A method for extracting potassium salt from biomass fly ash
Extracting high-purity potassium salt from biomass fly ash through crushing and recycling processes solves the problems of low water saving efficiency and environmental pollution in the existing technology, and achieves efficient and low-cost potassium salt extraction and biomass fly ash extraction. Comprehensive utilization, the products comply with national standards and have significant environmental protection and economic benefits.
Patent Information
- Application Number
- CN202111234609.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-22
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-10-22
AI Technical Summary
The existing technology has problems of low water saving efficiency, high production cost and environmental pollution when extracting potassium salt from biomass fly ash, and fails to effectively utilize the potassium resources in biomass fly ash.
By crushing biomass fly ash and mixing it with water, repeating the solid-liquid separation step, adding calcium chloride or potassium sulfate, heating and stirring, combined with the recycling process of plate and frame filter press, gradually extract high-purity potassium salt, and The by-produced calcium sulfate or calcium carbonate is used in industries such as building materials.
It achieves high-efficiency, water-saving and low-cost potassium salt extraction, reduces the accumulation and pollution of biomass fly ash, and improves the comprehensive utilization rate of biomass fly ash. The product complies with national standards and has environmental protection and economic benefits.
Smart Images

Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The present invention relates to a method for extracting potassium salt, in particular to a method for extracting potassium salt from biomass fly ash. Background Art
[0002] In recent years, with the rapid development of biomass power generation technology in my country, the production of biomass ash, a byproduct of power generation, has increased significantly year by year. If this biomass ash is not promptly processed, it will lead to accumulation and management pressures, polluting the environment and wasting resources. Furthermore, operating costs and fuel supply costs for a biomass power plant in China account for the majority of the plant's revenue. Biomass generally contains 3-20% ash, of which biomass fly ash contains various nutrients essential for plant growth, with potassium being the most abundant, with an average (K2O) content of approximately 5% to 12%. This makes it a valuable potassium resource, but direct application to crops is ineffective. Extracting high-purity potassium for use in potash fertilizer could significantly increase its fertility.
[0003] So far, potassium salts are usually obtained from biomass fly ash by leaching, evaporation, concentration and crystallization. However, this method wastes a lot of water and is an inefficient intermittent production method. Therefore, it is very necessary to find a water-saving and efficient potassium extraction process. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to overcome the above-mentioned shortcomings of the existing technology and provide a method for extracting high-purity potassium salt from biomass fly ash that effectively saves water, has simple process conditions, is energy-efficient and environmentally friendly, and has low production costs. This method can effectively solve the comprehensive problems of biomass fly ash accumulation and environmental pollution, thereby improving the comprehensive utilization rate of biomass fly ash. The by-product calcium sulfate or calcium carbonate can be used in construction materials, plaster bandages, chalk, papermaking, and other industries.
[0005] The technical solution adopted by the present invention to solve the technical problem is a method for extracting potassium salt from biomass fly ash, comprising the following steps:
[0006] (1) Grinding biomass fly ash to obtain raw material A;
[0007] (2) mixing the raw material A obtained in step (1) with water, stirring, and performing solid-liquid separation, and repeating this step 10 to 20 times to obtain a high-concentration potassium salt solution B and a filter residue C;
[0008] (3) heating the high-concentration potassium salt solution B obtained in step (2), adding the raw material A obtained in step (1) and stirring, and performing solid-liquid separation, and repeating this step 10 to 20 times to obtain a high-concentration potassium salt solution C and a filter residue D;
[0009] (4) adding calcium chloride or potassium sulfate to the high-concentration potassium salt solution C obtained in step (3), stirring, and solid-liquid separation to obtain a high-concentration potassium salt solution D and a product of calcium sulfate or calcium carbonate;
[0010] (5) stirring the high-concentration potassium salt solution D obtained in step (4), cooling it, allowing it to stand, and then subjecting it to solid-liquid separation to obtain a high-concentration potassium salt solution E and a high-purity potassium salt product;
[0011] (6) The high-concentration potassium salt solution E obtained in step (5) has a similar composition to the high-concentration potassium salt solution B, and the high-concentration potassium salt solution E obtained in step (5) is repeated with steps (3) to (5) (preferably once);
[0012] (7) Mixing the filter residue C obtained in step (2) and the filter residue D obtained in step (3) to obtain a filter residue E, adding water to the filter residue E, stirring, and performing solid-liquid separation to obtain a filtrate F and a water-containing filter residue F;
[0013] (8) passing the aqueous filter residue F obtained in step (7) through a plate and frame filter press to obtain aqueous filter residue G and filtrate G;
[0014] (9) The filtrate F obtained in step (7) and the filtrate G obtained in step (8) are mixed and used as the feed liquid for step (3) and recycled.
