Silver nanowire dispersion, conductor containing silver nanowires, and conductive laminate containing silver nanowires

By using a specific aromatic heterocyclic compound chelating agent in the silver nanowire dispersion, the problem of silver particle generation and particulation caused by electric fields is solved, and the stability and performance of the conductive layer are improved.

CN115997257BActive Publication Date: 2024-10-15SEIKO PMC CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180041769.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-17
Filing Date
2021-03-30
Publication Date
2024-10-15
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

The generation of silver particles in the existing silver nanowire dispersion leads to deterioration of optical properties, and the silver nanowires are prone to particleization when an electric field is applied, affecting the stability and performance of the conductive material.

Method used

Silver nanowires are formed by coexisting silver nanowires with specific chelating agents, such as 1,10-phenanthroline, quinoline substituted with hydroxyl or amino groups at the 8-position, 2,2′-bipyridine and other aromatic heterocyclic compounds. Dispersion liquid, inhibits the generation of silver particles and improves the stability of the conductive layer.

Benefits of technology

It effectively suppresses the generation of silver particles in the silver nanowire dispersion, improves the stability and durability of the conductive layer, prevents particleization when an electric field is applied, and improves optical characteristics and conductive properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004951201800000011
    Figure FDA0004951201800000011
  • Figure FDA0004951201800000021
    Figure FDA0004951201800000021
  • Figure FDA0004951201800000022
    Figure FDA0004951201800000022
Patent Text Reader

Abstract

In view of the problems in the prior art, the problem of the present invention is to provide a method for suppressing the generation of silver particles in a dispersion of silver nanowires compared with the existing methods, and to suppress the particle formation of silver nanowires on the anode side by a simple method. The present invention further provides a silver nanowire dispersion, a conductor containing silver nanowires, and a conductive laminate containing silver nanowires. The silver nanowire dispersion comprises silver nanowires, a dispersion solvent, and a chelating agent, wherein the average diameter of the silver nanowires is less than 100 nm, and the silver nanowire dispersion is characterized in that the chelating agent is contained in an amount of 0.1 μmol / g to 1000 μmol / g relative to the content of the silver nanowires, and the chelating agent is a specific aromatic heterocyclic compound having at least one imine skeleton in the molecule.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a silver nanowire dispersion characterized by containing a specific chelating agent, a silver nanowire-containing conductor containing the specific chelating agent, and a silver nanowire-containing conductive laminate. Background Art

[0002] In recent years, the use of display devices such as liquid crystal displays, plasma displays, organic electroluminescent displays or electronic paper, input sensors such as touch screens, and solar cells that utilize sunlight such as thin-film amorphous Si solar cells or dye-sensitized solar cells has increased, and the demand for transparent conductive films, which are essential components in these devices, has also increased.

[0003] Indium tin oxide (ITO) has been mainly used as a material for the transparent conductive film. Although a thin film using ITO can obtain high transparency and high conductivity, it is generally produced by a sputtering device or an evaporation device, so there are problems in terms of production speed or manufacturing cost. Furthermore, since indium, which is a raw material of ITO, is a rare metal whose stable supply is considered to be a problem, it is required to develop an alternative material to ITO.

[0004] One of the materials that has attracted attention as a material for a transparent conductive film that replaces ITO is metal nanowires. Metal nanowires have a small diameter and therefore have high light transmittance in the visible light region, so they can be used as transparent conductive films. In particular, transparent conductive films using silver nanowires have attracted attention because of their high conductivity and stability.

[0005] In a transparent conductive film using silver nanowires, generally, the smaller the diameter of the silver nanowires, the more light scattering can be suppressed, thereby improving the optical properties of the film. Therefore, methods for producing thinner silver nanowires have been studied, and for example, Patent Document 1 reports a method for producing silver nanowires having an average diameter of less than 30 nm and a low-haze transparent conductor using the silver nanowires.

[0006] However, it is known that the silver nanowires obtained in Patent Document 1 are unstable due to their very small diameters, and for example, the dispersion of the silver nanowires gradually produces silver particles as a by-product due to time-dependent changes. Such silver particles scatter light in a film coated with the silver nanowires, causing the optical properties of the film to deteriorate. Therefore, a method for solving such a problem is required.

[0007] Several solutions have been proposed for additives that improve the stability of silver nanowires. For example, Patent Document 2 reports that the use of a pyridine-ketone compound can suppress the increase in the surface resistance of a film coated with silver nanowires. Patent Document 3 reports that the use of a heterocyclic compound having a specific interaction potential improves the thermal stability of a silver nanowire coating. In addition, several stabilizers for conductive films coated with silver nanowires against light or high temperature and high humidity conditions have been reported (for example, Patent Documents 4 to 8), but additives that suppress the generation of silver particles in the state of a silver nanowire dispersion are unknown.

[0008] In addition, it is known that in a conductive material using silver nanowires, the degradation of the silver nanowires represented by migration is aggravated due to the application of an electric field. It can be confirmed that the degradation is actually aggravated due to the particle formation of the silver nanowires on the anode side when the electric field is applied. Therefore, a method for preventing the degradation of silver nanowires due to the application of an electric field is being developed. For example, in Patent Document 9, the durability is improved by plating different metals on the surface of silver, but a separate plating process is required, and there is a problem that the process becomes complicated. In Patent Document 10, it is reported that the migration resistance is improved by mixing a low molecular weight compound having a urea bond in the silver nanowire ink, but it is only an evaluation of the presence or absence of a short circuit. Therefore, a method that can suppress the particle formation of silver nanowires on the anode side by a simple method is required.

[0009] [Prior art literature]

[0010] [Patent Document]

[0011] Patent Document 1: Japanese Patent Publication No. 2013-517603

[0012] Patent Document 2: U.S. Patent Application Publication No. 2014 / 0255708

[0013] Patent Document 3: Japanese Patent Application Publication No. 2010-086714

[0014] Patent Document 4: U.S. Patent Application Publication No. 2015 / 0270024

[0015] Patent Document 5: Japanese Patent Application Publication No. 2016-001608

[0016] Patent Document 6: Japanese Patent Publication No. 2016-515280

[0017] Patent Document 7: Japanese Patent Re-publication No. 2018-008464

[0018] Patent Document 8: Japanese Patent Re-publication No. 2018-116501

[0019] Patent Document 9: Japanese Patent Application Publication No. 2013-151752

[0020] Patent Document 10: Japanese Patent Re-publication No. 2019-198494 Summary of the invention

[0021] [Problems to be solved by the invention]

[0022] In view of the above problems in the prior art, the present invention aims to provide a method for suppressing the generation of silver fine particles in a dispersion of silver nanowires compared with the conventional methods, and to suppress the particle formation of silver nanowires on the anode side by a simple method.

[0023] [Technical means to solve the problem]

[0024] The present inventors have conducted intensive studies to solve the above-mentioned problems and, as a result, have found that the above-mentioned problems can be solved by allowing silver nanowires to coexist with a specific chelating agent, thereby completing the present invention.

[0025] That is, the present invention is

[0026] <1> A silver nanowire dispersion liquid comprises silver nanowires, a dispersion solvent and a chelating agent, wherein the average diameter of the silver nanowires is less than 100 nm, and the silver nanowire dispersion liquid is characterized in that the chelating agent is contained in an amount of 0.1 μmol / g to 1000 μmol / g relative to the content of the silver nanowires, and the chelating agent is at least one selected from the group consisting of 1,10-phenanthroline, quinoline substituted with a hydroxyl group or an amino group at the 8-position, 2,2′-bipyridine, biazole (wherein the azole is any one of imidazole, thiazole and oxazole) and derivatives thereof,

[0027] <2> According to the <1> The silver nanowire dispersion, wherein the chelating agent is at least one selected from the group consisting of general formula (1) to general formula (4),

[0028] [General formula (1)]

[0029] [Chemistry 1]

[0030]

[0031] (Wherein, in the general formula (1), L represents a hydroxyl group or an amino group, and R 1 ~R 4 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, or a halogen group, and R 2 , R 3 At least one of them is hydrogen, R 1 ~R 4 At least two of them are hydrogen)

[0032] [General formula (2)]

[0033] [Chemistry 2]

[0034]

[0035] (Wherein, in the general formula (2), R 5 , R 6 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, or a halogen group, and R 7 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, a phenyl group, a C6H4SO3Na group, or a halogen group, and R 5 ~R 7 At least one of them is hydrogen)

[0036] [General formula (3)]

[0037] [Chemistry 3]

[0038]

