A method for preparing a fan-shaped rutile titanium dioxide composite material with antioxidant properties

By combining an organic titanium source with caffeic acid under mild conditions, needle-like nanocrystalline titanium dioxide with smaller particle size is prepared, which solves the problem of insufficient UVA and UVB shielding performance of nanotitanium dioxide and achieves excellent UVA and UVB shielding. Effectiveness and free radical scavenging ability, suitable for sunscreen cosmetics.

CN115998627BActive Publication Date: 2024-10-11CHANGZHOU NANO-MATERIALS S&T CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211734736.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-31
Publication Date
2024-10-11
Estimated Expiration
2042-12-31

AI Technical Summary

Technical Problem

Existing nano-titanium dioxide has insufficient UVA and UVB shielding performance in the field of sun protection, and organic sunscreens can easily cause skin irritation and allergies, and it is difficult to simultaneously optimize the UVA and UVB shielding effects by controlling the particle size of nano-titanium dioxide.

Method used

A method for preparing fan-shaped rutile titanium dioxide composite materials with antioxidant effect is adopted. By combining an organic titanium source with caffeic acid under mild conditions, and controlling the reaction conditions and pH value, needle-like nanocrystalline titanium dioxide with smaller particle size is prepared. Combined with the antioxidant and UV-absorbing properties of caffeic acid, it achieves excellent UVA and UVB shielding.

Benefits of technology

A nano-titanium dioxide composite material that is low-cost and easy to be industrially produced has been realized. It has excellent free radical scavenging ability and good shielding properties for both UVA and UVB, and improves the dispersion and compatibility of sunscreen cosmetics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115998627B_ABST
    Figure CN115998627B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of preparation of protective functional materials, and specifically relates to a method for preparing a fan-shaped rutile titanium dioxide composite material with antioxidant effect. The present invention prepares a novel fan-shaped rutile titanium dioxide under relatively mild process conditions by controlling reaction process conditions and adding caffeic acid, a natural plant extract component. The fan-shaped titanium dioxide / caffeic acid novel composite material prepared by the present invention has the ability to scavenge ROS free radicals, and has excellent shielding performance against both UVA and UVB.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of protective functional materials, and in particular relates to a method for preparing a fan-shaped rutile titanium dioxide composite material with antioxidant effect. Background Art

[0002] Skin is the first interface between the human body and its environment, that is, the interface between external and internal aggressions. Various environmental factors such as solar ultraviolet rays, visible light, and environmental pollution increase the production of reactive oxygen free radicals (ROS) in the skin. Excessive ROS will directly cause oxidative stress, damage mitochondrial DNA, protein composition, and telomerase, and accelerate skin aging. Therefore, sunscreen should not only have excellent attenuation effect on ultraviolet rays, but also have good free radical scavenging ability. Organic sunscreens have good sunscreen effects, but they are prone to cause skin irritation, allergies, inflammation and other side effects. In recent years, nano-titanium dioxide (TiO2) has become recognized as one of the most promising functional materials in the field of ultraviolet shielding due to its high refractive index, environmental friendliness and low cost. Studies have found that as the particle size of nano-titanium dioxide decreases, its performance in shielding medium-wave ultraviolet rays (UVB) becomes better, while its performance in shielding long-wave ultraviolet rays (UVA) becomes worse; as the particle size of nano-titanium dioxide increases, its performance in shielding UVA becomes better, while its performance in shielding UVB becomes worse. Researching and developing titanium dioxide with excellent shielding properties against both UVA and UVB is a difficult problem that needs to be solved urgently.

