A method for smelting molten steel
By controlling the argon gas flow rate and alloying process, adding low-nitrogen iron titanium or pure titanium wire to the LF furnace, the problem of high nitrogen content in the molten steel is solved, and the stability and production efficiency of the molten steel composition are improved.
Patent Information
- Application Number
- CN202310022404.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-01-07
AI Technical Summary
The existing technology is difficult to effectively reduce the nitrogen content in the molten steel, resulting in unstable composition of low-carbon, low-silicon, low-phosphorus, high-titanium, ultra-low-sulfur steel, which is difficult to produce, high cost, and accurate process requirements.
By controlling the argon flow rate of the converter and LF furnace, alloying the steel water, and adding low-nitrogen iron or pure titanium wire to the LF furnace, combining calcium wire, and setting the appropriate argon flow rate and time during the refining process, the steel is reduced. The nitrogen content in water.
It has achieved an effective reduction in the nitrogen content in molten steel, improved the composition stability of molten steel, reduced production difficulty and cost, and met the smelting requirements of low-carbon, low silicon, low phosphorus, high titanium, ultra-low sulfur steel.
Smart Images

Figure CN116005063B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of metallurgical technology, and in particular to a method for smelting molten steel. Background Art
[0002] The smelting of molten steel plays a key role in the subsequent preparation of steel plates. At present, the steel grade design adopts low-carbon, low-silicon, low-phosphorus, high-titanium and ultra-low-sulfur steel. It is difficult to produce in steel mills, with high processing costs, large fluctuations between each batch, and precise process requirements.
[0003] Since the converter and ladle have a great influence on the composition of steel, when they are difficult to control, the composition of low-carbon, low-silicon, low-phosphorus, high-titanium and ultra-low-sulfur steel will be unstable. In particular, how to reduce the nitrogen content in molten steel during the smelting process is a technical problem that needs to be solved urgently. Summary of the invention
[0004] The present application provides a method for smelting molten steel to solve the technical problem in the prior art that it is difficult to reduce the nitrogen content in molten steel.
[0005] In a first aspect, the present application provides a method for smelting molten steel, the method comprising:
[0006] Performing converter smelting on molten iron, and controlling the argon flow rate in the early stage and the late stage of the converter smelting respectively;
[0007] Alloying the molten iron after converter smelting to obtain first molten steel;
[0008] Performing LF furnace refining on the first molten steel, and controlling the early temperature rising process, the alloy fine-tuning process and the late argon gas flow rate of the LF furnace refining respectively;
[0009] Under the condition of setting the argon gas flow rate, low nitrogen ferrotitanium and or pure titanium wire are added to the first molten steel after being refined in the LF furnace, and calcium wire is fed after waiting for a set time to obtain molten steel.
[0010] Optionally, the argon flow rate in the early stage of the converter smelting is 800NL / min-1000NL / min, and the argon flow rate in the later stage of the converter smelting is 400NL / min-550NL / min.
[0011] Optionally, the molten iron is subjected to converter smelting, and the argon flow rates in the early and late stages of the converter smelting are respectively controlled, including:
[0012] The molten iron is subjected to converter smelting, and the argon flow rates in the early and late stages of the converter smelting are respectively controlled, as well as the process parameters of slag making and dephosphorization of the converter smelting.
[0013] Optionally, the process parameters of slag making and dephosphorization include: the distance between the oxygen lance position and molten iron in the early stage of converter smelting, the ratio of slag making materials, the temperature of converter auxiliary lance probes TSC and TSO, and the amount of ore added.
[0014] Optionally, the distance between the oxygen lance position in the early stage of converter smelting and the molten iron is 210mm-230mm;
[0015] The proportion of the slag-making material is as follows: 40kg-44kg of lime and 16kg-20kg of light burnt are added to each ton of molten steel;
[0016] The temperature of the converter auxiliary gun probe TSC is ≤1580°C, and the temperature of the converter auxiliary gun probe TSO is 1610°C-1640°C;
[0017] The amount of the ore added is 800kg-1000kg.
[0018] Optionally, the argon flow rate in the early heating process of the LF furnace refining is 150NL / min-300NL / min, the argon flow rate in the fine-tuning alloy process of the LF furnace refining is 400NL / min-600NL / min, and the argon flow rate in the later stage of the LF furnace refining is 30NL / min-100NL / min.
[0019] Optionally, the set argon gas flow rate is 20NL / min-40NL / min, and the set time is 1min-3min.