[0039] (Wherein, in the general formula (3), R 8 , R 9 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, or a halogen group, and R 10 represents hydrogen, an alkyl group having 1 to 4 carbon atoms, or a halogen group, and R 8 ~R 10 At least two of them are hydrogen)

[0040] [General formula (4)]

[0041] Z 1 -Z 2

[0042] (Wherein, in the general formula (4), Z 1 , Z 2 Each independently represents any one of the nitrogen-containing heterocyclic rings represented by the general formula (5) or the general formula (6)

[0043] [General formula (5)]

[0044] [Chemistry 4]

[0045]

[0046] (Wherein, in the general formula (5), X 1 represents any one of NH, O, and S, and R 11 , R 12 represents hydrogen, a straight-chain alkyl group having 1 to 4 carbon atoms, a halogen group, or a benzene ring formed together; the arrow represents the Z 1 or Z 2 Single key)

[0047] [General formula (6)]

[0048] [Chemistry 5]

[0049]

[0050] (Wherein, in the general formula (6), X 2 represents any one of NH, O, and S, and R 13 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, or a halogen group, and the arrow represents a 1 or Z 2 Single key)

[0051] <3> According to the <1> or <2> The silver nanowire dispersion, wherein the content of the chelating agent is 1 μmol / g to 300 μmol / g relative to the content of the silver nanowires,

[0052] <4> According to the <1> to <3> The silver nanowire dispersion according to any one of the preceding claims, wherein the chelating agent is at least one selected from the group consisting of 1,10-phenanthroline, neocuprous reagent, bathophenanthroline and its sodium sulfonate, 2,2′-bipyridine, 8-hydroxyquinoline, 8-aminoquinoline, and 2-(4-thiazolyl)benzimidazole,

[0053] <5> According to the <1> to <4> The silver nanowire dispersion according to any one of the preceding claims, wherein the average diameter of the silver nanowires is 30 nm or less,

[0054] <6> According to the <1> to <5> The silver nanowire dispersion according to any one of the preceding claims, wherein the concentration of the silver nanowires is 0.01 mass % to 3 mass %,

[0055] <7> According to the <1> to <6> The silver nanowire dispersion according to any one of the preceding claims further comprises a polymer compound selected from polymers having amide bonds or polysaccharides, wherein the concentration of the polymer compound is 0.02 mass % to 1 mass %,

[0056] <8> According to the <1> to <7> The silver nanowire dispersion according to any one of the preceding claims, wherein the dispersion medium comprises water or a monohydric alcohol having 1 to 3 carbon atoms, and the content of water or the monohydric alcohol having 1 to 3 carbon atoms in the dispersion medium is 85% by mass or more,

[0057] <9> A conductor containing silver nanowires, comprising a substrate and at least one conductive layer containing silver nanowires, characterized in that the conductive layer further comprises 0.1 μmol / g to 1000 μmol / g of a chelating agent relative to the content of the silver nanowires, wherein the chelating agent is at least one selected from the group consisting of 1,10-phenanthroline, quinoline substituted with a hydroxyl group or an amino group at the 8-position, 2,2′-bipyridine, biazole (wherein the azole is any one of imidazole, thiazole, and oxazole) and derivatives thereof, among aromatic heterocyclic compounds having at least one imine skeleton in the molecule.

[0058] <10> According to the <9> The conductor containing silver nanowires, wherein the sheet resistance of the conductive layer is 1Ω / □ to 100Ω / □,

[0059] <11> According to the <9> or <10> The silver nanowire-containing conductor further has a Δ haze of less than 1.5%,

[0060] <12> A conductive laminate containing silver nanowires, comprising a substrate, a conductive layer containing silver nanowires, and a protective layer containing a chelating agent, wherein the chelating agent is at least one selected from the group consisting of 1,10-phenanthroline, quinoline substituted with a hydroxyl group or an amino group at the 8-position, 2,2′-bipyridine, biazole (wherein the azole is any one of imidazole, thiazole, and oxazole) and derivatives thereof, among aromatic heterocyclic compounds having at least one imine skeleton in the molecule.

[0061] <13> According to the <12> In the conductive laminate containing silver nanowires, the protective layer contains 0.05% to 5% by mass of a chelating agent.

[0062] [Effects of the Invention]

[0063] According to the present invention, by using a specific chelating agent, the generation of fine particles that cause deterioration of optical properties from the dispersion of silver nanowires can be suppressed compared to the conventional method. Furthermore, if the chelating agent used in the present invention is used, the particle formation of the conductive layer containing silver nanowires when an electric field is applied can also be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] none DETAILED DESCRIPTION

[0065] Hereinafter, the present invention will be described in detail.

[0066] [Silver Nanowires]

[0067] The "silver nanowire" of the present invention refers to a silver structure having a diameter of less than 1 μm and an aspect ratio (major axis length / diameter) of at least 2. The "microparticle" of the present invention refers to a structure having a diameter of less than 1 μm and an aspect ratio (major axis length / diameter) of less than 2.

[0068] [Diameter of silver nanowire]

[0069] When silver nanowires are used as transparent conductive films, in order to improve transparency, it is advantageous that the average diameter of the wire is small, and it is preferred. The "diameter of the silver nanowire" in the present invention refers to the diameter measured using a scanning electron microscope (SEM (scanning electron microscope); manufactured by JEOL Ltd., JSM-5610LV). In addition, the "average diameter of the silver nanowire" refers to the average value of the diameters observed and measured for more than 100 silver nanowires. In the present invention, the average diameter of the silver nanowire is preferably 100 nm or less, more preferably 40 nm or less, further preferably 30 nm or less, and particularly preferably 25 nm or less.

[0070] [Long axis length of silver nanowires]

[0071] The transparent conductive film containing silver nanowires is formed by the mutual contact of silver nanowires, and the three-dimensional conductive network structure is widely distributed in space, thereby showing conductivity. Therefore, from the perspective of conductivity, it is preferred that the average long axis length of the nanowires is long. On the other hand, since too long nanowires are easy to entangle, short nanowires are preferred from the perspective of dispersion stability. The "long axis length of the silver nanowire" in the present invention refers to the value calculated by photographing the silver nanowires using a dark field microscope (trade name: BX51, manufactured by Olympus (stock)) and using image processing software (trade name: Image-Pro Premier, manufactured by Media Cybemetics, Inc.). In addition, the "average long axis length of the silver nanowire" refers to the average value of the long axis length observed and measured for more than 1,000 silver nanowires. In the present invention, the average long axis length of the silver nanowires is preferably 1 μm to 100 μm, more preferably 5 μm to 30 μm, and further preferably 7 μm to 20 μm.

[0072] [Method for producing silver nanowires]

[0073] The method for producing the silver nanowires used in the present invention is not particularly limited, and silver nanowires obtained by a known production method can be used. Among them, a production method in which silver nanowires are obtained by reducing a silver salt in a polyol in the presence of a growth control agent and a halide salt is preferably used.

[0074] [Polyol]

[0075] As the polyol, there is no particular limitation as long as it is a compound that can reduce silver ions, and at least one can be appropriately selected from compounds having two or more hydroxyl groups according to the purpose. As specific examples, diols such as ethylene glycol, propylene glycol, butylene glycol, and diethylene glycol, and triols such as glycerol can be cited. Among these, diols of saturated hydrocarbons having 1 to 5 carbon atoms and triols of saturated hydrocarbons having 1 to 5 carbon atoms are preferred in terms of the ease of solubility of liquids or growth control agents. Among them, ethylene glycol, 1,2-propylene glycol (propylene glycol (Propylene glycol)), 1,3-propylene glycol, 1,3-butylene glycol, and glycerol are more preferably used, and propylene glycol is further preferably used.

[0076] [Growth control agent]

[0077] The growth control agent is not particularly limited, and at least one polymer can be appropriately selected according to the purpose. As specific examples, it is polyvinyl pyrrolidone, poly (meth) acrylamide, poly N-substituted (meth) acrylamide, poly (meth) acrylic acid and its derivatives, polyvinyl alcohol or their copolymers. Among these, preferably a polymer having an amide skeleton, more preferably polyvinyl pyrrolidone, poly N-substituted (meth) acrylamide or their copolymers, and further preferably polyvinyl pyrrolidone. The N-substituted (meth) acrylamide used here is not particularly limited as long as the hydrogen atom at the N position of (meth) acrylamide is substituted by one or more functional groups such as alkyl, hydroxyalkyl, aryl, alkoxyalkyl, etc.