[0003] Caffeic acid (3,4-dihydroxycinnamic acid) is found in coffee, honey, potatoes, berries, herbs and vegetables (such as olives, beets and carrots). Studies have shown that caffeic acid not only has antioxidant capacity, but also has UV protection, immunomodulatory, antibacterial, neuroprotective, anti-anxiety and anti-inflammatory activities. At present, there are few reports on the use of caffeic acid in the synthesis and surface modification of nano-titanium dioxide. Summary of the invention

[0004] In view of the problems in the background technology of the harm of reactive oxygen free radicals ROS to the human body, the harm caused by nano-titanium dioxide penetrating the skin to the human body and the insufficient ultraviolet shielding performance of titanium dioxide, the purpose of the present invention is to provide a method for preparing a fan-shaped rutile titanium dioxide composite material with antioxidant effect, which method has the characteristics of low cost and simplicity.

[0005] The technical solution adopted by the present invention is:

[0006] A method for preparing a fan-shaped rutile titanium dioxide composite material with antioxidant effect comprises the following steps:

[0007] 1. Add the organic titanium source dropwise into a certain amount of deionized water at a temperature of 25 to 60°C with stirring, and keep warm and stir for 0.5 to 2 hours, perform solid-liquid separation, and wash to obtain a titanium dioxide precursor filter cake.

[0008] 2. Add concentrated hydrochloric acid and deionized water to the filter cake obtained in step 1 to prepare a dispersion of 0.5-2 mol / L titanium dioxide and 2-4 mol / L hydrochloric acid, and react at 30-50° C. for 2-6 hours; heat to 80-100° C., add caffeic acid, and stir at this temperature for 4-10 hours; add an alkaline solution to adjust the pH to 5-7, and continue to react at 80-100° C. for 1-3 hours.

[0009] 3. The dispersion obtained in step 2 is subjected to solid-liquid separation, washing, and drying to obtain a fan-shaped rutile titanium dioxide composite material with antioxidant effect.

[0010] Furthermore, the organic titanium source described in step 1 includes titanium ethylene glycol, titanium isopropoxide, propyl titanate, tetraisobutyl titanate, and tetrabutyl titanate, and the preferred titanium sources are titanium isopropoxide and tetraisobutyl titanate.

[0011] Furthermore, the molar ratio of the organic titanium source in step 1 to deionized water is 1:8 to 1:15.

[0012] Furthermore, the mass ratio of the caffeic acid in step 2 to the titanium dioxide in the dispersion is 0.01 to 0.1:1.

[0013] Further, the alkaline solution described in step 2 is one of sodium hydroxide, potassium hydroxide, ammonia water, sodium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium carbonate and ammonium bicarbonate.

[0014] Beneficial effects of the present invention:

[0015] 1. The present invention prepares a novel fan-shaped rutile titanium dioxide under relatively mild process conditions by controlling reaction process conditions and adding caffeic acid, a natural plant extract ingredient. The raw material source is green, the cost is low, and it is easy to industrialize and mass-produce.

[0016] 2. Caffeic acid can not only regulate the morphology of titanium dioxide, but also play a role in surface modification of titanium dioxide, which can improve the dispersibility and compatibility of titanium dioxide in sunscreen cosmetics.

[0017] 3. The present invention prepares a new type of fan-shaped titanium dioxide / caffeic acid composite material, which has the ability to scavenge ROS free radicals. In addition, caffeic acid has a certain ultraviolet absorption performance, and caffeic acid and titanium dioxide can play a synergistic effect of shielding ultraviolet rays.

[0018] 3. The fan-shaped titanium dioxide synthesized in the present invention is formed by the aggregation of needle-shaped nanocrystals with smaller particle sizes, and has excellent shielding performance against both UVA and UVB. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a TEM photo of the product obtained in Example 1;

[0020] Figure 2 This is a TEM photo of the product obtained in Example 2;

[0021] Figure 3 This is a TEM photo of the product obtained in Example 3;

[0022] Figure 4 This is a TEM photo of the product obtained in Comparative Example 1;

[0023] Figure 5 The X-ray diffraction patterns of the products obtained in Examples 1 to 3 and Comparative Example 1 are as follows;

[0024] Figure 6 This is the infrared spectrum of Example 2. DETAILED DESCRIPTION

[0025] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.

