A method for simultaneously preparing hydrogen and light olefins using hydrocarbon raw materials

By using hydrocarbon raw materials and catalysts in the fluidization reactor to conduct carbon-hydrogen bond fracture reaction, hydrogen and low-carbon olefins are generated, and the high energy consumption and environmental protection problems of fossil energy hydrogen production technology are solved through the regeneration and reduction of the catalyst. , achieving efficient and low-carbon hydrogen production and low-carbon olefin by-production, meeting the hydrogen demand of refineries.

CN116004277BActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111229822.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-22
Publication Date
2024-11-12
Estimated Expiration
2041-10-22

AI Technical Summary

Technical Problem

The existing fossil energy hydrogen production technology has high energy consumption, environmental protection problems and challenges that cannot meet future hydrogen demand, especially in large-scale production of refineries.

Method used

Hydrocarbon raw materials are used to carry out carbon-hydrogen bond fracture reactions with zeolite-containing and metal oxide catalysts in the fluidization reactor to generate hydrogen and low-carbon olefins, and reduce energy consumption and achieve optimal resource utilization through the catalyst regeneration and reduction treatment. .

Benefits of technology

It has achieved efficient preparation of hydrogen and low-carbon olefins, reduced energy consumption in the hydrogen production process, optimized resource utilization, reduced carbon emissions, and improved the economic and social benefits of refineries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116004277B_ABST
    Figure CN116004277B_ABST
Patent Text Reader

Abstract

A method for simultaneously preparing hydrogen and low-carbon olefins using hydrocarbon raw materials, wherein the hydrocarbon raw materials are fed into a fluidized reactor, contacted with a catalyst containing zeolite and metal oxides to generate hydrogen and low-carbon olefins by carbon-hydrogen bond breaking reaction, and the reaction oil gas and carbonized catalyst obtained by the reaction are separated; the reaction oil gas is further separated into products containing hydrogen, carbon monoxide, carbon dioxide, low-carbon olefins and other hydrocarbon products; the obtained carbonized catalyst is sent to a regenerator for charring reaction, and the carbonized catalyst is sent to a reducer as a regenerated catalyst after charring and regeneration, and the reduced regenerated catalyst is sent to a fluidized reactor for recycling after stripping; the regenerated flue gas enters a separation unit, and carbon monoxide and carbon dioxide are separated. The method of the present invention converts low-value hydrocarbon raw materials into hydrogen and low-carbon olefins, realizes the efficient utilization of limited petroleum resources, and at the same time realizes CO2 enrichment, which is conducive to carbon recovery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for producing hydrogen and low-carbon olefins by taking hydrocarbon raw materials as raw materials. Background Art

[0002] Hydrogen is hailed as the core of the future world energy architecture and is also considered the cleanest fuel. However, if hydrogen comes from fossil fuels, its preparation process is not "clean". At present, more than 96% of commercial hydrogen is produced from fossil fuels, and a large amount of carbon dioxide is emitted during the hydrogen production process. This type of hydrogen is also called "gray hydrogen". Water resources, including seawater, are the largest "hydrogen mine" on the earth, and water electrolysis is considered to be an effective method for producing hydrogen. However, whether the production of green hydrogen by electrolysis of water from renewable energy can be actually solved and applied to large-scale carbon reduction still needs to overcome three major problems: large-scale electrolysis of water, low energy consumption and high stability.

[0003] Using fossil energy as a resource to realize the production of "blue hydrogen" is an effective technical means to solve the current hydrogen energy problem. The more mature technical routes for the existing fossil energy hydrogen production methods include the use of fossil energy such as coal and natural gas to reform hydrogen, and the high-temperature decomposition reforming of chemical raw materials represented by alcohol cracking hydrogen production technology. At present, domestic natural gas reforming hydrogen production and high-temperature cracking hydrogen production are mainly used in large-scale hydrogen production industries. The raw gas in the natural gas hydrogen production process is also fuel gas, which does not need to be transported, but the investment in natural gas hydrogen production is relatively high, which is suitable for large-scale industrial production. Coal gasification hydrogen production is the first choice for large-scale industrial hydrogen production, and it is also the mainstream fossil energy hydrogen production method in my country. This hydrogen production process converts coal into synthesis gas (CO, CH4, H2, CO2, N2, etc.) through gasification technology, and then separates and processes it through water-gas shift to extract high-purity hydrogen. It is the raw material for preparing synthetic ammonia, methanol, liquid fuel, natural gas and other products, and is widely used in petrochemical, steel and other fields. The coal-to-hydrogen technology is mature and efficient, and can be produced on a large scale and stably. However, the fuel power consumption of coal-to-hydrogen is higher than that of natural gas-to-hydrogen, and the system steam and electricity requirements are high, and enterprises need supporting boilers. In addition, environmental protection issues are prominent, the existing urban refineries have strict environmental requirements, and coal transportation is subject to many factors, which also limits the application of this technology in modern refineries.