[0015] Furthermore, in step (1), the mass fraction of K2O in the biomass fly ash is 1.8-35.4%, and the mass fraction of CaO is 6-35%.
[0016] Furthermore, in step (1), the pulverization is to pulverize the biomass fly ash into a particle size of 5 to 15 mm, preferably 8 to 10 mm. If the particle size is too large, it is not conducive to the leaching of potassium in the biomass fly ash, and the stirring intensity and time need to be increased, which increases the production load and time. If the particle size is too small, the pulverization cost is increased, but the purification effect is not greatly improved.
[0017] Furthermore, in step (2), the water is tap water at a temperature of 15-30°C, preferably 20-25°C; the stirring time is 0.5-2 hours, and the stirring speed is 250-500 r / min. The stirring time and speed are determined by the mass ratio of raw material A to water and the particle size of raw material A.
[0018] Furthermore, in step (2), the mass ratio of water to raw material A is M, M = 0.3 to 3.0, preferably M = 0.5 to 1.0. If the mass ratio of water to raw material A is too low, the water will be absorbed by raw material A during the stirring process, and a fluid mixed solution cannot be formed, which is not conducive to subsequent production; if the mass ratio of water to raw material A is too high, step (2) needs to be repeated multiple times, which prolongs the production time and reduces production efficiency.
[0019] Furthermore, in step (3), the heating is to a temperature of 50°C to 99°C, preferably 60°C to 80°C; the stirring time is 0.5 to 2 hours, preferably 0.5 to 1 hour; and the stirring speed is 250 to 500 r / min, preferably 350 to 450 r / min.
[0020] Furthermore, in step (3), the mass ratio of the high-concentration potassium salt solution B to the raw material A is N, N = 0.3 to 2.0, preferably N = 0.5 to 1.5. If the mass ratio is too low, the high-concentration potassium salt solution B will be absorbed by the raw material A during the stirring process, and a fluid mixed solution cannot be formed, which is not conducive to subsequent production; if the mass ratio of the high-concentration potassium salt solution B to the raw material A is too high, step (3) needs to be repeated multiple times, which prolongs the production time and reduces production efficiency.
[0021] Furthermore, in step (4), the specific process includes: first analyzing and detecting the concentrations of calcium ions and carbonate ions or calcium ions and sulfate ions in the high-concentration potassium salt solution C, adding calcium chloride or potassium sulfate in a molar equivalent amount required to complete the reaction with the calcium ions according to reaction formula (4-1) or (4-2), stirring until the reaction is complete, and separating the calcium carbonate or calcium sulfate from the solid-liquid to obtain a high-concentration potassium salt solution D.
[0022] Ca 2+ +CO3 2- →CaCO3↓ (4-1)
[0023] Ca 2+ +SO4 2- →CaSO4↓ (4-2)
[0024] Furthermore, in steps (2) to (5), due to the differences in elements contained in the biomass, the high-concentration potassium salt solutions B, C, D, and E are one of high-concentration potassium chloride solutions, high-concentration potassium sulfate solutions, and high-concentration potassium carbonate solutions.
[0025] Furthermore, in steps (2) to (5), the high-concentration potassium salt solution refers to a near-saturation concentration of the corresponding potassium salt at the corresponding temperature. For example, the mass fraction of potassium chloride in high-concentration potassium chloride solution B is between 22.1% and 26.4%, and the mass fraction of potassium chloride in high-concentration potassium chloride solution C is between 31.4% and 35.9%.
[0026] Furthermore, in step (5), the temperature is lowered to 15-30°C, preferably 20-25°C; the stirring speed is 300-500 r / min, and the standing time is 2-5 hours; the high-purity potassium salt product is high-purity potassium chloride, high-purity potassium sulfate or high-purity potassium carbonate.
[0027] Furthermore, in step (7), the water is tap water, and the water temperature is 15-30°C, preferably 20-25°C; the mass ratio of the water to the filter residue E is L=0.1-1.0, preferably L=0.3-0.5; and the stirring time is 0.1-2.0h, preferably 0.5-1.0h.
[0028] Further, in step (9), the filtrate F and the filtrate G are mixed in any proportion.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) The potassium chloride product produced by the present invention meets the national standard "GB / T 6549-2011 Potassium Chloride", the potassium sulfate product produced meets the national standard "GB / T 20406-2017 Potassium Sulfate for Agricultural Use", and the potassium carbonate product produced meets the national standard "GB / T 1587-2016 Industrial Potassium Carbonate".
