0110] Component x is a random polypropylene with the brand name F5006, purchased from Yanshan Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.2g / 10min; component y is a polyolefin elastomer with the brand name 6102, purchased from Exxon, which is an ethylene-propylene copolymer with an ethylene structural unit content of 16wt%; component z is polypropylene-g-vinyltriethoxysilane C2. The above-prepared components are weighed and mixed according to the ratio, wherein the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 5 parts by weight, and the mass fraction Wz of component z is 10 parts by weight. Wb:Wy is 4:1. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR B =4.68g / 10min.
[0111] (3) Preparation of composite films:
[0112] The polypropylene composition A and polypropylene composition B pellets obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition B is added to the upper surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is added to the upper surface layer extruder, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is wound to form a composite film, which is composed of an upper surface layer (film layer B) and a core layer (film layer A). The film thickness is 50μm, wherein the thickness ratio of the film layer B to the film layer A is 1:2.
[0113] Example 2
[0114] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0115] (1) Preparation of polypropylene composition A:
[0116] Component a is polypropylene-g-vinyltriethoxysilane C1; component b is a polyolefin elastomer with a brand name of DF640, purchased from Mitsui Co., Ltd., which is an ethylene-1-butene copolymer with a butene structural unit content of 32wt%. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 95 parts by weight, and the mass fraction Wb of component b is 5 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the masses of the above-mentioned component a and component b being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain pellets of a polypropylene composition A. The melt mass flow rate MFR thereof is tested. A =4.73g / 10min.
[0117] (2) Preparation of polypropylene composition B:
[0118] Component x is a random polypropylene with the brand name F500EPS, purchased from Shanghai Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.3g / 10min; component y is a polyolefin elastomer with the brand name DF640, purchased from Mitsui Company, which is an ethylene-1-butene copolymer with a butene structural unit content of 32wt%; component z is polypropylene-g-vinyltriethoxysilane C1. The above-prepared components are weighed and mixed according to the ratio, wherein the mass fraction Wx of component x is 60 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the mass fraction Wz of component z is 20 parts by weight. Wb:Wy is 1:4. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. After testing, its melt mass flow rate MFR B =4.85g / 10min.
[0119] (3) Preparation of composite films:
[0120] The polypropylene composition A and polypropylene composition B pellets obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition B is added to the upper surface layer extruder and the lower surface layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is added to the upper and lower surface layer extruders, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is rolled up to form a composite film, which is composed of upper and lower surface layers (film layer B) and a core layer (film layer A). The film thickness is 50μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers to the thickness of the core layer is 1:1.
[0121] Example 3
[0122] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0123] (1) Preparation of polypropylene composition A:
[0124] Component a is polypropylene-g-vinyl triisopropoxysilane C3; component b is a polyolefin elastomer with the grade of EXACT3139, purchased from Exxon, which is an ethylene-1-octene copolymer with an octene structural unit content of 14wt%. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 85 parts by weight, and the mass fraction Wb of component b is 15 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the masses of the above-mentioned component a and component b being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain pellets of a polypropylene composition A. The melt mass flow rate MFR thereof is tested. A =9.18g / 10min.
[0125] (2) Preparation of polypropylene composition B:
[0126] Component x is a random polypropylene with the brand name F800EPS, purchased from Shanghai Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 8.2g / 10min; component y is a polyolefin elastomer with the brand name EXACT3139, purchased from Exxon, which is an ethylene-1-octene copolymer with an octene structural unit content of 14wt%; component z is polypropylene-g-vinyltriisopropoxysilane C3. The above-prepared components are weighed and mixed according to the ratio, wherein the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 10 parts by weight, and the mass fraction Wz of component z is 5 parts by weight. Wb:Wy is 3:2. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR B =8.70g / 10min.
[0127] (3) Preparation of composite films:
[0128] The preparation process is the same as step (3) of Example 1.
[0129] Example 4
[0130] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0131] (1) Preparation of polypropylene composition A:
[0132] The steps are the same as those in Example 1. The difference is that the mass fraction Wa of component a is 70 parts by weight, and the mass fraction Wb of component b is 30 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR is tested. A =3.2g / 10min.