[0004] The country's standards for oil quality requirements have been raised (sulfur content has been reduced), and the market demand for light oil products has increased. These factors have led to the wider application of hydrogenation technology, which has become the main driving force for the surge in refinery hydrogen demand. According to statistics, the annual growth rate of global refinery hydrogen demand exceeds 4%. The importance of hydrogen production in the refining process has gradually become prominent. A 10Mt / a refinery equipped with a residue oil hydrogenation unit consumes about 1% of the crude oil processing volume, while a refinery without residue oil hydrogenation consumes about 0.7%. The hydrogen supply from within the refinery will be difficult to meet the future growth demand for hydrogen, so it is necessary to explore a more flexible and feasible hydrogen supply strategy. At present, there is an overcapacity in refining capacity, and the transformation of refining enterprises from "fuel type" to "chemical type" is already a general trend. If flexible hydrogen production technology can be developed to produce low-carbon olefins, it will undoubtedly have good economic and social benefits. Summary of the invention

[0005] The object of the present invention is to provide a method for simultaneously preparing hydrogen and light olefins by using hydrocarbon raw materials.

[0006] The method for simultaneously preparing hydrogen and light olefins using hydrocarbon raw materials provided by the present invention comprises the following steps:

[0007] The hydrocarbon raw material is fed into a fluidized reactor, and is contacted with a catalyst containing zeolite and metal oxide to generate hydrogen through a carbon-hydrogen bond breaking reaction and light olefins through a carbon-carbon bond breaking reaction, thereby obtaining a reaction oil gas containing hydrogen and light olefins and a carbon-bearing catalyst;

[0008] Separating the reaction oil gas containing hydrogen and light olefins from the carbon-bearing catalyst;

[0009] The separated reaction oil and gas are further separated into products including hydrogen, carbon monoxide, carbon dioxide, light olefins and other hydrocarbon products;

[0010] The obtained carbonized catalyst is sent to a regenerator for carbonization reaction. After the carbonized catalyst is regenerated by burning, it is sent to a reducer as a regenerated catalyst. The regenerated flue gas enters a separation unit to separate carbon monoxide and carbon dioxide.

[0011] The regenerated catalyst enters the reducer, contacts with the reducing agent and undergoes a reduction reaction. The reduced regenerated catalyst enters the fluidized bed reactor after stripping.

[0012] The hydrocarbon raw material is selected from one or more mixtures of petroleum hydrocarbons, mineral oils and synthetic oils. The petroleum hydrocarbons are gaseous hydrocarbons, gasoline, diesel, vacuum wax oil, atmospheric residue oil, vacuum wax oil mixed with part of vacuum residue oil or hydrocarbon oil obtained by secondary processing; mineral oil is selected from one or more mixtures of coal liquefaction oil, oil sand oil and shale oil; synthetic oil is a distillate oil obtained by Fischer-Tropsch synthesis of coal, natural gas or asphalt. The hydrocarbon oil obtained by secondary processing is selected from one or more of coker gasoline, catalytic diesel, hydrogenated diesel, coker diesel, coker wax oil, deasphalted oil and furfural refined raffinate oil.