[0031] (2) The by-product calcium carbonate produced by the present invention complies with the "HG2226-91 Industrial Precipitated Calcium Carbonate Chemical Industry Standard"; the by-product calcium sulfate produced can meet the "GB / T 9776-2008 Building Gypsum Standard".
[0032] (3) The production process of the present invention does not evaporate a large amount of water and can rely on preheating from a power plant to heat, thus saving water and energy.
[0033] (4) The present invention makes full use of the soluble potassium enriched in biomass fly ash, turns waste into treasure, reduces waste accumulation, alleviates environmental pressure and generates certain benefits for the biomass power plant, thus having extremely high environmental and economic benefits.
[0034] (5) The process of the present invention is simple, the production cost is low and the efficiency is high. DETAILED DESCRIPTION
[0035] The present invention will be further described below with reference to specific embodiments.
[0036] Example 1
[0037] A method for extracting potassium salt from biomass fly ash comprises the following steps:
[0038] (1) Grinding biomass fly ash (containing 11.6 wt% K2O and 6.1 wt% CaO) and sieving to 8 mm to obtain processed raw material A;
[0039] (2) adding water to 10 kg of the treated raw material A obtained in step (1) at a mass ratio of 0.5 between water and raw material A, mixing and stirring, and filtering at a water temperature of 20° C., a stirring time of 1 h, and a stirring speed of 500 r / min. Repeating this step 10 times to obtain a high-concentration KCl solution B and a filter residue C;
[0040] (3) heating the high-concentration KCl solution B obtained in step (2) to 80° C., adding raw material A at a mass ratio of solution B to raw material A of 0.5, stirring, and filtering, wherein the stirring time is 1 hour and the stirring speed is 350 r / min. Repeat this step 10 times to obtain a high-concentration KCl solution C and a filter residue D;
[0041] (4) The contents of calcium ions, carbonate ions, and sulfate ions in solution C obtained in step (3) were analyzed. The results showed that carbonate ions were negligible. 2+ +SO4 2- →CaSO4↓, add calcium chloride to solution C to completely precipitate calcium ions and sulfate ions in the solution in the form of calcium sulfate, stir and filter to obtain high-concentration KCl solution D and product calcium sulfate;
[0042] (5) stirring the solution D obtained in step (4) and cooling it to 20° C. at a stirring speed of 250 r / min, and standing for 2 h to obtain a mixed slurry for solid-liquid separation, and filtering to obtain a high-concentration KCl solution E and a high-purity potassium chloride product;
[0043] (6) The high-concentration KCl solution E obtained in step (5) has a similar composition to the high-concentration potassium salt solution B, so it is treated in the same way as the high-concentration KCl solution B, and steps (3) to (5) are repeated again;
[0044] (7) The filter residue C obtained in step (2) and the filter residue D obtained in step (3) are mixed to obtain a filter residue E, and water is added to the filter residue at a mass ratio of water to filter residue E of 0.3, stirred, and filtered, wherein the water temperature is 20° C., the stirring speed is 300 r / min, and the stirring time is 1 h, to obtain a filtrate F and a filter residue F with a high water content;
[0045] (8) Passing the filter residue F with a high water content obtained in step (6) through a plate and frame filter press to obtain a filter residue G with a low water content and a filtrate G;
[0046] (9) The low-water filter residue G can be used as an ingredient for building materials such as concrete. The filtrate F and filtrate G can be mixed in any proportion and used as the feed liquid in the front-end high-temperature heating step.
[0047] After testing, the potassium chloride content in the potassium chloride product obtained from step (5) of the present invention is 98.8%, and the yield is 70%.