[0133] (2) Preparation of polypropylene composition B:
[0134] The steps are the same as those in Example 1. The difference is that the mass fraction Wx of component x is 90 parts by weight, the mass fraction Wy of component y is 5 parts by weight, and the mass fraction Wz of component z is 5 parts by weight. Wb:Wy is 6:1. The other steps are the same as those in step (1), and finally a pellet of polypropylene composition B is obtained. The melt mass flow rate MFR thereof is tested. B =4.89g / 10min.
[0135] (3) Preparation of composite films:
[0136] The steps are the same as those in Example 1. The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 1:3.
[0137] Example 5
[0138] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0139] (1) Preparation of polypropylene composition A:
[0140] The steps are the same as those in Example 3, except that the mass fraction Wa of component a is 75 parts by weight, and the mass fraction Wb of component b is 25 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR is tested. A =9.63g / 10min.
[0141] (2) Preparation of polypropylene composition B:
[0142] The steps are the same as those in Example 3, except that the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 13 parts by weight, and the mass fraction Wz of component z is 2 parts by weight. Wb:Wy is 25:13. Finally, pellets of polypropylene composition B are obtained, and the melt mass flow rate MFR thereof is tested. B =8.83g / 10min.
[0143] (3) Preparation of composite films:
[0144] The steps are the same as those in Example 2. The film thickness is 50 μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers to the thickness of the core layer is 2:1.
[0145] Example 6
[0146] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0147] (1) Preparation of polypropylene composition A:
[0148] The steps are the same as those in Example 3, except that the mass fraction Wa of component a is 100 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR thereof is measured. A =8.94g / 10min.
[0149] (2) Preparation of polypropylene composition B:
[0150] The steps are the same as those in Example 3, except that the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 30 parts by weight, and the mass fraction Wz of component z is 20 parts by weight. Finally, pellets of polypropylene composition B are obtained, and the melt mass flow rate MFR thereof is tested. B =9.70g / 10min.
[0151] (3) Preparation of composite films:
[0152] The steps are the same as those in Example 3. The film thickness is 50 μm, wherein the ratio of the sum of the thickness of the upper surface layer to the thickness of the core layer is 1:4.
[0153] Example 7
[0154] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.
[0155] (1) Preparation of polypropylene composition A:
[0156] The steps are the same as those in Example 1. The difference is that the mass fraction Wa of component a is 100 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR thereof is measured. A =3.1g / 10min.
[0157] (2) Preparation of polypropylene composition B:
[0158] The steps are the same as those in Example 1. The difference is that the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the mass fraction Wz of component z is 30 parts by weight. The other steps are the same as those in step (1), and finally a pellet of polypropylene composition B is obtained. The melt mass flow rate MFR B =3.55g / 10min.
[0159] (3) Preparation of composite films:
[0160] The steps are the same as those in Example 1. The film thickness is 50 μm, wherein the thickness ratio of the film layer B to the film layer A is 1:3.
[0161] Example 8
[0162] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of the polypropylene composition A, the mass fraction Wa of component a is 100 parts by weight. Finally, the polypropylene composition A pellets were obtained, and the melt mass flow rate MFR A =3.1g / 10min.
[0163] Example 9
[0164] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of the polypropylene composition A, the mass fraction Wa of component a is 50 parts by weight, and the mass fraction Wb of component b is 50 parts by weight. Wb:Wy is 10:1. Finally, the polypropylene composition A pellets were obtained, and the melt mass flow rate MFR A =3.5g / 10min.
[0165] Example 10
[0166] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 40 parts by weight, the mass fraction Wy of component y is 30 parts by weight, and the mass fraction Wz of component z is 30 parts by weight. Wb:Wy is 2:3. The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR thereof was tested. B =3.33g / 10min.
[0167] Embodiment 11
[0168] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 40 parts by weight, and the mass fraction Wz of component z is 10 parts by weight. Wb:Wy is 1:2. The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR thereof was tested. B =3.92g / 10min.