[0013] Based on the dry weight of the catalyst, the catalyst includes 5%-65% natural minerals, 10%-60% oxides, 10%-60% zeolites and 0.1%-30% metal active components. The zeolite includes medium-pore zeolite and optional large-pore zeolite, the medium-pore zeolite is ZSM series zeolite and / or ZRP zeolite, and the large-pore zeolite is selected from one or more of rare earth Y, rare earth hydrogen Y, ultra-stable Y and high silicon Y. The medium-pore zeolite accounts for 5-100% by weight of the total weight of the zeolite, preferably 20-50% by weight. The content of the metal active component is 0.1%-30% by weight, preferably 0.5-20% by weight. The metal active component is selected from one or more compounds of transition metal elements, preferably one or more of nickel, cobalt, iron, tungsten, molybdenum, manganese, copper, zirconium and chromium.

[0014] The reaction temperature of the fluidized reactor is 450-800°C, preferably 550-700°C, the reaction time is 0.1-10 seconds, preferably 1-8 seconds, the weight ratio of the catalyst to the hydrocarbon feedstock is 5-100, preferably 20-50, and the weight ratio of water vapor to the hydrocarbon feedstock is 0.1-20, preferably 1-10.

[0015] The fluidized reactor is selected from one or a combination of a riser reactor, a fast bed and a dense phase fluidized bed. The fluidized reactor comprises a pre-lifting section and a fluidized reactor of at least one reaction zone from bottom to top, and the number of the reaction zones is preferably 2-8, more preferably 2-3.

[0016] The oxygen concentration in the oxygen-containing gas at the bottom of the regenerator is 22-100 volume % and preferably 25-80 volume %.

[0017] The regeneration operation conditions are: temperature of 550-700°C, preferably 600-650°C; gas superficial velocity of 0.2-1.2 m / s, preferably 0.4-0.8 m / s; average residence time of deactivated catalyst of 1-10 minutes, preferably 2-6 minutes.

[0018] The volume ratio of CO / CO2 in the regeneration flue gas is 0.2-2.0, preferably 0.8-1.5.

[0019] The operating conditions of the reducer are: temperature of 550-700°C; gas superficial velocity of 0.5-3 m / s.

[0020] The reducing agent is selected from one or more small molecule alkanes, preferably one or more of methane, ethane, propane, n-butane and isobutane.

[0021] The separated gas obtained from the regenerated flue gas and the separation unit is rich in carbon monoxide, which can be used as a raw material for water-gas shift to further produce hydrogen and carbon dioxide; it can also be sent to a carbon monoxide boiler to recover the waste heat of the flue gas to produce high-quality steam.

[0022] The present invention adopts a fluidized reactor to produce hydrogen, and the catalyst circulates between the reactor and the regenerator, which not only realizes the regeneration of the deactivated catalyst, but also transfers a large amount of heat for the reaction, greatly reducing the energy required for the hydrogen production process and achieving process economy.

[0023] The present invention preferably adopts low-temperature incomplete regeneration technology, and the CO / CO2 ratio in the regenerated flue gas is high, which can provide cheap raw gas for the water-gas shift process and realize the optimal utilization of resources. It can also recover the waste heat of the flue gas to produce hot water or high-quality steam for supply to other devices, which can play the role of a public engineering island, realize the rational utilization of energy in the refinery, and improve the process economy.

[0024] The oxygen-containing gas used for regenerating the deactivated catalyst in the hydrogen production process of the present invention is preferably oxygen-rich gas, which greatly increases the concentration of CO2 in the flue gas, can achieve large-scale production of CO2, and then reduce carbon emissions through capture, utilization, and storage technology, thereby achieving the production of blue hydrogen.

[0025] The present invention performs reduction treatment on the catalyst before the hydrogen production reaction to reduce the high-valent metal oxide to a low-valent metal oxide, thereby increasing the dehydrogenation activity of the catalyst and improving the hydrogen selectivity.

[0026] The present invention adopts a catalytic conversion method to convert hydrocarbon raw materials into hydrogen and produce low-carbon olefins as by-products, with a high hydrogen yield. The present invention not only realizes the high-value utilization of hydrocarbon raw materials and meets the market demand for low-carbon olefins, but also enriches the CO2 generated in the process, which not only brings hydrogen energy, but also facilitates carbon capture, and can bring greater economic and social benefits to the petrochemical industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A process flow chart of a specific implementation method of the present invention for simultaneously producing hydrogen and light olefins using hydrocarbon raw materials. DETAILED DESCRIPTION

[0028] A method for simultaneously preparing hydrogen and light olefins using hydrocarbon raw materials, the method comprising the following steps:

[0029] The hydrocarbon raw material is fed into a fluidized reactor, and is contacted with a catalyst containing zeolite and metal oxide to generate hydrogen through a carbon-hydrogen bond breaking reaction and light olefins through a carbon-carbon bond breaking reaction, thereby obtaining a reaction oil gas containing hydrogen and light olefins and a carbon-bearing catalyst;

[0030] Separating the reaction oil gas containing hydrogen and light olefins from the carbon-bearing catalyst;

[0031] The separated reaction oil and gas are further separated into products including hydrogen, carbon monoxide, carbon dioxide, light olefins and other hydrocarbon products;

[0032] The obtained carbonized catalyst is sent to a regenerator for carbonization reaction. After the carbonized catalyst is regenerated by burning, it is sent to a reducer as a regenerated catalyst. The regenerated flue gas enters a separation unit to separate carbon monoxide and carbon dioxide.

[0033] The regenerated catalyst enters the reducer, contacts with the reducing agent and undergoes a reduction reaction. The reduced regenerated catalyst enters the fluidized bed reactor after stripping.

[0034] The carbon monoxide obtained from the regenerated flue gas and the separation unit can be used as a raw material for water-gas shift to further produce hydrogen and carbon dioxide; it can also be sent to a carbon monoxide boiler to recover flue gas waste heat to generate high-pressure steam.

[0035] The hydrocarbon raw material is various animal and plant oils rich in hydrocarbons, and the hydrocarbon raw material is selected from one or more mixtures of petroleum hydrocarbons, mineral oils and synthetic oils. Petroleum hydrocarbons are well known to those skilled in the art, for example, it can be a petroleum distillate obtained by a primary processing device, and can be selected from one or more mixed oils such as gasoline, diesel, vacuum wax oil, atmospheric residue oil, vacuum residue oil, or a distillate obtained by a secondary processing device, and can be selected from one or more of coker gasoline, catalytic diesel, hydrogenated diesel, coker diesel, coker wax oil, deasphalted oil, furfural refined raffinate oil. Mineral oil is selected from one or more mixtures of coal liquefaction oil, oil sand oil and shale oil. Synthetic oil is a distillate obtained by Fischer-Tropsch synthesis of coal, natural gas or asphalt.

[0036] The catalyst comprises the following components by weight percentage:

[0037] A) 5%-65% natural minerals,

[0038] B) 10%-60% oxide,

[0039] C) 10% to 60% of zeolite, and

[0040] D) 0.1%-30% metal active component.

[0041] The method provided by the present invention can be carried out in various existing fluidized reactors, wherein the fluidized reactor is selected from one or a combination of a turbulent bed, a fast bed and a dilute phase transport bed. The fluidized reactor includes a pre-lifting section and at least one reaction zone fluidized reactor from bottom to top. In order to allow the crude oil to react fully and according to different quality requirements of the target product, the reaction zones can be 2-8, preferably 2-3.

[0042] The conditions of the catalytic decomposition reaction include: the reaction temperature of the fluidized reactor is 450-800°C, preferably 550-700°C, the reaction time is 0.1-10 seconds, preferably 1-8 seconds, the weight ratio of the catalyst to the hydrocarbon feedstock is 5-100, preferably 20-50; the weight ratio of water vapor to the hydrocarbon feedstock is 0.1-20, preferably 1-10.

[0043] According to the method provided by the present invention, the deactivated catalyst is generally first separated from the reaction oil and gas to obtain the deactivated catalyst and the reaction oil and gas, and then the obtained reaction oil and gas are separated into hydrogen, CO2, CO, gaseous hydrocarbons and liquid hydrocarbons and other fractions through a subsequent separation unit, and the gaseous hydrocarbons are further separated by a gas separation device to obtain hydrocarbon components such as ethylene and propylene. The method for separating hydrogen, ethylene, propylene, etc. from the reaction products is similar to the conventional technical method in the field, and the present invention is not limited to this and is not described in detail herein.

[0044] In the method provided by the present invention, the CO obtained in the separation unit can be sent to the water-gas shift unit to further react with water vapor to obtain hydrogen and enriched CO2. The water-gas shift of CO and water vapor adopts the existing technology well known to those skilled in the art.