[0078] [Halide salts]

[0079] As long as the halide salt is a compound that dissociates halide ions by dissolving an inorganic salt or an organic salt in a polar solvent, there is no particular limitation, and at least one can be appropriately selected according to the purpose. As a specific example of the halide salt, there can be listed: alkali metal halides such as lithium chloride, sodium chloride, potassium chloride, sodium bromide, potassium bromide, alkaline earth metal halides such as magnesium chloride, calcium chloride, magnesium bromide, earth metal halides such as aluminum chloride, zinc group metal halides such as zinc chloride, carbon group metal halides such as tin chloride, transition metal halides such as ferric chloride, ferric bromide, nickel chloride, zirconium oxychloride, triethylamine hydrochloride, amine hydrochlorides such as dimethylethanolamine hydrochloride, ammonium chloride, ammonium bromide, tetrabutylammonium chloride, tetrabutylammonium bromide, benzyltriethylammonium chloride, phosphonium salt halides such as tetrabutylphosphonium chloride, etc. These can be used alone or in combination of two or more. In particular, the use of chloride salts increases the yield of silver nanowires, so it is preferred to use chloride salts. By using bromide salts, silver nanowires with smaller diameters can be obtained, so it is more preferred to use both chloride salts and bromide salts. As the chloride salt, lithium chloride, sodium chloride, potassium chloride, zirconium oxychloride, ammonium chloride, benzyltriethylammonium chloride is preferably used, and sodium chloride is more preferably used. As the bromide salt, sodium bromide, potassium bromide, ammonium bromide, tetrabutylammonium bromide is preferably used, and sodium bromide is more preferably used.

[0080] [Silver salt]

[0081] As the silver salt, there is no particular limitation as long as it is a silver compound reduced by a polyol, and at least one can be appropriately selected according to the purpose. As specific examples, inorganic acid salts such as silver nitrate, silver sulfate, silver sulfamate, silver chlorate, and silver perchlorate, and organic acid salts such as silver acetate and silver lactate can be listed. Among these, silver nitrate is preferably used. In addition, the halide salt and the silver salt can also be used in combination with the same substance. As such a compound, for example, silver chloride or silver bromide can be listed.

[0082] [Purification of silver nanowires]

[0083] The silver nanowires obtained by the silver nanowire production method are preferably prepared by purifying the reaction solution by a conventionally known method such as centrifugation, filtration, decantation, elutriation, or a method of precipitation with a solvent followed by dispersion treatment to prepare a silver nanowire dispersion using a dispersion solvent.

[0084] [Silver Nanowire Dispersion]

[0085] The silver nanowire dispersion of the present invention is a dispersion in which silver nanowires are dispersed in a dispersion solvent. Various additives may be used in the silver nanowire dispersion as needed to the extent that the effects of the invention are not impaired. Specific examples of the additives include surfactants and polymer compounds.

[0086] [Concentration of silver nanowire dispersion]

[0087] The silver nanowire concentration of the silver nanowire dispersion used in the present invention can be set arbitrarily. From the viewpoint of dispersion stability, it is preferably 10% by mass or less, more preferably 5% by mass or less, further preferably 3% by mass or less, and particularly preferably 1% by mass or less. In addition, when the silver nanowire concentration is extremely low, in order to achieve the target resistance value during coating, it is necessary to increase the coating thickness or to coat multiple times, which increases the man-hours during use. Therefore, from the viewpoint of productivity, it is preferably 0.005% by mass or more, more preferably 0.01% by mass or more, and further preferably 0.05% by mass or more.

[0088] [Haze of diluted silver nanowire dispersion]

[0089] By measuring the haze of a silver nanowire dispersion of a specific concentration, the degree of light scattering when the silver nanowire dispersion is made into a coating film can be estimated. The "haze of a diluted silver nanowire dispersion" in the present invention refers to a value obtained by placing a diluted silver nanowire dispersion having a silver concentration of 0.0015% using ion exchange water into a cell having an optical path length of 1 cm and measuring the haze using NDH5000 (manufactured by Nippon Denshoku Industries Co., Ltd.). From the perspective of transparency when the dispersion is formed into a film, the haze of the diluted silver nanowire dispersion is preferably less than 10.0%, more preferably less than 5.0%, further preferably less than 3.0%, and particularly preferably less than 2.6%.

[0090] [dispersion solvent]

[0091] The dispersion solvent used in the present invention may be any compound as long as it can disperse the silver nanowires and dissolve other components contained in the silver nanowire dispersion such as a polymer compound. In addition, since the silver nanowire dispersion can also be used to form a conductive layer containing silver nanowires, the dispersion solvent is preferably a compound that forms a uniform coating film by evaporating the conductive layer containing silver nanowires during film formation. As specific examples, alcohols such as water, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, and diacetone alcohol can be cited; polyols such as ethylene glycol, propylene glycol, 1,3-propylene glycol, 1,3-butanediol, 1,4-butanediol, and glycerol; glycol ethers such as ethylene glycol monobutyl ether and propylene glycol monomethyl ether; glycol dimethyl ethers such as ethylene glycol dimethyl ether; glycol ether esters such as ethylene glycol monomethyl ether acetate; esters such as ethyl acetate and butyl acetate; ketones such as acetone and methyl ethyl ketone; aromatics such as toluene; and solvents containing two or more thereof. Among them, from the perspective of the dispersibility of silver nanowires, it is preferred to use a polar solvent. Among them, the content of water or monohydric alcohols having 1 to 3 carbon atoms in the dispersion solvent is preferably 50% by mass or more, more preferably 75% by mass or more, and further preferably 85% by mass or more.

[0092] [Chelating agent]

[0093] A chelating agent refers to a compound having the ability to coordinate with respect to a certain metal center at at least two different positions in the same molecule. In the present invention, a specific aromatic heterocyclic compound having at least one imine skeleton in the chelating agent molecule is used together with silver nanowires. An aromatic heterocyclic ring having an imine skeleton is an aromatic ring in which at least one carbon of a ring forming an aromatic ring such as benzene or furan is substituted with nitrogen, and specifically, pyridine or oxazole can be cited. The chelating agent used in the present invention is a compound that can be chelated and coordinated by an imine nitrogen of an aromatic heterocyclic ring having at least one imine skeleton and at least one heteroatom. It is believed that a chelating agent having an aromatic heterocyclic structure containing an imine skeleton exerts the effect of the invention through the moderate coordination ability of the imine nitrogen contained in the heterocyclic structure to silver and the stabilization based on the chelating effect. The positional relationship between the imine nitrogen with coordination ability and another heteroatom is also important, and it is preferred that another heteroatom with coordination ability is configured at a position away from the imine nitrogen of the aromatic heterocyclic ring by three bonds, and a compound with a chelating structure can be adopted. Among them, the structure of the chelating agent is preferably fixed to a structure capable of chelating coordination. In addition, another functional group having a heteroatom is also important and must be any one of hydroxyl, amino, and imine nitrogen. Among these, from the viewpoint of affinity to silver, amino or imine nitrogen is preferred, and imine nitrogen is more preferred. Thus, the aromatic heterocycle having an imine skeleton possessed by the chelating agent that can be used in the present invention is at least one selected from the group consisting of 1,10-phenanthroline, quinoline substituted with a hydroxyl or amino group at the 8th position, 2,2′-bipyridine, oxazole (wherein, azole is any one of imidazole, thiazole, oxazole) and derivatives thereof. The chelating agents having each aromatic heterocyclic structure are described in detail below.

[0094] 1,10-phenanthroline and its derivatives are the most preferably used compound group because the two heteroatoms that can be chelated in the 1,10-phenanthroline skeleton are both imine nitrogen and are fixed to a structure that performs chelation coordination. As examples of 1,10-phenanthroline and its derivatives that can be preferably used, the compounds represented by the following general formula (7) can be cited.

[0095] [General formula (7)]

[0096] [Chemistry 6]

[0097]

[0098] (Wherein, in the general formula (7), R 5 , R 6 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, or a halogen group, and R 7 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, a phenyl group, a C6H4SO3Na group, or a halogen group, and R 5 ~R 7 At least one of them is hydrogen)

[0099] Specific examples of these 1,10-phenanthroline and derivatives thereof include 1,10-phenanthroline, neocuprous reagent, 2,9-dibutyl-1,10-phenanthroline, 4,7-dimethyl-1,10-phenanthroline, 3,4,7,8-tetramethyl-1,10-phenanthroline, 2,9-dichloro-1,10-phenanthroline, 4,7-dichloro-1,10-phenanthroline, bathophenanthroline and its sodium sulfonate, 2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline (bathocuproin) and its sodium sulfonate, etc. Among them, from the viewpoint of easy availability, it is preferred to use 1,10-phenanthroline, neocuprous reagent, bathophenanthroline and its sodium sulfonate, and it is more preferred to use 1,10-phenanthroline. In addition, the smaller the substituent near the coordinating functional group, the less steric hindrance it will have, which is beneficial for the interaction with silver. 5 Preferred is hydrogen or methyl, more preferred is hydrogen.