[0169] Example 12
[0170] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 50 parts by weight, the mass fraction Wy of component y is 10 parts by weight, and the mass fraction Wz of component z is 40 parts by weight. Wb:Wy is 2:1. The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR thereof was tested. B =3.36g / 10min.
[0171] Example 13
[0172] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 99 parts by weight, and the mass fraction Wb of component b is 1 part by weight. Wb:Wy is 1:5. Finally, pellets of polypropylene composition A were obtained, and the melt mass flow rate MFR was tested. A =3.2g / 10min.
[0173] Embodiment 14
[0174] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 97.5 parts by weight, and the mass fraction Wb of component b is 2.5 parts by weight. Wb:Wy is 1:2. Finally, pellets of polypropylene composition A were obtained, and the melt mass flow rate MFR was tested. A =3.1g / 10min.
[0175] Embodiment 15
[0176] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 95 parts by weight, and the mass fraction Wb of component b is 5 parts by weight. Wb:Wy is 1:1. Finally, pellets of polypropylene composition A were obtained, and the melt mass flow rate MFR A =3.2g / 10min.
[0177] Example 16
[0178] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 90 parts by weight, and the mass fraction Wb of component b is 10 parts by weight. Wb:Wy is 2:1. Finally, pellets of polypropylene composition A were obtained, and the melt mass flow rate MFR was tested. A =3.3g / 10min; In the preparation of polypropylene composition B, component z is polypropylene-g-vinyltrimethoxysilane C4, and the polypropylene composition B pellets are obtained, and the melt mass flow rate MFR is detected B =5.40g / 10min.
[0179] Embodiment 17
[0180] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition A, the mass fraction Wa of component a is 75 parts by weight, and the mass fraction Wb of component b is 25 parts by weight. Wb:Wy is 5:1. Finally, pellets of polypropylene composition A were obtained, and the melt mass flow rate MFR was tested. A =3.1g / 10min.
[0181] Comparative Example 1
[0182] A polypropylene composite film was prepared according to the method of Example 1. The difference was that only the polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 50 μm.
[0183] Comparative Example 2
[0184] A polypropylene composite film was prepared according to the method of Example 2. The difference was that only the polypropylene composition B was used for extrusion casting into a single-layer film with a thickness of 50 μm.
[0185] Comparative Example 3
[0186] A polypropylene composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition B contained only component x.
[0187] Comparative Example 4
[0188] A polypropylene composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition B contained only component x and component y, wherein the mass fraction Wx of component x was 85 parts by weight, and the mass fraction Wy of component y was 15 parts by weight.
[0189] Comparative Example 5
[0190] A polypropylene composite film was prepared according to the method of Example 2. The difference was that the polypropylene composition B only contained component x and component z, wherein the mass fraction Wx of component x was 70 parts by weight, and the mass fraction Wz of component z was 30 parts by weight.
[0191] Table 1
[0192]
[0193]
[0194] From the results of the examples in Table 1, it can be concluded that the polypropylene composite film of the present invention has good impact resistance, optical properties and tensile properties, and has good heat sealing strength. The longitudinal tensile strength (MD) of the film of the present invention is ≥40MPa, the film haze is ≤5.5%, the pendulum impact strength is ≥0.8J, and the heat sealing strength at 150°C is ≥17N / 15mm, and the volume resistivity is ≥1.8×10 15Ω·m. It can be seen from the preferred embodiment that the longitudinal (MD) tensile strength of the film is ≥55MPa, the film haze is ≤2.7%, the pendulum impact strength is ≥1.8J, the heat sealing strength at 150°C is ≥20N / 15mm, and the volume resistivity is ≥1.9×10 15 Ω·m. From the comparative examples, it can be seen that it is difficult to achieve a balance of various properties by only using a single-layer film or changing the composition ratio of the film layer, and during extrusion casting, the film surface is unstable and it is difficult to obtain a film with uniform thickness.