[0045] In the method provided by the present invention, preferably the deactivated catalyst enters the stripping section under the action of gravity, the hydrocarbon products adsorbed on the deactivated catalyst are stripped by water vapor, and the deactivated catalyst after stripping enters the regenerator.

[0046] The deactivated catalyst can be regenerated in a conventional regenerator, and a single regenerator or multiple regenerators can be used. During the regeneration process, an oxygen-containing gas is generally introduced from the bottom of the regenerator. After the oxygen-containing gas is introduced into the regenerator, the deactivated catalyst contacts with oxygen and burns and regenerates. The flue gas generated after the catalyst burns and regenerates is separated into gas and solid at the top of the regenerator, and the flue gas enters the water-gas shift unit. The oxygen-containing gas used for regenerating the deactivated catalyst is preferably an oxygen-rich gas. The oxygen concentration in the oxygen-containing gas at the bottom of the regenerator is 22-100% by volume, preferably 25%-80% by volume.

[0047] In the method provided by the present invention, low-temperature incomplete regeneration is preferred, and the operating conditions are: temperature is 550-700°C, preferably 600-650°C; gas superficial linear velocity is 0.2-1.2 m / s, preferably 0.4-0.8 m / s, and the average residence time of the deactivated catalyst is 1-10 minutes, preferably 2-6 minutes.

[0048] In the method provided by the present invention, the volume ratio of CO / CO2 in the regeneration flue gas is 0.2-2.0, preferably 0.8-1.5.

[0049] In the method provided by the present invention, the operating conditions of the reducer for regenerating the catalyst are: temperature of 550-700° C.; gas superficial linear velocity of 0.5-3 m / s.

[0050] In the method provided by the present invention, the reducing agent for regenerating the catalyst is selected from one or more small molecule alkanes, preferably one or more of methane, ethane, propane, n-butane and isobutane.

[0051] In the method provided by the present invention, the stripping gas for regenerating the catalyst is nitrogen.

[0052] In the method provided by the present invention, the natural minerals in the catalyst are selected from one or more of kaolin, halloysite, montmorillonite, diatomite, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite, and the content of natural minerals on a dry basis is 5% to 65% by weight, preferably 15% to 60% by weight; the oxide is one or more of silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, and amorphous silicon aluminum, and the content of the oxide is 10% to 60% by weight, preferably 10% to 30% by weight, and more preferably 12% to 28% by weight, based on the total amount of the catalyst and in terms of oxide weight percentage. The zeolite includes a medium-pore zeolite and an optional large-pore zeolite, and the large-pore zeolite is selected from one or more of rare earth Y, rare earth hydrogen Y, ultrastable Y and high silicon Y. The medium-pore zeolite is a ZSM series zeolite and / or a ZRP zeolite, and the medium-pore zeolite accounts for 5-100% by weight of the total weight of the zeolite, preferably 20-50% by weight.

[0053] Based on the weight of the catalyst, the metal active component content is 0.1%-30% by weight, preferably 0.5-20% by weight. The metal active component is selected from one or more compounds of transition metal elements, preferably one or more of nickel, cobalt, iron, tungsten, molybdenum, manganese, copper, zirconium and chromium.

[0054] In the method provided by the present invention, the catalyst preparation method adopts the preparation method of conventional catalytic cracking catalyst, which is a preparation method well known to those skilled in the art. The metal can be loaded on the catalyst by impregnation method or slurry method, preferably impregnation method, which are well known to those skilled in the art.

[0055] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention, but do not constitute a limitation of the present invention.