[0100] Quinoline and its derivatives substituted with hydroxyl or amino at position 8 can adopt a chelate structure based on imine nitrogen and hydroxyl or amino, and are compounds fixed to a structure for chelate coordination. As examples of quinoline and its derivatives that can be preferably used, compounds represented by the following general formula (8) can be cited.

[0101] [General formula (8)]

[0102] [Chemistry 7]

[0103]

[0104] (Wherein, in the general formula (8), L represents a hydroxyl group or an amino group, and R 1 ~R 4 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, or a halogen group, and R 2 , R 3 At least one of them is hydrogen, R 1 ~R 4 At least two of them are hydrogen)

[0105] Specific examples of quinoline and its derivatives substituted with a hydroxyl group or an amino group at the 8-position include 8-hydroxyquinoline, 8-hydroxy-2-methylquinoline, 8-hydroxy-2-propylquinoline, 5-fluoro-8-hydroxyquinoline, 5-chloro-8-hydroxyquinoline, 7-bromo-5-chloro-8-hydroxyquinoline, 8-aminoquinoline, 8-amino-2-methylquinoline, etc. Among them, from the viewpoint of easy availability, 8-hydroxyquinoline, 8-hydroxy-2-methylquinoline, 5-chloro-8-hydroxyquinoline, and 8-aminoquinoline are preferably used, and 8-hydroxyquinoline and 8-aminoquinoline are more preferably used. In addition, the smaller the substituent near the coordinating functional group, the more moderate the steric hindrance is, which is beneficial to the interaction with silver. In the general formula (8), R 1 It is preferably hydrogen or methyl, and more preferably hydrogen. From the viewpoint of interaction with silver, L in the general formula (8) is more preferably an amino group.

[0106] In 2,2'-bipyridine and its derivatives, the pyridyl groups of the 2,2'-bipyridine skeleton are connected to each other by a single bond, so they can rotate freely around the bond axis. Therefore, although the structure for chelating coordination is not fixed, the two heteroatoms that can be chelated are both imine nitrogen and can be preferably used. As examples of 2,2'-bipyridine and its derivatives that can be preferably used, the compounds represented by the following general formula (9) can be cited.

[0107] [General formula (9)]

[0108] [Chemistry 8]

[0109]

[0110] (Wherein, in the general formula (9), R 8 , R 9 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, or a halogen group, and R 10 represents hydrogen, an alkyl group having 1 to 4 carbon atoms, or a halogen group, and R 8 ~R 10 At least two of them are hydrogen)

[0111] Specific examples of these 2,2′-bipyridines and their derivatives include 2,2′-bipyridine, 4,4′-dimethyl-2,2′-bipyridine, 5,5′-dimethyl-2,2′-bipyridine, 6,6′-dimethyl-2,2′-bipyridine, 4,4′-dibromo-2,2′-bipyridine, 6,6′-dibromo-2,2′-bipyridine, and 4,4′-di-tert-butyl-2,2′-bipyridine. Among them, 2,2′-bipyridine is preferably used from the viewpoint of easy availability. In addition, since the smaller the substituent near the coordinating functional group, the more moderate the steric hindrance is, which is beneficial to the interaction with silver, R in the general formula (9) is preferably 1,2′-bipyridine. 8 Preferred is hydrogen or methyl, more preferred is hydrogen.

[0112] In general, the so-called oxazole is a compound in which two azoles are bonded by a single bond, and the oxazole mentioned in the present invention refers to each azole (wherein, azole is any one of imidazole, thiazole, and oxazole) at the 2nd or 4th position and another azole bonded to form a compound of the oxazole skeleton. In oxazole and its derivatives, the azole groups of the oxazole skeleton are connected to each other by a single bond, so they can rotate freely around the bond axis, so the structure of chelate coordination is not fixed in the same way as 2,2'-bipyridine. However, compared with 2,2'-bipyridine in which 6-member rings are bonded to each other by a single bond, the oxazole in which 5-member rings are bonded to each other by a single bond takes a coplanar shape in two rings and adopts a preferred structure for chelate coordination, and the steric hindrance of the two rings is small, so the preferred structure for chelate coordination can be stably present, so 2,2'-bipyridine and its derivatives can be more preferably used. Furthermore, since the two heteroatoms that can be chelated are both imine nitrogen, it can be preferably used. As examples of azole and its derivatives that can be preferably used, compounds represented by the following general formula (10) can be mentioned.

[0113] [General formula (10)]

[0114] Z 1 -Z 2

[0115] (Wherein, in the general formula (10), Z 1 , Z 2 Each independently represents any one of the nitrogen-containing heterocyclic rings represented by the general formula (11) or the general formula (12)

[0116] [General formula (11)]

[0117] [Chemistry 9]

[0118]

[0119] (Wherein, in the general formula (11), X 1 represents any one of NH, O, and S, and R 11 , R 12 represents hydrogen, a straight-chain alkyl group having 1 to 4 carbon atoms, a halogen group, or a benzene ring formed together; the arrow represents the Z 1 or Z 2 Single key)

[0120] Among them, the smaller the substituent near the coordinating functional group, the less steric hindrance it has, which is beneficial for the interaction with silver. In general formula (11), R 11 Preferably hydrogen or R 12 Together they form a benzene ring.

[0121] [General formula (12)]

[0122] [Chemistry 10]

[0123]

[0124] (Wherein, in the general formula (12), X 2 represents any one of NH, O, and S, and R 13 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, or a halogen group, and the arrow represents a 1 or Z 2 Single key)

[0125] Among them, the smaller the substituent near the coordinating functional group, the less steric hindrance it has, which is beneficial for the interaction with silver. In general formula (12), R 13 Preferred is hydrogen or methyl, more preferred is hydrogen.

[0126] Specific examples of these biazoles and their derivatives include 2-(4-thiazolyl)benzimidazole, 2,2′-biimidazole, 2,2′-bis-(4,5-dimethylimidazole), 2,2′-dimethyl-4,4′-bithiazole, etc. Among them, 2-(4-thiazolyl)benzimidazole is preferably used from the viewpoint of easy availability.

[0127] [Content of Chelating Agent in Silver Nanowire Dispersion Liquid]

[0128] By adding the chelating agent specified in the present invention to the dispersion of silver nanowires, the generation of microparticles in the silver nanowire dispersion over time can be suppressed. The more the amount of chelating agent used in the present invention, the more the generation of microparticles can be suppressed, so the chelating agent contained in the silver nanowire dispersion needs to be used at 0.1 μmol / g or more relative to the silver nanowires. Among them, it is preferably 0.5 μmol / g or more, more preferably 1 μmol / g or more, further preferably 2 μmol / g or more, and particularly preferably 5 μmol / g or more. On the other hand, from the perspective of the dispersibility or conductivity of the silver nanowires, the amount of the chelating agent used is preferably small. Therefore, the amount of the chelating agent used is preferably 1000 μmol / g or less, more preferably 300 μmol / g or less, and further preferably 100 μmol / g or less relative to the silver nanowires.

[0129] [Polymer compounds]

[0130] In order to improve the dispersion stability or coating adaptability of silver nanowires, it is preferred to add a polymer compound to the silver nanowire dispersion of the present invention. Specific examples of polymer compounds include: methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, nitrocellulose, cellulose acetate, guar gum, xanthan gum, tamarind gum, psyllium gum, ghatti gum, locust bean gum, hydroxyethyl guar gum, hydroxypropyl guar gum and other polysaccharides and their derivatives, poly (meth) acrylic resin, polyurethane resin, polyester resin, alkyd resin, epoxy resin, ethylene vinyl acetate resin, polyvinyl pyrrolidone and other poly-N-vinyl compounds, poly (meth) acrylamide, poly N-substituted (meth) acrylamide, polyvinyl alcohol and its derivatives, etc. Among them, it is preferred to use polysaccharides and their derivatives or polymers having amide bonds. Among polysaccharides and their derivatives, methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose are preferred, and hydroxypropyl methyl cellulose is more preferred. Among polymers having an amide bond, poly-N-substituted (meth)acrylamide and polyvinyl pyrrolidone are preferably used, and polyvinyl pyrrolidone is more preferred.