[0026] Example 1

[0027] 506g of titanium isopropoxide was added dropwise to 288g of deionized water at 25°C with stirring, and the mixture was stirred for 0.5h, filtered, and washed with deionized water to obtain a titanium dioxide precursor filter cake. Concentrated hydrochloric acid and deionized water were added to the filter cake to prepare 800mL of a dispersion with a titanium dioxide concentration of 0.5mol / L and a hydrochloric acid concentration of 2mol / L, and the mixture was reacted at 30°C for 6h; the mixture was heated to 80°C, 3.20g of caffeic acid was added, and the mixture was stirred for 4h; 2mol / L of sodium hydroxide solution was added to adjust the pH to 5, and the reaction was continued at 100°C for 1h. The dispersion was filtered, washed with deionized water, and dried at 80°C to obtain fan-shaped rutile titanium dioxide.

[0028] Example 2

[0029] 680g of tetraisobutyl titanate was added dropwise to 360g of deionized water at 40℃ and stirred, and the mixture was stirred for 1h, filtered, and washed with deionized water to obtain a titanium dioxide precursor filter cake. Concentrated hydrochloric acid and deionized water were added to the filter cake to prepare 1200mL of a dispersion with a titanium dioxide concentration of 1mol / L and a hydrochloric acid concentration of 3mol / L, and the mixture was reacted at 40℃ for 4h; the mixture was heated to 90℃, 2.88g of caffeic acid was added, and the mixture was stirred for 6h; 1mol / L sodium carbonate solution was added to adjust the pH to 7, and the mixture was reacted at 90℃ for 2.5h. The dispersion was filtered, washed with deionized water, and dried at 90℃ to obtain fan-shaped rutile titanium dioxide.

[0030] Example 3

[0031] 568g of titanate propyl was added dropwise to 540g of deionized water at 60℃ and stirred, and the mixture was stirred for 2h. The mixture was separated into solid and liquid, filtered, and washed with deionized water to obtain a titanium dioxide precursor filter cake. Concentrated hydrochloric acid and deionized water were added to the filter cake to prepare 700mL of a dispersion with a titanium dioxide concentration of 2mol / L and a hydrochloric acid concentration of 4mol / L. The mixture was reacted at 50℃ for 2h. The mixture was heated to 100℃, 1.12g of caffeic acid was added, and the mixture was stirred for 10h. A 3mol / L potassium hydroxide solution was added to adjust the pH to 6, and the mixture was reacted at 80℃ for 3h. The dispersion was filtered, washed with deionized water, and dried at 120℃ to obtain fan-shaped rutile titanium dioxide.

[0032] Comparative Example 1

[0033] 680g of tetraisobutyl titanate was added dropwise to 360g of deionized water at 40°C with stirring, and the mixture was stirred for 1h, filtered, and washed with deionized water to obtain a titanium dioxide precursor filter cake. Concentrated hydrochloric acid and deionized water were added to the filter cake to prepare 1200mL of a dispersion with a titanium dioxide concentration of 1mol / L and a hydrochloric acid concentration of 3mol / L, and the mixture was reacted at 40°C for 4h; the mixture was heated to 90°C and stirred for 6h; 1mol / L sodium carbonate solution was added to adjust the pH to 7, and the mixture was reacted at 90°C for 2.5h. The dispersion was filtered, washed with deionized water, and dried at 90°C to obtain a long strip of rutile nano-titanium dioxide.

[0034] Simulate sunscreen sun protection factor test

[0035] The sunscreen performance analyzer (UV-2000S, Lanfei Company, USA) was used to analyze and test the sun protection index of the prepared composite material. 0.2g sample (sunscreen) and 1.8g vaseline were ground evenly in a mortar until there was no particle, which was used as a simulated sunscreen. According to the Colipa standard, 32.5mg sunscreen was accurately weighed and evenly dispersed on a clean PMMA board. The sunscreen was evenly applied to the entire sample board using a latex finger cot, and the SPF value and PFA value of the sample were tested. The SPF value reflects the protective effect against medium-wave ultraviolet rays (UVB), and the PFA value reflects the protective effect against long-wave ultraviolet rays (UVA). The larger the value, the better the protective effect. As can be seen from Table 1, this product has a good shielding effect on long-wave ultraviolet rays (UVA) and medium-wave ultraviolet rays (UVB).