[0056] like Figure 1 As shown, the regenerated catalyst enters the reducer 23 and contacts with the reducing agent 16 to undergo a reduction reaction. The reduced regenerated catalyst enters the stripper 24 and contacts with the nitrogen 17 injected at the bottom to strip the carbon monoxide and carbon dioxide carried by the catalyst. The reduced and stripped regenerated catalyst enters the fluidized reactor 1 through the regeneration inclined tube 18 and accelerates upward along the reactor under the action of the pre-lifting medium 22. The hydrocarbon raw material is mixed with the water vapor from the pipeline 6 through the pipeline 5 and then injected into the fluidized reactor 1 to contact the regenerated catalyst. The hydrocarbon raw material undergoes a catalytic reaction on the hot catalyst and accelerates upward. The generated reaction products and the carbon-bearing catalyst are separated by the cyclone separator 7 and collected by the gas collection chamber 8. The reaction products enter the separation unit 3 through the pipeline 9 and are separated into hydrogen 10, carbon monoxide 11, carbon dioxide 12, and hydrocarbon products 13. The hydrocarbon products can be further separated to obtain low-carbon olefins such as ethylene, propylene and butene, low-carbon alkanes and other hydrocarbon products. The low-carbon alkanes can be used as the reducing agent of the present invention, and the remaining other hydrocarbon products can be further converted by partial or full refining. The separated carbon monoxide can be used as a raw material for water gas shift, and low-carbon olefins can be further separated into ethylene.

[0057] The catalyst with carbon enters the stripping section 4 and contacts the stripping steam 18 for stripping, then enters the regenerator 2 through the inclined tube 19 and contacts the oxygen-rich gas 14 entering through the main air distribution plate 15 to undergo a carbonization reaction, burning off the coke on the deactivated catalyst to regenerate the catalyst with carbon. The regenerated flue gas enters the separation unit 3 through the separator 20 and the flue gas pipeline 21, and carbon monoxide 11 and carbon dioxide 12 are separated. The regenerated catalyst enters the reducer 23 and the stripper 24 in sequence, and the regenerated catalyst after reduction and stripping enters the fluidized reactor through the inclined tube 18 for recycling.

[0058] The present invention will be further described in the following examples, but the present invention is not limited thereto.

[0059] The raw materials used in the examples and comparative examples are all catalytic diesel, and the properties are shown in Table 1. The catalyst used in the comparative example is an industrial catalyst, the trade name is DMMC-1, and the properties are shown in Table 2.

[0060] The catalyst preparation method used in the examples is briefly described as follows:

[0061] 1) 75.4 kg of kaolin (solid content 71.6 wt%) was slurried with 250 kg of decationized water, and then 54.8 kg of pseudo-boehmite (solid content 63 wt%) was added, and the pH was adjusted to 2-4 with hydrochloric acid, and stirred evenly. The mixture was allowed to stand and age at 60-70°C for 1 hour, maintaining the pH at 2-4, and the temperature was lowered to below 60°C. 41.5 kg of aluminum sol (Al2O3 content of 21.7 wt%) was added, and stirred for 40 minutes to obtain a mixed slurry.

[0062] 2) ZRP-1 (22 kg on dry basis) and DASY zeolite (22.5 kg on dry basis) were added to the obtained mixed slurry, stirred evenly, spray-dried to form, washed with diammonium phosphate solution (phosphorus content of 1 wt%) to remove free Na+, and calcined to obtain a molecular sieve catalyst sample.

[0063] 3) 3 kg of Ni(NO3)2 was dissolved in 5.5 kg of water to prepare a Ni(NO3)2·6H2O aqueous solution, 10 kg of the molecular sieve catalyst sample was immersed in the Ni(NO3)2·6H2O aqueous solution, and the obtained mixture was dried at 180°C for 4 hours and calcined at 600°C for 2 hours. After repeated immersion, drying and calcination, the content of Ni loaded on the catalyst sample reached 15%, and the catalyst A of the embodiment was obtained.

[0064] Example 1

[0065] according to Figure 1 The catalytic decomposition reaction test of catalytic diesel was carried out on the riser reactor. The catalytic diesel entered the lower part of the riser reactor, contacted with the hot regenerated catalyst and underwent catalytic decomposition reaction. The reaction products and the deactivated catalyst entered the closed cyclone separator from the reactor outlet. The reaction products and the deactivated catalyst were quickly separated. The reaction products were separated into cracked gas and liquid according to the distillation range in the separation system.

[0066] The deactivated catalyst enters the stripping section under the action of gravity, and the hydrocarbon products adsorbed on the deactivated catalyst are stripped by water vapor. The deactivated catalyst after stripping enters the regenerator and contacts with oxygen-rich air for regeneration; the regenerated catalyst contacts with methane in turn for reduction reaction, and then returns to the riser reactor for recycling after nitrogen stripping. The operating conditions and product distribution are listed in Table 3.