[0020] Optionally, alloying the molten iron after converter smelting to obtain first molten steel comprises:
[0021] sequentially adding steel grit aluminum, slag washing material and metal alloy to the molten iron after converter smelting to alloy the molten iron to obtain first molten steel;
[0022] The metal alloy includes at least one of the following: metallic manganese and ferromanganese.
[0023] Optionally, before the step of sequentially adding steel grit aluminum, slag washing material and metal alloy to the molten iron after converter smelting for alloying to obtain the first molten steel, the step further comprises:
[0024] Blow argon into the ladle under the condition of set time;
[0025] The setting time is 2min-4min.
[0026] Optionally, before performing converter smelting on the molten iron and respectively controlling the argon flow rates at the early stage and the late stage of the converter smelting, the method further includes:
[0027] Under the conditions of set stirring parameters and set slag removal times, KR desulfurization is performed on the molten iron so that the molten iron reaches the target sulfur content;
[0028] The target sulfur content is ≤0.002 wt %;
[0029] The setting stirring parameters include: stirring time ≥ 10min, stirring speed ≤ 140rpm, stirring depth ≥ 1400mm;
[0030] The set scraping times is>2.
[0031] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0032] The method for smelting molten steel provided in the embodiment of the present application reduces the nitrogen content in molten steel by controlling the bottom blowing argon flow rate of the converter, alloying the molten steel, and controlling the bottom blowing argon flow rate and low nitrogen ferro-titanium alloy or pure titanium wire in the LF furnace refining process. The content of the present application solves the technical problem that it is difficult to reduce the nitrogen content in molten steel in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0034] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0035] Figure 1 A schematic flow chart of a method for smelting molten steel provided in an embodiment of the present application. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0037] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0038] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0039] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0040] In the first aspect, the present application provides a method for smelting molten steel, see Figure 1 , the method comprising:
[0041] S1, performing converter smelting on molten iron, and controlling the argon flow rate in the early stage and the late stage of the converter smelting respectively;
[0042] S2, alloying the molten iron after converter smelting to obtain first molten steel;
[0043] S3, performing LF furnace refining on the first molten steel, and respectively controlling the early temperature rising process, the alloy fine-tuning process and the late argon gas flow rate of the LF furnace refining;
[0044] S4. Under the condition of setting the argon gas flow rate, low nitrogen ferrotitanium and or pure titanium wire are added to the first molten steel after being refined in the LF furnace, and calcium wire is fed after waiting for a set time to obtain molten steel.
[0045] In this embodiment, the nitrogen content in the molten steel is reduced by controlling the bottom blowing argon flow rate of the converter, alloying the molten steel, controlling the bottom blowing argon flow rate of the LF furnace refining process, and controlling the low-nitrogen ferro-titanium alloy or pure titanium wire.
[0046] The positive effect of adding low nitrogen ferrotitanium and or pure titanium wire is that the molten steel is solid solution strengthened with titanium without increasing the nitrogen content in the molten steel.
[0047] In some embodiments, the argon flow rate in the early stage of the converter smelting is 800NL / min-1000NL / min, and the argon flow rate in the later stage of the converter smelting is 400NL / min-550NL / min.
[0048] In the embodiment of the present application, "the early stage of converter smelting" means the dephosphorization and desiliconization stage of steelmaking, from the start of oxygen blowing to about 5 minutes of oxygen blowing. In the early stage of the converter smelting, the positive effect of setting the argon flow rate to 800NL / min-1000NL / min is: meeting the kinetic conditions of the dephosphorization reaction. If the argon flow rate is too high, the gas flow rate will be too fast to a certain extent, which will cause molten steel to splash; if the argon flow rate is too low, the kinetic conditions will not be achieved to a certain extent, deep phosphorus cannot be removed, and the effect of deep dephosphorization cannot be achieved. If the bottom blowing argon flow rate is too large, it will cause serious splashing of molten steel, and the molten steel will be exposed to the air, causing oxygen and nitrogen absorption. If the bottom blowing argon flow rate is too small, the dephosphorization kinetic conditions cannot be met, and the bottom blowing argon flow rate is too small, resulting in poor dynamic stirring effect of the converter and low denitrification rate. Specifically, in the early stage of converter smelting, the argon flow rate can be 800NL / min, 850NL / min, 900NL / min, 950NL / min, 1000NL / min, etc.