[0036] Table 1 Sunscreen performance test of different embodiments and comparative examples

[0037]

[0038] Antioxidant activity test - DPPH free radical scavenging test: Take a certain amount of DPPH, prepare it into 0.2mmol / L DPPH solution with anhydrous ethanol, take 2mL of solution with different concentrations (2, 4, 6, 8, 10mg / mL), mix them evenly, leave them at room temperature for 30min, centrifuge them at 5000r / min for 10min, take the supernatant and measure the absorbance at 517nm, use VC as positive control, and calculate the scavenging rate of the sample for DPPH free radicals using the following formula:

[0039]

[0040] Where: A0 is the absorbance of 2ml anhydrous ethanol + 2ml DPPH solution;

[0041] A1: absorbance of 2ml sample solution + 2ml DPPH;

[0042] A2: absorbance of 2ml sample solution + 2ml anhydrous ethanol.

[0043] Table 2 DPPH free radical scavenging rate of different embodiments and comparative examples

[0044]

[0045] Combining Example 2 and Figure 6 This shows the presence of titanium dioxide and caffeic acid in the composite material prepared by the method of the present invention. It can be seen from Examples 1, 2, 3 and Comparative Example 1 that the fan-shaped titanium dioxide composite material prepared by the method of the present invention has a certain free radical scavenging ability (antioxidation). Comparative Example 1 does not add caffeic acid, not only can the fan-shaped titanium dioxide not be obtained, but also no antioxidant property is shown.

Claims

1. A method for preparing a fan-shaped rutile titanium dioxide composite material with antioxidant effect, characterized in that: The steps include: (1) adding an organic titanium source dropwise into deionized water at a temperature of 25 to 60°C with stirring, and keeping the mixture warm and stirring for 0.5 to 2 hours, performing solid-liquid separation, and washing to obtain a titanium dioxide precursor filter cake; (2) Add concentrated hydrochloric acid and deionized water to the filter cake obtained in step (1) to prepare a dispersion of 0.5-2 mol / L titanium dioxide and 2-4 mol / L hydrochloric acid, and react at 30-50°C for 2-6 hours; heat to 80-100°C, add caffeic acid, and stir at this temperature for 4-10 hours; add an alkaline solution to adjust the pH to 5-7, and continue to react at 80-100°C for 1-3 hours; (3) subjecting the dispersion obtained in step (2) to solid-liquid separation, washing, and drying to obtain a fan-shaped rutile titanium dioxide composite material with antioxidant effect; The organic titanium source described in step (1) is selected from one of titanium isopropoxide, propyl titanate, and tetraisobutyl titanate; and the mass ratio of caffeic acid to titanium dioxide described in step (2) is 0.01-0.1:

1.

2. The method for preparing the fan-shaped rutile titanium dioxide composite material with antioxidant effect as claimed in claim 1, characterized in that: The organic titanium source in step (1) is selected from titanium isopropoxide or tetraisobutyl titanate.

3. The method for preparing the fan-shaped rutile titanium dioxide composite material with antioxidant effect as claimed in claim 1, characterized in that: The molar ratio of the organic titanium source to deionized water in step (1) is 1:8 to 1:

15.

4. The method for preparing the fan-shaped rutile titanium dioxide composite material with antioxidant effect as claimed in claim 1, characterized in that: The alkaline solution in step (2) is one of sodium hydroxide, potassium hydroxide, ammonia water, sodium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium carbonate and ammonium bicarbonate.