[0067] From the results in Table 3, it can be seen that the hydrogen yield is as high as 18.33%, the ethylene yield is 2.38%, the propylene yield is 6.05%, the CO yield in the reaction product is 28.53%, and the CO2 yield is 25.64%. The CO concentration in the regeneration flue gas is 7.60% by volume, and the CO2 concentration is 25.33% by volume.

[0068] Comparative Example 1

[0069] The test was carried out on a medium-sized device of a riser, the catalytic diesel feedstock was the same as in Example 1, and the catalyst was DMMC-1.

[0070] The catalytic diesel enters the riser reactor and contacts the hot DMMC-1 catalyst to undergo a catalytic decomposition reaction. The reaction products and the deactivated catalyst enter the closed cyclone separator from the reactor outlet. The reaction products and the deactivated catalyst are quickly separated. The reaction products are separated into gas and liquid products according to the distillation range in the separation system.

[0071] The deactivated catalyst enters the stripping section under the action of gravity, and the hydrocarbon products adsorbed on the deactivated catalyst are stripped out by water vapor. The deactivated catalyst after stripping enters the regenerator and is regenerated by contact with air; the regenerated catalyst is then returned to the riser reactor for recycling; the operating conditions and product distribution are listed in Table 3.

[0072] From the results in Table 3, it can be seen that the hydrogen yield is 1.42%, the ethylene yield is 3.69%, the propylene yield is 9.52%, and the CO and CO2 yields in the reaction products are low. No CO was detected in the regeneration flue gas, the CO2 concentration was 15.56% by volume, and the O2 concentration was 3.50% by volume.

[0073] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0074] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0075] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the content of the present invention.

[0076] Table 1

[0077] project Catalytic diesel <![CDATA[Density (20 °C) / (kg / m 3 )]]> 948.9 <![CDATA[Kinematic viscosity (20 °C) / (mm 2 / s)]]> 3.754 Total acid value / (mg KOH / g) <0.05 Freezing point / ℃ -27 Closed cup flash point / ℃ 66 Distillation range / ℃ Initial distillation point 197.9 5% 220.4 10% 228.4 50% 262.5 70% 283.1 90% 308.6 95% 319.5 Final distillation point 329.9

[0078] Table 2

[0079] Example 1 Comparative Example 1 Catalyst A Industrial catalyst DMMC-1 Physical properties <![CDATA[Specific surface area, m 2 / g]]> 118 106 <![CDATA[Specific surface area of molecular sieve, m 2 / g]]> 30 42 <![CDATA[Pore volume, cm 3 / g]]> 0.126 0.13 Sieve composition, weight % 0~40 microns 22.7 30.9 0~80 microns 64.4 75.0 0~105 microns 87.1 89.1 0~149 microns 97.9 98.4 Average particle size / micron 55.0 55.6 Micro-anti-activity, % 50 65 Metal content, % Ni 14.5 0.06

[0080] Table 3

[0081] Example 1 Comparative Example 1 Riser reaction conditions Reaction temperature, °C 675 675 Reaction time, seconds 1.8 1.8 Weight ratio of catalyst to catalytic diesel 20 20 Water to oil weight ratio 0.25 0.25 Regeneration conditions Regeneration temperature, °C 645 680 Oxygen concentration in regeneration air, volume % 50 21 Gas superficial velocity, m / s 0.8 0.8 Average stay time, minutes 4.5 4.5 Reduction conditions Reduction temperature, °C 650 / Weight ratio of reducing agent to catalyst circulation 0.005 / Product distribution, weight % CO 28.53 0.25 <![CDATA[CO2]]> 25.64 1.01 <![CDATA[H2]]> 18.33 1.42 Ethylene 2.38 3.69 Propylene 6.05 9.52 Other gaseous hydrocarbons 11.09 30.47 Liquid hydrocarbons 2.67 43.53 Coke 5.31 10.11 total 100.00 100.00 Regeneration flue gas composition, volume % CO 7.60 / <![CDATA[CO2]]> 25.33 15.56 <![CDATA[N2]]> 67.05 80.94 <![CDATA[O2]]> 0.02 3.5