[0049] In the embodiment of the present application, "the later stage of converter smelting" means the last 5 minutes close to the end of oxygen blowing. In the later stage of converter smelting, the positive effect of setting the argon flow rate to 400NL / min-550NL / min is: under the premise of satisfying the heating and stirring, a good denitrification effect is achieved. If the argon flow rate is too high, it will aggravate the bottom blowing effect to a certain extent, causing violent carbon-oxygen reaction and severe splashing of molten steel, and the molten steel is exposed to oxygen and nitrogen increase; if the argon flow rate is too low, it cannot meet the converter denitrification effect to a certain extent. According to the determination requirements of the nitrogen content of the smelting steel grade, specifically, in the later stage of converter smelting, the argon flow rate can be selected as 400NL / min, 450NL / min, 500NL / min, 550NL / min, etc.
[0050] In some embodiments, the molten iron is subjected to converter smelting, and the argon flow rates in the early and late stages of the converter smelting are respectively controlled, including:
[0051] The molten iron is subjected to converter smelting, and the argon flow rates in the early and late stages of the converter smelting are respectively controlled, as well as the process parameters of slag making and dephosphorization of the converter smelting.
[0052] In some embodiments, the process parameters of slag making and dephosphorization include: the distance between the oxygen lance position and the molten iron in the early stage of converter smelting, the ratio of slag making materials, the temperature of converter auxiliary lance probes TSC and TSO, and the amount of ore added.
[0053] In some embodiments, the distance between the oxygen lance position in the early stage of converter smelting and the molten iron is 210 mm-230 mm;
[0054] The proportion of the slag-making material is as follows: 40kg-44kg of lime and 16kg-20kg of light burnt are added to each ton of molten steel;
[0055] The temperature of the converter auxiliary gun probe TSC is ≤1580°C, and the temperature of the converter auxiliary gun probe TSO is 1610°C-1640°C;
[0056] The amount of the ore added is 800kg-1000kg.
[0057] The positive effect of setting the distance between the initial oxygen lance position and the molten iron to 210mm-230mm is: achieving the control of slag amount and alkalinity for slagging. If the distance between the initial oxygen lance position and the molten iron is too long, the reaction rate will be reduced to a certain extent, and the initial dephosphorization kinetic conditions cannot be met; if the distance between the initial oxygen lance position and the molten iron is too short, the reaction heating rate will be aggravated to a certain extent, reducing the dephosphorization rate, and the violent reaction will cause oxygen and nitrogen absorption. Specifically, the distance between the initial oxygen lance position and the molten iron can be 210mm, 220mm, 230mm, etc.
[0058] The positive effect of controlling the amount of lime added to 40kg-44kg: achieving deep dephosphorization effect. If the amount of lime added is too high, the processing cost will increase to a certain extent under the condition of sufficient deep dephosphorization; if the amount of lime added is too low, the deep dephosphorization effect will not be achieved to a certain extent. Specifically, the amount of lime added can be 40kg, 41kg, 42kg, 43kg, 44kg, etc.
[0059] The positive effect of controlling the amount of light burnt to be 16kg-20kg: ensuring good basicity and fluidity of the converter top slag. If the amount of light burnt added is too high, to a certain extent, too much light burnt will increase the processing cost, and at the same time, the heat loss in the reaction process will increase; if the amount of light burnt added is too low, to a certain extent, it will lead to serious dry-out during the converter blowing process, poor control of the top slag fluidity, and serious nitrogen increase in the later stage of the converter. Specifically, the amount of light burnt added can be 16kg, 17kg, 18kg, 19kg, 20kg, etc.
[0060] The positive effect of controlling the temperature of the converter auxiliary gun probe TSC to ≤ 1580°C is that the early temperature is low, which is conducive to achieving a strong dephosphorization effect. If the temperature of the converter auxiliary gun probe TSC is too high, the dephosphorization rate will be reduced to a certain extent, and the low phosphorus target cannot be achieved. Specifically, the temperature of the converter auxiliary gun probe TSC can be 1580°C, 1582°C, 1584°C, etc.
[0061] The positive effect of controlling the temperature of the converter auxiliary gun probe TSO to 1610℃-1640℃ is: meeting the processing requirements of the refining process....... If the temperature of the converter auxiliary gun probe TSO is too high, the phosphorus content will be controlled too high to a certain extent; if the temperature of the converter auxiliary gun probe TSO is too low, the refining station temperature will be too low to a certain extent, and the refining process will take a long time to heat up, causing the molten steel to absorb nitrogen and oxygen, which will deteriorate the quality of the molten steel. Specifically, the temperature of the converter auxiliary gun probe TSO can be 1610℃, 1620℃, 1630℃, 1640℃, etc.