[0195] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
[0196] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A polypropylene composite film, It is characterized in that The polypropylene composite film comprises at least one film layer A formed by a polypropylene composition A and at least one film layer B formed by a polypropylene composition B, wherein the polypropylene composition A comprises polypropylene a and an optional polyolefin elastomer b, and the polypropylene composition B comprises random polypropylene x, polyolefin elastomer y and polypropylene graft z; the polypropylene graft z comprises a structural unit derived from copolymerized polypropylene and a structural unit derived from an alkenyl-containing silane monomer; Based on the weight of the polypropylene graft z, the content of the structural unit derived from the alkenyl-containing silane monomer and in the grafted state in the polypropylene graft z is 0.2-6 wt %; the copolymerized polypropylene has the following characteristics: The comonomer content is 0.5-30 mol%; the xylene soluble content is 2-80 wt%; the comonomer content in the solubles is 10-70 wt%; the intrinsic viscosity ratio of the solubles to the polypropylene is 0.3-5; Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-100 wt% of polypropylene a and 0-50 wt% of polyolefin elastomer b; based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 50-90 wt% of random polypropylene x, 5-40 wt% of polyolefin elastomer y and 2-40 wt% of polypropylene graft z; When the polypropylene composition A includes the polyolefin elastomer b, based on the total weight of the polypropylene composition A being 100 parts by weight, the weight of the polyolefin elastomer b is calculated as Wb, based on the total weight of the polypropylene composition B being 100 parts by weight, the weight of the polyolefin elastomer y is calculated as Wy, and the ratio of Wb to Wy is 6:1-1:4; At 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-10 g / 10 min; at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 3-10 g / 10 min; When the polypropylene composite film has a structure of three or more layers, the film layer B is the surface layer; The alkenyl-containing silane monomer is selected from at least one monomer having a structure shown in Formula I, Formula I Among them, R 1 C 2 -C 12 alkenyl; R 2 , R 3 , R 4 are each independently selected from substituted or unsubstituted C 1 -C 12 Straight chain alkyl, substituted or unsubstituted C 3 -C 12 Branched alkyl, substituted or unsubstituted C 1 -C 12 Alkoxy, substituted or unsubstituted C 1 -C 12 The acyloxy group.
2. The polypropylene composite film according to claim 1, It is characterized in that The polypropylene composite film has at least one of the following characteristics: longitudinal tensile strength ≥40MPa; film haze ≤5.5%; pendulum impact strength ≥0.8J; heat sealing strength at 150°C ≥17N / 15mm; volume resistivity ≥1.8×10 15 Ω•m.
3. The polypropylene composite film according to claim 2, It is characterized in that The longitudinal tensile strength of the polypropylene composite film is ≥55MPa.
4. The polypropylene composite film according to claim 2, It is characterized in that The film haze of the polypropylene composite film is ≤2.7%.
5. The polypropylene composite film according to claim 2, It is characterized in that The pendulum impact strength of the polypropylene composite film is ≥1.8J.
6. The polypropylene composite film according to claim 2, It is characterized in that The heat sealing strength of the polypropylene composite film at 150° C. is ≥20N / 15mm.
7. The polypropylene composite film according to claim 2, It is characterized in that The volume resistivity of the polypropylene composite film is ≥1.9×10 15 Ω•m.
8. The polypropylene composite film according to claim 1, It is characterized in that At 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 3-8 g / 10 min.
9. The polypropylene composite film according to claim 1, It is characterized in that At 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 4-8 g / 10 min.
10. The polypropylene composite film according to claim 1, It is characterized in that The polypropylene a is homopolymer polypropylene and / or polypropylene graft z.
11. The polypropylene composite film according to claim 10, It is characterized in that The homopolymer polypropylene has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity of more than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.
0.
12. The polypropylene composite film according to claim 1, It is characterized in that Based on the weight of the polypropylene graft z, the content of the structural unit derived from the alkenyl-containing silane monomer and in the grafted state in the polypropylene graft z is 0.2-2.5 wt%; and / or, The polypropylene grafted product z has a melt mass flow rate of 0.01-30 g / 10 min at 230° C. and a load of 2.16 kg.
13. The polypropylene composite film according to claim 12, It is characterized in that The polypropylene grafted product z has a melt mass flow rate of 0.05-20 g / 10 min at 230° C. and a load of 2.16 kg.