[0131] [Concentration of polymer compounds]

[0132] From the viewpoint of improving the dispersibility or coating suitability of the silver nanowires, the concentration of the polymer compound contained in the silver nanowire dispersion is preferably 0.005% by mass or more, more preferably 0.02% by mass or more, and further preferably 0.05% by mass or more. In addition, from the viewpoint of the conductivity of the coating film, the content of the polymer compound is preferably 5% by mass or less, more preferably 1% by mass or less, and further preferably 0.4% by mass or less.

[0133] [Film formation of a silver nanowire-containing conductive layer using a silver nanowire dispersion]

[0134] The silver nanowire dispersion of the present invention can be used, for example, to form a conductive layer containing silver nanowires, and the conductive layer containing silver nanowires can be obtained by coating on a substrate using a known method. Specific examples of coating methods include spin coating, slit coating, dip coating, blade coating, rod coating, spray coating, relief printing, gravure printing, screen printing, lithographic printing, dispensing, and inkjet. In addition, these coating methods can be used to repeatedly coat multiple times.

[0135] [Conductor containing silver nanowires]

[0136] The conductor containing silver nanowires is a conductor having a substrate and a conductive layer containing silver nanowires.

[0137] [Conductive laminate containing silver nanowires]

[0138] The conductive laminate containing silver nanowires is a laminate having at least one layer each of a substrate, a conductive layer containing silver nanowires, and a protective layer. The conductive layer containing silver nanowires can be formed by film-forming a silver nanowire dispersion. In addition, the protective layer can be formed by film-forming a protective layer-forming resin composition. In the present invention, a chelating agent may be included in the conductive layer containing silver nanowires and / or the protective layer. By including the chelating agent specified in the present invention in at least one of the conductive layer containing silver nanowires and / or the protective layer, the particle formation of the silver nanowires when an electric field is applied can be suppressed.

[0139] [Layering method]

[0140] The method for producing the conductive laminate containing silver nanowires is not particularly limited. For example, the following methods can be cited: forming a conductive layer containing silver nanowires by film-forming a silver nanowire dispersion on a substrate, and then forming a protective layer on the upper surface thereof; or forming a protective layer on the substrate in advance, and then sequentially forming a conductive layer containing silver nanowires and a protective layer thereon.

[0141] [Substrate]

[0142] The substrate can be appropriately selected according to the application, and can be hard or easily bendable. In addition, it can also be colored. The substrate of the present invention can be used without particular limitation as long as it is obtained by a known method or a commercially available substrate. Specific examples of substrate materials include glass, polyimide, polycarbonate, polyether sulfone, polyacrylate, polyester, polyethylene terephthalate, polyethylene naphthalate, polyolefin, and polyvinyl chloride. Organic functional materials and inorganic functional materials can also be formed on the substrate. In addition, multiple substrates can also be stacked.

[0143] [Conductive layer containing silver nanowires]

[0144] The silver nanowire-containing conductive layer is a layer containing silver nanowires. The silver nanowire-containing conductive layer can be prepared by forming a film of a silver nanowire dispersion. The silver nanowire dispersion can use a known dispersion, but preferably contains a chelating agent specified in the present invention.

[0145] [Sheet resistance of conductive layer containing silver nanowires]

[0146] The sheet resistance of the conductive layer containing silver nanowires is used as an indicator of the conductivity of the conductive body containing silver nanowires or the conductive laminate containing silver nanowires. The sheet resistance of the conductive layer containing silver nanowires can be arbitrarily set according to the purpose of use by changing the amount of silver nanowires contained in the conductive layer. The range of sheet resistance that can be preferably used is 0.1Ω / □ to 1000Ω / □, and more preferably 1Ω / □ to 100Ω / □.

[0147] [Protective layer]

[0148] The protective layer is formed of a protective layer-forming resin composition, and is provided mainly for the purpose of physically and chemically protecting the conductive layer containing the silver nanowires. The protective layer may be provided adjacent to the conductive layer containing the silver nanowires, or may have multiple layers between the protective layer and the conductive layer. From the perspective of protecting the conductive layer containing the silver nanowires, the protective layer is preferably provided adjacent to the conductive layer containing the silver nanowires.

[0149] [Resin composition for forming protective layer]

[0150] The protective layer forming resin composition is a composition containing a photopolymerization initiator and / or a thermal polymerization initiator, and a polymerizable monomer and / or a macromonomer. The protective layer forming resin composition may further contain a chelating agent, a weather resistance improving agent, a solvent, a curing aid, and other additives described later as needed. In the present invention, by using a protective layer forming resin composition containing a chelating agent specified in the present invention to form a protective layer of a conductive laminate containing silver nanowires, the particle formation of silver nanowires when an electric field is applied can be suppressed.

[0151] [Film formation of protective layer]

[0152] As a coating method for the protective layer-forming resin composition, a known coating method can be used. Specific examples of the coating method include spin coating, slit coating, dip coating, blade coating, rod coating, spray coating, relief printing, gravure printing, screen printing, lithographic printing, dispensing, and inkjet. In addition, these coating methods can be used repeatedly for multiple times.

[0153] [Content of Chelating Agent in Protective Layer]

[0154] By adding the chelating agent specified in the present invention to the conductive laminate containing silver nanowires, the particle formation of the silver nanowires can be suppressed when an electric field is applied. The more the amount of chelating agent used in the protective layer of the conductive laminate containing silver nanowires, the more the particle formation can be suppressed, so the chelating agent contained in the protective layer is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and further preferably 0.1% by mass or more, and particularly preferably 0.2% by mass or more. On the other hand, from the point of view of conductivity, it is believed that the amount of chelating agent used is preferably less. Thus, the amount of chelating agent contained in the protective layer is preferably 15% by mass or less, more preferably 7% by mass or less, and further preferably 5% by mass or less, and particularly preferably 2% by mass or less. The amount of chelating agent contained in the protective layer can be obtained by the amount of chelating agent relative to the amount of components contained in the resin composition for forming the protective layer, excluding the solvent.

[0155] [Photopolymerization initiator]

[0156] The photopolymerization initiator is not particularly limited, and can be a photopolymerization initiator obtained by a known method or a commercially available one. Specific examples of the photopolymerization initiator include: 1-hydroxycyclohexyl phenyl ketone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoylbenzoic acid, benzoylbenzoic acid methyl ester, 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone, xanthone, anthraquinone, 2-methylanthraquinone, etc. These can be used alone or in combination of two or more.

[0157] [Thermal polymerization initiator]

[0158] The thermal polymerization initiator is not particularly limited, and may be a thermal polymerization initiator obtained by a known method or a commercially available one. Specific examples of thermal polymerization initiators include: persulfates such as ammonium persulfate, sodium persulfate, and potassium persulfate; peroxides such as tert-butyl hydroperoxide, cumene hydroperoxide, benzoyl peroxide, and lauroyl peroxide; redox initiators formed by combining persulfates or peroxides with reducing agents such as sulfites, bisulfites, thiosulfates, sodium formaldehyde sulfoxylate, ferrous sulfate, ammonium ferrous sulfate, glucose, and ascorbic acid; azo compounds such as 2,2′-azobisisobutyronitrile, 2,2′-azobis(2,4-dimethylvaleronitrile), 2,2′-azobis(2-methylbutyronitrile), 2,2′-azobis(2-methylpropionic acid) dimethyl ester, and 2,2′-azobis(2-amidinopropane) dihydrochloride. These can be used alone or in combination of two or more.

[0159] [Polymerizable monomers and macromonomers]

[0160] As the polymerizable monomer and macromonomer, any monomer or macromonomer can be used without particular limitation as long as it is a monomer or macromonomer that undergoes polymerization reaction directly or under the action of an initiator when irradiated with visible light, ultraviolet rays, or ionizing radiation such as electron beams. Specific examples of polymerizable monomers having one polymerizable unsaturated group in one molecule include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, phenoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, methoxy-diethylene glycol (meth)acrylate, methoxy-triethylene glycol (meth)acrylate and the like (meth)acrylates; (meth)allyl compounds such as (meth)allyl alcohol and glycerol mono(meth)allyl ether; aromatic vinyls such as styrene, methylstyrene and butylstyrene; carboxylic acid vinyl esters such as vinyl acetate; (meth)acrylamides such as (meth)acrylamide, N-cyclohexyl (meth)acrylamide, N-phenyl (meth)acrylamide and N-(2-hydroxyethyl) (meth)acrylamide. In addition, specific examples of polymerizable monomers having two or more polymerizable unsaturated groups in one molecule include polyethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, di-trimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, alkyl-modified dipentaerythritol (meth)acrylate, ethylene oxide-modified bisphenol A di(meth)acrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, ethylene oxide-modified isocyanuric acid tri(meth)acrylate, etc. As specific examples of macromonomers, polymerizable urethane acrylate resins, polymerizable polyurethane resins, polymerizable acrylic resins, polymerizable epoxy resins, and polymerizable polyester resins having one or more polymerizable unsaturated groups per molecule can be used. These can be used alone or in combination of two or more.