[0048] Example 2
[0049] A method for extracting potassium salt from biomass fly ash comprises the following steps:
[0050] (1) Grinding biomass fly ash (containing 9.3 wt% K2O and 7.13 wt% CaO) and sieving to 10 mm to obtain processed raw material A;
[0051] (2) adding water to the treated raw material A obtained in step (1) at a mass ratio of 1, mixing, stirring, and filtering at a water temperature of 20° C., a stirring time of 0.5 h, and a stirring speed of 400 r / min to obtain a solution B containing a high concentration of K2CO3 and a filter residue C;
[0052] (3) The high-concentration K2CO3 solution B obtained in step (2) was heated to 80°C, and raw material A was added at a mass ratio of solution B to raw material A of 0.5, stirred, and filtered. The stirring time was 1 hour and the stirring speed was 350 r / min. This step was repeated 10 times to obtain a high-concentration K2CO3 solution C and a filter residue D;
[0053] (4) The contents of calcium ions, carbonate ions, and sulfate ions in solution C obtained in step (3) were analyzed. The results showed that sulfate ions were negligible. 2+ +CO3 2- →CaCO3↓, add calcium chloride to solution C to completely precipitate calcium ions and carbonate ions in the solution in the form of calcium carbonate, stir and filter to obtain solution D containing high concentration of K2CO3 and product calcium carbonate;
[0054] (5) stirring the solution D obtained in step (4) and cooling it to 20° C. at a stirring speed of 250 r / min, and standing for 2 h to obtain a mixed slurry for solid-liquid separation, which was filtered to obtain a high-concentration K2CO3 solution E and a high-purity potassium chloride product;
[0055] (6) The high-concentration K2CO3 solution E obtained in step (5) has a similar composition to the high-concentration K2CO3 solution B, so it is treated in the same way as the high-concentration K2CO3 solution B, and steps (3) to (5) are repeated again;
[0056] (7) The filter residue C obtained in step (2) and the filter residue D obtained in step (3) are mixed to obtain a filter residue E, and water is added to the filter residue at a mass ratio of water to filter residue E of 0.5, stirred, and filtered, wherein the water temperature is 20° C., the stirring speed is 400 r / min, and the stirring time is 1 h, to obtain a filtrate F and a filter residue F with a high water content;
[0057] (7) passing the filter residue F with a high water content obtained in step (6) through a plate and frame filter press to obtain a filter residue G with a low water content and a filtrate G;
[0058] (8) The low-water filter residue G can be used as an ingredient for building materials such as concrete. The filtrate F and filtrate G can be mixed in any proportion and used as the feed liquid in the front-end high-temperature heating step.
[0059] After testing, the potassium carbonate product obtained from step (5) of the present invention has a potassium carbonate content of 99.7% and a yield of 65%.
[0060] Example 3
[0061] A method for extracting potassium salt from biomass fly ash comprises the following steps:
[0062] (1) Grinding biomass fly ash (containing 9.13 wt% K2O and 6.19 wt% CaO) and sieving to 10 mm to obtain processed raw material A;
[0063] (2) adding water to the treated raw material A obtained in step (1) at a mass ratio of 0.5, mixing and stirring, and filtering at a water temperature of 25° C., a stirring time of 1 h, and a stirring speed of 500 r / min. Repeating this step 8 times to obtain a solution B containing a high concentration of K2SO4 and a filter residue C;
[0064] (3) The high-concentration K2SO4 solution B obtained in step (2) was heated to 80°C, and raw material A was added at a mass ratio of solution B to raw material A of 1, stirred, and filtered. The stirring time was 1.5 hours and the stirring speed was 300 r / min. This step was repeated 10 times to obtain a high-concentration K2SO4 solution C and a filter residue D;
[0065] (4) The contents of calcium ions, carbonate ions, and sulfate ions in solution C obtained in step (3) were analyzed. The results showed that carbonate ions were negligible. 2+ +SO4 2- →CaSO4↓, add calcium chloride to solution C to completely precipitate the calcium ions and sulfate ions in the solution in the form of calcium sulfate, stir and filter to obtain solution D containing high concentration of K2SO4 and product calcium sulfate;
[0066] (5) stirring the solution D obtained in step (4) and cooling it to 25° C. at a stirring speed of 250 r / min, and standing for 2 h to obtain a mixed slurry for solid-liquid separation, which was filtered to obtain a high-concentration K2SO4 solution E and a high-purity potassium chloride product;
[0067] (6) The high-concentration K2SO4 solution E obtained in step (5) has a similar composition to the high-concentration K2SO4 solution B, so it is treated in the same way as the high-concentration K2SO4 solution B, and steps (3) to (5) are repeated again;
[0068] (7) The filter residue C obtained in step (2) and the filter residue D obtained in step (3) are mixed to obtain a filter residue E, and water is added to the filter residue at a mass ratio of water to filter residue E of 0.3, stirred, and filtered, wherein the water temperature is 25° C., the stirring speed is 300 r / min, and the stirring time is 1 h, to obtain a filtrate F and a filter residue F with a high water content;
[0069] (8) Passing the filter residue F with a high water content obtained in step (6) through a plate and frame filter press to obtain a filter residue G with a low water content and a filtrate G;
[0070] (8) The low-water filter residue G can be used as an ingredient for building materials such as concrete. The filtrate F and filtrate G can be mixed in any proportion and used as the feed liquid in the front-end high-temperature heating step.