14. The polypropylene composite film according to claim 13, It is characterized in that The polypropylene grafted product z has a melt mass flow rate of 0.1-10 g / 10 min at 230° C. and a load of 2.16 kg.
15. The polypropylene composite film according to claim 14, It is characterized in that The polypropylene grafted product z has a melt mass flow rate of 0.2-8 g / 10 min at 230° C. and a load of 2.16 kg.
16. The polypropylene composite film according to claim 1, It is characterized in that The polypropylene grafted product Z is prepared by solid phase grafting reaction of copolymerized polypropylene and silane monomers containing alkenyl.
17. The polypropylene composite film according to claim 1, It is characterized in that The comonomer of the copolymerized polypropylene is selected from C 2 -C 8 at least one of the α-olefins of the present invention; and / or, the copolymerized polypropylene has at least one of the following characteristics: a comonomer content of 4-25 mol%; a xylene soluble content of 18-75 wt%; a comonomer content in the solubles of 10-50 wt%; a ratio of the intrinsic viscosity of the solubles to the polypropylene of 0.5-3; a melt mass flow rate of 0.01-60 g / 10 min at 230 °C and a load of 2.16 kg; a melting temperature Tm of above 100 °C; a weight average molecular weight of 20×10 4 -60×10 4 g / mol.
18. The polypropylene composite film according to claim 17, It is characterized in that The xylene soluble content of the copolymerized polypropylene is 30-70 wt %.
19. The polypropylene composite film according to claim 17, It is characterized in that The comonomer content in the soluble matter of the copolymerized polypropylene is 20-35wt%.
20. The polypropylene composite film according to claim 17, It is characterized in that The intrinsic viscosity ratio of the soluble matter of the copolymerized polypropylene to the polypropylene is 0.8-1.
3.
21. The polypropylene composite film according to claim 17, It is characterized in that The copolymerized polypropylene has a melt mass flow rate of 0.05-35 g / 10 min at 230° C. and a load of 2.16 kg.
22. The polypropylene composite film according to claim 21, It is characterized in that The copolymerized polypropylene has a melt mass flow rate of 0.5-15 g / 10 min at 230° C. and a load of 2.16 kg.
23. The polypropylene composite film according to claim 17, It is characterized in that The melting temperature Tm of the copolymerized polypropylene is 110-180°C.
24. The polypropylene composite film according to claim 23, It is characterized in that The melting temperature Tm of the copolymerized polypropylene is 120-170°C.
25. The polypropylene composite film according to claim 1, It is characterized in that R 1 It is a monounsaturated olefinic group.
26. The polypropylene composite film according to claim 1, It is characterized in that R 1 C 2 -C 6 The alkenyl group.
27. The polypropylene composite film according to claim 26, It is characterized in that R 1 It is a monounsaturated olefinic group.
28. The polypropylene composite film according to claim 1, It is characterized in that R 2 , R 3 , R 4 are each independently selected from substituted or unsubstituted C 1 -C 6 Straight chain alkyl, substituted or unsubstituted C 3 -C 6 Branched alkyl, substituted or unsubstituted C 1 -C 6 Alkoxy, substituted or unsubstituted C 1 -C 6 The acyloxy group.
29. The polypropylene composite film according to claim 1, It is characterized in that The alkenyl-containing silane monomer is selected from at least one of vinyl triethoxysilane, vinyl trimethoxysilane, vinyl triisopropoxysilane, vinyl tri-tert-butoxysilane, vinyl triacetoxysilane, methyl vinyl dimethoxysilane, ethyl vinyl diethoxysilane, allyl triethoxysilane, allyl trimethoxysilane, allyl triisopropoxysilane, vinyl tri(β-methoxyethoxy)silane, allyl tri(β-methoxyethoxy)silane, allyl tri-tert-butoxysilane, allyl triacetoxysilane, methyl allyl dimethoxysilane and ethyl allyl diethoxysilane.
30. The polypropylene composite film according to claim 1, It is characterized in that The polyolefin elastomer b and the polyolefin elastomer y are each independently an elastomeric copolymer of ethylene and an α-olefin.