[0161] [Weather resistance enhancer]

[0162] From the viewpoint of stability over time, the protective layer forming resin composition preferably contains a weather resistance improver. The weather resistance improver is a compound that functions to suppress the degradation of silver nanowires under the environment. Such weather resistance improvers can use known substances. Among them, it is preferably used in combination with a compound represented by the following general formula (13) or general formula (14), and more preferably used in combination with a compound selected from 2-mercaptothiazoline, 2-mercaptobenzothiazole, 2-mercaptobenzothiazole methyl ether, 3-(1,3-benzothiazol-2-ylthio) propionic acid, and (1,3-benzothiazol-2-ylthio) succinic acid.

[0163] [General formula (13)]

[0164] [Chemistry 11]

[0165]

[0166] (Wherein, in the general formula (13), R 14 represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a (di)carboxyalkyl group having an alkyl group having 1 to 3 carbon atoms)

[0167] [General formula (14)]

[0168] [Chemistry 12]

[0169]

[0170] (Wherein, in the general formula (14), R 15 represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a (di)carboxyalkyl group having an alkyl group having 1 to 3 carbon atoms)

[0171] [Solvent for protective layer forming resin composition]

[0172] The protective layer forming resin composition may further contain a solvent. The solvent may be a compound that dissolves other components in the resin composition and forms a uniform coating by evaporation during film formation. As a specific example of the solvent, water, methanol, ethanol, 1-propanol, 2-propanol, acetone, methyl ethyl ketone, toluene, n-hexane, n-butyl alcohol, diacetone alcohol, methyl isobutyl ketone, methyl butyl ketone, ethyl butyl ketone, cyclohexanone, ethyl acetate, butyl acetate, propylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, 1,3-butylene glycol diacetate, cyclohexanol acetate, propylene glycol diacetate, tetrahydrofurfuryl alcohol and N-methyl-2-pyrrolidone, etc., may be used alone or in combination.

[0173] [Hardening aid]

[0174] The protective layer forming resin composition may further contain a curing aid. The curing aid can be a compound having two or more reactive functional groups in one molecule. Specific examples of reactive functional groups include isocyanate groups, acrylic groups, methacrylic groups, mercapto groups, etc. These can be used alone or in combination of two or more.

[0175] [Other additives]

[0176] Various additives may be added to the protective layer forming resin composition within the range that does not hinder the effects of the present invention. Examples of additives include organic fine particles, flame retardants, flame retardant aids, oxidation stabilizers, leveling agents, lubricity imparting agents, antistatic agents, dyes, fillers, and the like.

[0177] The silver nanowire-containing conductor of the present invention or the silver nanowire-containing conductive laminate of the present invention can be widely used in various devices such as electrode materials for liquid crystal displays, electrode materials for plasma displays, electrode materials for organic electroluminescent displays, electrode materials for electronic paper, electrode materials for touch screens, electrode materials for thin-film amorphous Si solar cells, electrode materials for dye-sensitized solar cells, electromagnetic wave shielding materials, antistatic materials, etc.

[0178] Example

[0179] Hereinafter, the present invention will be described in detail based on examples, but the present invention is not limited to these examples.

[0180] In addition, the abbreviations of each drug in the table have the following meanings.

[0181] Phen: 1,10-phenanthroline monohydrate

[0182] Neoc: Neocuprous Reagent 0.5 Hydrate

[0183] Batho: Disodium phenanthroline disulfonate hydrate

[0184] bpy: 2,2′-bipyridine

[0185] 8-HQ: 8-Hydroxyquinoline

[0186] 8-AQ: 8-aminoquinoline

[0187] TBZ: 2-(4-thiazolyl)benzimidazole

[0188] HPBO: 2-(2-hydroxyphenyl)benzoxazole

[0189] box:2,2′-(2-bisoxazoline)

[0190] DAcPy: 2,6-diacetylpyridine

[0191] HEPy: 2-pyridineethanol

[0192] Im:imidazole

[0193] ImA: 4-imidazolecarboxylic acid

[0194] MBI: 2-Mercaptobenzimidazole

[0195] IPA: 2-propanol

[0196] HPMC-1: Hydroxypropyl methylcellulose (manufactured by Dow Chemical, Methocel 311)

[0197] HPMC-2: Hydroxypropyl methylcellulose (manufactured by Shin-Etsu Chemical Co., Ltd., Metolose (registered trademark) 60SH10000)

[0198] MBT: 2-Mercaptobenzothiazole

[0199] DETA: Diethylenetriamine

[0200] 4,4′-bpy: 4,4′-bipyridine

[0201] <Production of Silver Nanowires>

[0202] (Synthesis example 1)

[0203] While nitrogen was introduced into a four-necked flask equipped with a stirrer, a thermometer, and a nitrogen inlet tube, 666.97 parts by mass of a 1.0% by mass polyvinyl pyrrolidone (Sokalan (registered trademark) K90P manufactured by BASF) propylene glycol solution, 5.35 parts by mass of a 1.5% by mass sodium chloride propylene glycol solution, 1.87 parts by mass of a 2.2% by mass sodium bromide propylene glycol solution, and 162.95 parts by mass of propylene glycol were added, and stirred at room temperature for 30 minutes. Then, after the internal temperature was raised to 145° C., a solution in which 1.06 parts by mass of 2,5-dimethyl-4-hydroxy-3(2H)-furanone, 4.80 parts by mass of ion exchange water, and 30 parts by mass of propylene glycol were mixed and dissolved was added, and stirred for 10 minutes. Thereafter, while maintaining the internal temperature at 145° C., 127 parts by mass of a 5.5% by mass silver nitrate propylene glycol solution was added over 90 minutes, followed by stirring for 30 minutes. The obtained solution was then cooled to obtain a reaction solution containing silver nanowires.

[0204] [Preparation of Silver Nanowire Dispersion Liquid (a)]

[0205] 3000 parts by mass of water were added to 1000 parts by mass of the reaction solution containing silver nanowires for dilution, and suction filtration was performed using a membrane filter. Water was then added to the residue, and suction filtration was repeated 5 times, and water was added again, thereby obtaining a 0.15% by mass crude silver nanowire dispersion. The obtained crude silver nanowire dispersion was treated at a speed of 2000 rpm using a centrifugal separator for 10 minutes, and the remaining supernatant was collected to remove the silver nanowires with a relatively large diameter. The obtained supernatant was concentrated using a membrane filter to prepare a silver nanowire dispersion (a) with a content of 0.7% by mass. The obtained silver nanowires had an average major axis length of 12 μm and an average diameter of 25 nm.

[0206] [Stability test of silver nanowire dispersion]

[0207] Regarding the stability test of the silver nanowire dispersion, the stability can be evaluated by the following method, that is, the silver nanowire dispersion is allowed to stand at 40°C for 10 days, the haze of the diluted silver nanowire dispersion obtained is measured, and the haze increase rate compared with the silver nanowire dispersion just prepared is calculated. Specifically, the haze increase rate is given by the following formula (1). When the value of the haze increase rate is low, the generation of silver particles is suppressed due to the change over time, thereby indicating that the degree of deterioration of the optical properties is small. NDH5000 (manufactured by Nippon Denshoku Industries Co., Ltd.) was used in the measurement.

[0208] (H2-H1) / H1×100(%)…(1)

[0209] H1: Haze of the diluted silver nanowire dispersion immediately after preparation

[0210] H2: Haze of the diluted silver nanowire dispersion after standing at 40°C for 10 days

[0211] The haze increase rate is preferably less than 15%, more preferably less than 12%, further preferably less than 7%, and particularly preferably less than 4%.

[0212] (Example A-1)

[0213] In a plastic container, 7.14 parts by mass of a 0.7% silver nanowire dispersion (a), 0.10 parts by mass of a 5% polyvinyl pyrrolidone (Sokalan (registered trademark) K30P manufactured by BASF), 0.10 parts by mass of a 0.1% aqueous solution of 1,10-phenanthroline monohydrate, 0.10 parts by mass of ethanol, and 2.56 parts by mass of ion exchange water were added, and the container was covered with a lid and mixed with an oscillator for 5 minutes to prepare a 0.5% silver nanowire dispersion (A-1). The haze of the diluted solution of the prepared silver nanowire dispersion (A-1) was 2.27%. The prepared silver nanowire dispersion (A-1) was subjected to a stability test, and the results are shown in Table 1.