Claims

1. A method for simultaneously producing hydrogen and light olefins using hydrocarbon raw materials, comprising the following steps: The hydrocarbon feedstock is fed into a fluidized reactor and contacted with a catalyst to cause a carbon-hydrogen bond breaking reaction. The reaction temperature of the fluidized reactor is 450-800°C, the reaction time is 0.1-10 seconds, the weight ratio of the catalyst to the hydrocarbon feedstock is 5-100, and the weight ratio of water vapor to the hydrocarbon feedstock is 0.1-20. Hydrogen and carbon-carbon bond breaking reaction are generated to produce low-carbon olefins, and reaction oil and gas containing hydrogen and low-carbon olefins and a carbon-bearing catalyst are obtained. The hydrocarbon feedstock is catalytic diesel. Based on the dry weight of the catalyst, the catalyst includes 5%-65% of natural minerals, 10%-60% of oxides, 10%-60% of zeolites and 0.1%-30% metal active component, the natural mineral is selected from one or more of kaolin, montmorillonite, diatomite, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite, the oxide is one or more of silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, amorphous silicon aluminum, the metal active component is selected from one or more of nickel, cobalt, iron, tungsten, molybdenum, manganese, copper, zirconium and chromium, the zeolite includes medium-pore zeolite and optional large-pore zeolite, the medium-pore zeolite is ZSM series zeolite and / or ZRP zeolite, the large-pore zeolite is one or more selected from rare earth Y, rare earth hydrogen Y, ultra-stable Y and high silicon Y; Separating the reaction oil gas containing hydrogen and light olefins from the carbon-bearing catalyst; The obtained carbonized catalyst is sent to a regenerator to contact with oxygen-rich gas for carbonization reaction. The regeneration operating conditions are: temperature of 550-700°C; gas superficial linear velocity of 0.2-1.2 m / s, average residence time of deactivated catalyst of 1-10 minutes, CO / CO2 volume ratio in regenerated flue gas of 0.2-2.

0. After incomplete regeneration by burning, the carbonized catalyst is sent to a reducer as a regenerated catalyst, and the reaction oil gas and regenerated flue gas are combined and separated to obtain products containing hydrogen, carbon monoxide, carbon dioxide, low-carbon olefins and other hydrocarbons; The regenerated catalyst enters the reducer and contacts with the reducing agent to undergo a reduction reaction. The operating conditions of the reducer are: temperature of 550-700°C; gas superficial velocity of 0.5-3 m / s. The reducing agent is selected from one or more small molecule alkanes. The reduced regenerated catalyst enters the fluidized reactor after stripping.

2. The method according to claim 1, characterized in that The reducing agent is selected from one or more of methane, ethane, propane, n-butane and isobutane.

3. The method according to claim 1, characterized in that The reaction temperature of the fluidized reactor is 550-700° C., the reaction time is 1-8 seconds, the weight ratio of the catalyst to the hydrocarbon raw material is 20-50; and the weight ratio of water vapor to the hydrocarbon raw material is 1-10.

4. The method according to claim 1, characterized in that: The fluidized reactor is selected from one or a combination of a riser reactor, a fast bed and a dense phase fluidized bed.

5. The method according to claim 4, characterized in that The fluidized reactor comprises, from bottom to top, a pre-lifting section and at least one reaction zone.

6. The method according to claim 5, characterized in that The number of the reaction zones is 2-8.

7. The method according to claim 5, characterized in that The number of the reaction zones is 2-3.

8. The method according to claim 1, characterized in that: The concentration of oxygen in the oxygen-rich gas is 22-100% by volume.

9. The method according to claim 1, characterized in that: The concentration of oxygen in the oxygen-rich gas is 25-80% by volume.

10. The method according to claim 1, characterized in that The regeneration operation conditions are: temperature of 600-650° C.; gas superficial linear velocity of 0.4-0.8 m / s; and average residence time of the deactivated catalyst of 2-6 minutes.

11. The method according to claim 1, characterized in that: The volume ratio of CO / CO2 in the regeneration flue gas is 0.8-1.

5.

12. The method according to claim 1, characterized in that The medium-pore zeolite accounts for 5-100% by weight of the total weight of the zeolite.

13. The method according to claim 1, characterized in that The medium-pore zeolite accounts for 20-50% by weight of the total weight of the zeolite.

14. The method according to claim 1, characterized in that The content of the metal active component is 0.5-20% by weight.