31. The polypropylene composite film according to claim 30, It is characterized in that The alpha olefin is C 3 -C 12 of alpha olefins.
32. The polypropylene composite film according to claim 31, It is characterized in that The alpha olefin is at least one selected from propylene, 1-butene, 1-hexene and 1-octene.
33. The polypropylene composite film according to claim 1, It is characterized in that The random polypropylene x is a copolymer of propylene and ethylene and / or butene; and / or the random polypropylene x has a melt mass flow rate of 2-10 g / 10 min at 230° C. and a load of 2.16 kg.
34. The polypropylene composite film according to claim 33, It is characterized in that The random polypropylene x is at least one selected from ethylene-propylene-butene terpolymer, propylene-ethylene binary random copolymer, and propylene-butene binary random copolymer.
35. The polypropylene composite film according to claim 1, It is characterized in that Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 75-95 wt % of the polypropylene a and 5-25 wt % of the polyolefin elastomer b.
36. The polypropylene composite film according to claim 1, It is characterized in that Based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 60-85 wt% of random polypropylene x, 5-20 wt% of polyolefin elastomer y and 5-20 wt% of polypropylene graft z.
37. The polypropylene composite film according to claim 1, It is characterized in that The ratio of Wb to Wy is 4:1-1:
4.
38. The polypropylene composite film according to claim 1, It is characterized in that In the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:4-2:
1.
39. The polypropylene composite film according to claim 38, It is characterized in that In the polypropylene composite film, the ratio of the sum of the thicknesses of other film layers to the thickness of the film layer A is 1:2-1:
1.
40. The polypropylene composite film according to any one of claims 1 to 39, It is characterized in that The polypropylene composition A and / or the polypropylene composition B further comprises an antioxidant and / or a lubricant.
41. The polypropylene composite film according to claim 40, It is characterized in that The antioxidant is selected from at least one of antioxidant 1076, antioxidant 1010, antioxidant 168 and thioester antioxidants.
42. The polypropylene composite film according to claim 40, It is characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the antioxidant is 0.1-0.8 parts by weight.
43. The polypropylene composite film according to claim 42, It is characterized in that The content of the antioxidant is 0.2-0.4 parts by weight.
44. The polypropylene composite film according to claim 40, It is characterized in that The lubricant is a PEG lubricant and / or a monoglyceride lubricant.
45. The polypropylene composite film according to claim 40, It is characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.01-0.5 parts by weight.
46. The polypropylene composite film according to claim 45, It is characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the lubricant is 0.05-0.2 parts by weight.
47. The polypropylene composite film according to any one of claims 1 to 39, It is characterized in that The polypropylene composition A and / or the polypropylene composition B further comprises a film-forming aid.
48. The polypropylene composite film according to claim 47, It is characterized in that The film-forming aid is selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a filler, a lubricant, an anti-sticking agent and an antistatic agent.
49. The polypropylene composite film according to claim 47, It is characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.01-0.5 parts by weight.
50. The polypropylene composite film according to claim 49, It is characterized in that Based on 100 parts by weight of the total amount of the polypropylene composition A or the polypropylene composition B, the content of the film-forming aid is 0.05-0.3 parts by weight.
51. A method for preparing a polypropylene composite film according to any one of claims 1 to 50, include: The raw material composition for forming each layer is extruded and cast after an optional granulation process to form the composite film; optionally, the method further comprises stretching the obtained composite film.
52. The preparation method according to claim 51, It is characterized in that The stretching is bidirectional stretching.
53. Use of the polypropylene composite film according to any one of claims 1 to 50 in the field of packaging materials.
54. The use according to claim 53, It is characterized in that The packaging is battery packaging, electronic product packaging or food packaging.
Citation Information
Patent Citations
Method of preparing high-performance polypropylene composition
CN101058654A
Method of preparing polypropylene graft polymer
CN101492517B
Process for the preparation of soft propylene polymer compositions
CN101679557A
Toughening type three-layer coextru-laminated film and preparation method thereof
CN101913279A
Pre-irradiation polypropylene graft copolymer and preparation method thereof
CN102108112A