[0214] (Example A-2 to Example A-19, Comparative Example A-1 to Comparative Example A-8)

[0215] Examples A-2 to A-19 and Comparative Examples A-1 to A-8 were subjected to stability tests on silver nanowire dispersions in the same manner as in Example A-1 except that the conditions were changed as described in Table 1. The results are also described in Table 1. The amount of disodium bathophenanthroline disulfonate hydrate was calculated as a dihydrate.

[0216] [Table 1]

[0217]

[0218] (Example B-1)

[0219] [Preparation of a Conductor Containing Silver Nanowires]

[0220] In a plastic container, 5.71 parts by mass of a 0.7% silver nanowire dispersion (a), 2.40 parts by mass of a 0.5% aqueous solution of hydroxypropyl methylcellulose (Methocel 311, manufactured by Dow Chemical Co., Ltd.), 0.08 parts by mass of a 0.1% aqueous solution of 1,10-phenanthroline monohydrate, 9.81 parts by mass of ion-exchanged water, and 2.0 parts by mass of 2-propanol were placed, the container was covered with a lid, and mixed with an oscillator for 5 minutes to prepare a silver nanowire dispersion (B-1) having a silver nanowire concentration of 0.2%. The silver nanowire dispersion (B-1) was uniformly applied on a polyethylene terephthalate film (PET (polyethylene terephthalate) film, manufactured by Toray Co., Ltd., trade name "Lumirror U403") having a film thickness of 100 μm using a No. 7 wire rod, and dried for 2 minutes using a hot air convection dryer at 120° C. to prepare a conductor containing silver nanowires. The physical properties of the prepared conductor were measured, and the results are shown in Table 2.

[0221] (Example B-2 to Example B-11, Comparative Example B-1 to Comparative Example B-4)

[0222] Examples B-2 to B-11 and Comparative Examples B-1 to B-4 Silver nanowire-containing conductors were prepared and their physical properties were measured in the same manner as in Example B-1 except that the conditions were changed as described in Table 2. The results are also described in Table 2.

[0223] [Sheet resistance of a conductor containing silver nanowires]

[0224] The sheet resistance (Ω / □) of 9 different parts on the conductor containing silver nanowires was measured, and the average sheet resistance of the conductive layer in the conductor containing silver nanowires was calculated from the arithmetic mean value. In the determination of the sheet resistance, a non-contact surface resistivity meter EC-80P (manufactured by Napson) was used. Furthermore, in order to estimate the effect of the chelating agent on the sheet resistance, the sheet resistance change rate of the conductive layer of the conductor containing silver nanowires containing the chelating agent relative to the conductor containing silver nanowires without the chelating agent was calculated. The sheet resistance change rate is given by the following formula (2). A small value of the sheet resistance change rate indicates that the increase in sheet resistance caused by the chelating agent is suppressed.

[0225] (r2-r1) / r1×100(%)…(2)

[0226] r1: Average sheet resistance of the conductive layer in the conductor containing silver nanowires without chelating agent

[0227] r2: Average sheet resistance of the conductive layer in the conductor containing silver nanowires containing a chelating agent

[0228] The sheet resistance change rate is preferably less than 30%, more preferably less than 20%, further preferably less than 15%, and particularly preferably less than 10%.

[0229] [Total light transmittance of conductor containing silver nanowires]

[0230] The total light transmittance of the silver nanowire-containing conductor was measured using NDH5000 (manufactured by Nippon Denshoku Industries Co., Ltd.) and the difference between the total light transmittance of the silver nanowire-containing conductor and the substrate before coating was calculated by the following formula as Δ total light transmittance.

[0231] ΔTotal light transmittance (%) = Total light transmittance of the conductor containing silver nanowires - Total light transmittance of the substrate before coating

[0232] Here, the smaller the absolute value of Δ total light transmittance is, the better it is. The absolute value of Δ total light transmittance is preferably 10% or less, and more preferably 5% or less.

[0233] [Haze of Conductor Containing Silver Nanowires]

[0234] The haze of the silver nanowire-containing conductor was measured using NDH5000 (manufactured by Nippon Denshoku Industries Co., Ltd.) and the difference in haze between the silver nanowire-containing conductor and the substrate before coating was calculated by the following formula as Δ haze.

[0235] ΔHaze (%) = Haze of conductor containing silver nanowires - Haze of substrate before coating

[0236] Here, a smaller ΔHaze value indicates a more excellent property, and the ΔHaze value is preferably 3.0% or less, more preferably 1.5% or less, and still more preferably 1.0% or less.

[0237] [Table 2]

[0238]

[0239] (Example C-1)

[0240] [Preparation of silver nanowire dispersion]

[0241] In a plastic container, 3.43 parts by mass of a 0.7% silver nanowire dispersion (a), 1.20 parts by mass of a 0.5% aqueous solution of hydroxypropylmethylcellulose (Methocel 311, manufactured by Dow Chemical Co., Ltd.), 3.87 parts by mass of ion-exchanged water, and 1.5 parts by mass of 2-propanol were placed, and then the container was covered with a lid and mixed with an oscillator for 5 minutes to prepare a silver nanowire dispersion (C-1a) having a silver nanowire concentration of 0.24% by mass.

[0242] [Preparation of Conductor Containing Silver Nanowires]

[0243] The silver nanowire dispersion (C-1a) was evenly coated on a polyethylene terephthalate film (PET film, manufactured by Toray Co., Ltd., trade name "Lumirror U403") having a film thickness of 100 μm using a No. 7 wire rod, and dried for 2 minutes using a hot air convection dryer at 120° C. to prepare a conductor (C-1b) containing silver nanowires.

[0244] [Preparation of resin composition for forming protective layer]

[0245] In a four-necked flask, 15 parts by mass of dipentaerythritol hexaacrylate as a polymerizable monomer and a macromonomer, 5 parts by mass of trimethylolpropane triacrylate, 0.8 parts by mass of 1-hydroxycyclohexyl phenyl ketone as a polymerization initiator, 0.042 parts by mass of 1,10-phenanthroline monohydrate, and 80 parts by mass of propylene glycol monomethyl ether as a solvent were placed, and then stirred until a uniform solution was obtained, thereby preparing a resin composition for forming a protective layer (C-1c).

[0246] [Formation of Conductive Laminated Body Containing Silver Nanowires]

[0247] The protective layer-forming resin composition (C-1c) was diluted to 4 times with propylene glycol monomethyl ether and uniformly applied on the silver nanowire-containing conductor (C-1b) by spin coating (4000 rpm for 30 seconds). After drying for 2 minutes in a hot air convection dryer at 80° C., an ultraviolet irradiation device UV1501C-SZ (manufactured by SEN ENGINEERING Co., Ltd.) was used on a PET substrate at 500 mJ / cm from above. 2 The conductive laminate (C-1d) containing silver nanowires was obtained by irradiating ultraviolet light under the conditions of , thereby forming a protective layer for the silver nanowire layer. The amount of the chelating agent contained in the protective layer prepared using the protective layer forming resin composition (C-1c) was 0.042 / (15+5+0.8+0.042)×100=0.2 mass %.

[0248] [Electric field application high temperature and high humidity test]

[0249] The produced conductive laminate containing silver nanowires was cut into a size of 3 cm in length and 10 cm in width, and a non-conductive portion of about 30 μm in width was formed at a position of 5 cm in width by a cutter. Next, the remaining single-side separator of the glass substrate (manufactured by ASONE Co., Ltd., a slide glass made of sodium glass) was peeled off after peeling off the separator on one side for the optical elastic resin (manufactured by 3M Co., Ltd., trade name 8146-2, film thickness 50 μm), and the conductive laminate containing silver nanowires was laminated in such a manner that the optical elastic resin was arranged on the upper surface of the conductive laminate containing silver nanowires and the two ends of the conductive laminate containing silver nanowires were exposed, thereby obtaining a sample sheet in which the conductive laminate containing silver nanowires, the optical elastic resin, and the glass were sequentially laminated on the PET film. Next, the non-conductive portion of the sample sheet was clamped by a tester, and it was confirmed that no current flowed at both ends. Thereafter, the non-conductive part of the sample piece was clamped and three single triple batteries were connected in series at both ends. In the above state, a constant temperature and humidity tester (manufactured by ISUZU, TPAV-48-20) was used to stand for 10 hours in an environment of 85°C and 85% RH, thereby applying an electric field, high temperature and high humidity test. The sample piece after the test was observed using a dark field microscope (trade name: BX51, manufactured by Olympus (Olympus) (stock)), and it can be confirmed that the part where the silver nanowires disappeared from the non-conductive part was particle-formed toward the positive electrode side of the battery. The distance from the area where the silver nanowires disappeared to the non-conductive part was measured at equal intervals for 9 points, and the average value was calculated as the average value of the particle distance. The results are shown in Table 3. Here, the smaller the average value of the particle distance, the better it is, preferably 220 mm or less, more preferably 200 mm or less, and more preferably 175 mm or less.