[0071] After testing, the potassium sulfate content in the potassium sulfate product obtained from step (5) of the present invention is 98.9%, and the yield is 63%.
Claims
1. A method for extracting potassium salt from biomass fly ash, characterized in that: The following steps are involved: (1) crushing biomass fly ash to obtain raw material A; the mass fraction of K2O in the biomass fly ash is 1.8-35.4%, and the mass fraction of CaO is 6%-35%; (2) mixing the raw material A obtained in step (1) with water, stirring, and performing solid-liquid separation to obtain a high-concentration potassium salt solution B and a filter residue C; the mass ratio of the water to the raw material A is M, M=0.5-1.0; the stirring time is 0.5h-2h, and the stirring speed is 250-500r / min; (3) heating the high-concentration potassium salt solution B obtained in step (2), adding the raw material A obtained in step (1) and stirring, and separating the solid and liquid to obtain a high-concentration potassium salt solution C and a filter residue D; the heating is heating to a temperature of 50° C. to 99° C.; (4) adding calcium chloride or potassium sulfate to the high-concentration potassium salt solution C obtained in step (3), stirring, and separating the solid and the liquid to obtain a high-concentration potassium salt solution D and a product of calcium sulfate or calcium carbonate; The specific process is as follows: firstly, the concentrations of calcium ions and carbonate ions or calcium ions and sulfate ions in the high-concentration potassium salt solution C are analyzed and detected, and the molar equivalent of calcium chloride or potassium sulfate required to react with the calcium ions according to reaction formula (4-1) or (4-2) is added, and the mixture is stirred until the reaction is complete. After solid-liquid separation of calcium carbonate or calcium sulfate, a high-concentration potassium salt solution D is obtained; reaction formulas (4-1) and (4-2) are as follows: ; (5) stirring the high-concentration potassium salt solution D obtained in step (4), cooling it, standing it, and then separating the solid from the liquid to obtain a high-concentration potassium salt solution E and a high-purity potassium salt product; the cooling is to cool it to 15-30° C.; (6) Repeating steps (3) to (5) with the high concentration potassium salt solution E obtained in step (5); (7) Mixing the filter residue C obtained in step (2) and the filter residue D obtained in step (3) to obtain a filter residue E, adding water to the filter residue E, stirring, and performing solid-liquid separation to obtain a filtrate F and a water-containing filter residue F; the mass ratio of the water to the filter residue E is L=0.1~1.0; (8) passing the aqueous filter residue F obtained in step (7) through a plate and frame filter press to obtain aqueous filter residue G and filtrate G; (9) The filtrate F obtained in step (7) and the filtrate G obtained in step (8) are mixed and used as the feed liquid for step (3) for recycling.
2. The method for extracting potassium salt from biomass fly ash according to claim 1, characterized in that: In step (1), the pulverizing is to pulverize the biomass fly ash into a particle size of 5 to 15 mm.
3. The method for extracting potassium salt from biomass fly ash according to claim 1 or 2, characterized in that: In step (3), the stirring time is 0.5-2.0 h; the stirring speed is 250-500 r / min.
4. The method for extracting potassium salt from biomass fly ash according to claim 1 or 2, characterized in that: In step (3), the mass ratio of the high-concentration potassium salt solution B to the raw material A is N, where N=0.3~2.
0.
5. The method for extracting potassium salt from biomass fly ash according to claim 3, characterized in that: In step (3), the mass ratio of the high-concentration potassium salt solution B to the raw material A is N, where N=0.3~2.
0.
6. The method for extracting potassium salt from biomass fly ash according to claim 1 or 2, characterized in that: In steps (2) to (5), the high-concentration potassium salt solution B, the high-concentration potassium salt solution C, the high-concentration potassium salt solution D and the high-concentration potassium salt solution E are one of a high-concentration potassium chloride solution, a high-concentration potassium sulfate solution or a high-concentration potassium carbonate solution.
7. The method for extracting potassium salt from biomass fly ash according to claim 1 or 2, characterized in that: In step (5), the stirring speed is 300-500 r / min; the standing time is 2-5 h; and the high-purity potassium salt product is high-purity potassium chloride, high-purity potassium sulfate or high-purity potassium carbonate.
8. The method for extracting potassium salt from biomass fly ash according to claim 1 or 2, characterized in that: In step (7), the stirring time is 0.1 to 2.0 h.
Citation Information
Patent Citations
Method for producing potassium salt and sodium salt by using waste incineration fly ash
CN110040748A
Method for extracting potassium and sodium from fly ash water washing liquid
CN110563237A