[0250] (Example C-2 to Example C-9, Comparative Examples C-1 to C-4)

[0251] In Examples C-2 to C-9 and Comparative Examples C-1 to C-4, except that the conditions were changed as described in Table 3, conductive laminates containing silver nanowires were prepared in the same manner as in Example C-1, and physical properties were measured. The results are also described in Table 3.

[0252] [Table 3]

[0253]

[0254] It is understood that since Examples A-1 to A-19 contain a certain amount or more of the chelating agent specified in the present invention, the increase in haze due to the change over time can be suppressed compared to Comparative Example 1 which does not contain a chelating agent.

[0255] On the other hand, it is found that in Comparative Example A-2 using 2,6-diacetylpyridine exemplified as a pyridine-ketone compound in Patent Document 2, Comparative Example A-3 using 4-imidazolecarboxylic acid exemplified as a heterocyclic compound having a specific interaction potential in Patent Document 3, and Comparative Examples A-4 to A-7 using heterocyclic compounds different in structure from those specified in the present invention, the effect of suppressing the increase in haze due to time-dependent changes is insufficient compared to Examples A-1 to A-19 containing the chelating agent specified in the present invention.

[0256] It can be seen that, compared with Examples A-1 to A-6, A-18, and A-19, since the amount of the chelating agent contained in the silver nanowire dispersion relative to the silver nanowires is outside the range specified in the present invention, the effect of suppressing the increase in haze caused by the change over time is insufficient in Comparative Example A-8.

[0257] It is found that in Examples A-1 to A-6 and A-19, the amount of the chelating agent contained in the silver nanowire dispersion relative to the silver nanowires is within a more preferred range than in Example A-18, and thus an increase in haze can be further suppressed.

[0258] It can be seen that Examples B-1 to B-11 contain the chelating agent specified in the present invention in an amount below the specified amount, and therefore show the same sheet resistance value as Comparative Examples B-1 and B-3 that do not contain the chelating agent with the same silver nanowire content, and have little adverse effect on conductivity. However, in Comparative Example B-2 using more than the specified amount, it was confirmed that the sheet resistance increased significantly compared with Comparative Example B-1. From this, it can be seen that the chelating agent specified in the present invention needs to be used in an amount below the specified amount.

[0259] On the other hand, Comparative Example B-4 using 2-mercaptobenzimidazole exemplified as a heterocyclic compound having a specific interaction potential in Patent Document 3 showed a significantly increased sheet resistance compared with Comparative Example B-3, significantly adversely affecting conductivity and thus cannot be preferably used.

[0260] It is understood that since Examples C-1 to C-9 contain the chelating agent specified in the present invention, the particle region during electric field application becomes smaller and the tolerance is improved compared with Comparative Example C-1 which does not contain the chelating agent specified in the present invention.

[0261] On the other hand, it can be seen that in Comparative Examples C-2 to C-4 using compounds with structures different from those specified in the present invention, there is almost no effect of reducing the particle area when an electric field is applied compared to Comparative Example C-1, and the effect of suppressing degradation when an electric field is applied is limited.

Claims

1. A silver nanowire dispersion, comprising silver nanowires, a dispersion solvent and a chelating agent, wherein the average diameter of the silver nanowires is less than 100 nm, the silver nanowire dispersion is characterized in that the chelating agent is contained in an amount of 1 μmol / g to 300 μmol / g relative to the content of the silver nanowires, and the chelating agent is an aromatic heterocyclic compound having at least one imine skeleton in the molecule selected from 1,10-phenanthroline, quinoline substituted with a hydroxyl group or an amino group at the 8th position, 2,2'-bipyridine, and biazole, wherein: The azole is any one of imidazole, thiazole, oxazole, or at least one of the group of derivatives thereof, The dispersion solvent contains any one of water and a monohydric alcohol having 1 to 3 carbon atoms, and the content of water or the monohydric alcohol having 1 to 3 carbon atoms in the dispersion solvent is 85% by mass or more.

2. The silver nanowire dispersion according to claim 1, wherein The chelating agent is at least one selected from the group consisting of general formula (1) to general formula (4), General formula (1) In the general formula (1), L represents a hydroxyl group or an amino group, and R 1 ~R 4 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, or a halogen group, and R 2 , R 3 At least one of them is hydrogen, R 1 ~R 4 At least two of them are hydrogen, General formula (2) Among them, in the general formula (2), R 5 , R 6 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, or a halogen group, and R 7 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, a phenyl group, a C6H4SO3Na group, or a halogen group, and R 5 ~R 7 At least one of is hydrogen, General formula (3) Among them, in the general formula (3), R 8 , R 9 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, or a halogen group, and R 10 represents hydrogen, an alkyl group having 1 to 4 carbon atoms, or a halogen group, and R 8 ~R 10 At least two of them are hydrogen, General formula (4) WITH 1 -WITH 2 Among them, in the general formula (4), Z 1 , Z 2 Each independently represents any one of the nitrogen-containing heterocyclic rings represented by the general formula (5) or the general formula (6), General formula (5) Among them, in the general formula (5), X 1 represents any one of NH, O, and S, and R 11 , R 12 represents hydrogen, a straight-chain alkyl group having 1 to 4 carbon atoms, a halogen group, or a benzene ring formed together; the arrow represents the Z 1 or Z 2 A single key, General formula (6) Among them, in the general formula (6), X 2 represents any one of NH, O, and S, and R 13 represents hydrogen, a linear alkyl group having 1 to 4 carbon atoms, or a halogen group, and the arrow represents a 1 or Z 2 single key.

3. The silver nanowire dispersion according to claim 1, wherein The chelating agent is at least one selected from the group consisting of 1,10-phenanthroline, neocuprous reagent, bathophenanthroline or sodium sulfonate thereof, 2,2'-bipyridine, 8-hydroxyquinoline, 8-aminoquinoline, and 2-(4-thiazolyl)benzimidazole.

4. The silver nanowire dispersion according to claim 1, wherein The average diameter of the silver nanowires is less than 30 nm.

5. The silver nanowire dispersion according to claim 1, wherein The concentration of the silver nanowires is 0.01 mass % to 3 mass %. 6 . The silver nanowire dispersion according to claim 1 , further comprising a polymer compound selected from polymers having amide bonds or polysaccharides, wherein the concentration of the polymer compound is 0.02 mass % to 1 mass %.

7. The silver nanowire dispersion according to claim 1, wherein The haze increase rate calculated by the following (1) in the stability test of the silver nanowire dispersion is less than 15%, (H2-H1) / H1×100(%)…(1) H1: Haze of the diluted silver nanowire dispersion immediately after preparation H2: haze of the diluted silver nanowire dispersion after standing at 40°C for 10 days.

8. A conductor containing silver nanowires, comprising a substrate and at least one conductive layer containing silver nanowires, characterized in that: Furthermore, the conductive layer contains 1 μmol / g to 300 μmol / g of a chelating agent relative to the content of silver nanowires. The chelating agent is an aromatic heterocyclic compound having at least one imine skeleton in the molecule and is selected from 1,10-phenanthroline, quinoline substituted with a hydroxyl group or an amino group at the 8-position, 2,2'-bipyridine, and biazole, wherein the azole is any one of imidazole, thiazole, oxazole, or at least one of the group of derivatives thereof.

9. The silver nanowire-containing conductor according to claim 8, wherein: The sheet resistance of the conductive layer is 1 Ω / □ to 100 Ω / □. 10 . The silver nanowire-containing conductor according to claim 8 , wherein the Δ haze is less than 1.5%.

11. A conductive laminate containing silver nanowires, comprising a substrate, a conductive layer containing silver nanowires, and a protective layer containing a chelating agent, characterized in that: The chelating agent is an aromatic heterocyclic compound having at least one imine skeleton in the molecule and is selected from 1,10-phenanthroline, quinoline substituted with hydroxyl or amino at the 8-position, 2,2'-bipyridine, and biazole, wherein the azole is any one of imidazole, thiazole, oxazole, or at least one of the group of derivatives thereof.

12. The conductive laminate containing silver nanowires according to claim 11, wherein The protective layer contains 0.05 to 5% by mass of the chelating agent.