[0062] The positive effect of controlling the amount of the ore added to 800kg-1000kg is that the ore is added during the dynamic process of converter smelting to adjust the slag condition. If the amount of the ore added is too high, it will cause a large temperature drop in the converter to a certain extent, and the terminal temperature requirement cannot be met; if the amount of the ore added is too low, it will cause a thin slag layer of foam slag in the late converter to a certain extent, and it will not be able to provide good protection for the molten steel. Specifically, the amount of ore added can be 800kg, 850kg, 900kg, 950kg, 1000kg, etc.
[0063] In some embodiments, the argon flow rate of the initial heating process of the LF furnace refining is 150NL / min-300NL / min, the argon flow rate of the fine-tuning alloy process of the LF furnace refining is 400NL / min-600NL / min, and the argon flow rate of the later stage of the LF furnace refining is 30NL / min-100NL / min.
[0064] During the heating process, setting the argon flow rate to 150NL / min-300NL / min has the positive effect of making the composition and temperature of the molten steel uniform and stable. If the argon flow rate is too high, it will cause the graphite electrode to be eroded and damaged to a certain extent, resulting in carbon increase in the molten steel; if the argon flow rate is too low, it will not be able to even out the temperature of the molten steel in the LF furnace to a certain extent, making the temperature of the molten steel in the LF furnace uneven, resulting in an increase in the carbon content of some molten steel, and the top slag cannot be fully melted, resulting in serious nitrogen increase in the refining process, worsening the molten steel accident. Specifically, during the heating process, the argon flow rate can be 150NL / min, 170NL / min, 190NL / min, 210NL / min, 230NL / min, 250NL / min, 270NL / min, 290NL / min, etc.
[0065] In the process of fine-tuning the alloy, setting the argon flow rate to 400NL / min-600NL / min has the positive effect of: the composition in the LF furnace is uniform and stable. If the argon flow rate is too high, it will cause the molten steel to be exposed to a certain extent, which is easy to cause secondary oxidation of the molten steel, absorb nitrogen and oxygen in the air, and cause foreign inclusions in the molten steel; if the argon flow rate is too low, it will cause the alloy in the molten steel to be uniform for too long to a certain extent, and the kinetic conditions of desulfurization cannot be met. Specifically, in the process of fine-tuning the alloy, the argon flow rate can be 400NL / min, 450NL / min, 500NL / min, 550NL / min, 600NL / min, etc.
[0066] In the later process, the positive effect of setting the argon flow rate to 30NL / min-100NL / min is that the inclusions in the molten steel are fully floated and removed with the fine argon bubbles. If the argon flow rate is too high, it will cause the steel slag interface to fluctuate greatly to a certain extent, and the top slag of refining will be drawn into the molten steel, polluting the molten steel; if the argon flow rate is too low, it will not be able to promote the floating of fine inclusions to a certain extent, and the dynamic conditions are insufficient. Specifically, in the later process, the argon flow rate can be 30NL / min, 50NL / min, 70NL / min, 90NL / min, etc.
[0067] In some embodiments, the set argon gas flow rate is 20NL / min-40NL / min, and the set time is 1min-3min.
[0068] The positive effect of setting the flow rate of the third argon gas to 20NL / min-40NL / min is: it ensures that titanium is fully melted without being reoxidized by air. If the flow rate of argon gas is too high, it will cause strong stirring of molten steel to a certain extent, and the molten steel surface will be exposed to the air, causing the molten steel to absorb oxygen and nitrogen; if the flow rate of argon gas is too low, it will cause titanium iron to fail to fully melt to a certain extent, and the refining end composition will not meet the set requirements of the steel grade. Specifically, the flow rate of the third argon gas can be 20NL / min, 30NL / min, 40NL / min, etc.
[0069] The positive effect of setting the time to 1min-3min is that the titanium iron is fully melted and mixed in the ladle. If the waiting time is too long, the temperature drop of the molten steel will increase to a certain extent, and the smelting cost will increase; if the waiting time is too short, the titanium iron will not be fully melted to a certain extent. Specifically, the waiting time can be 1min, 2min, 3min, etc.
[0070] In some embodiments, alloying the molten iron after converter smelting to obtain first molten steel comprises:
[0071] sequentially adding steel grit aluminum, slag washing material and metal alloy to the molten iron after converter smelting to alloy the molten iron to obtain first molten steel;
[0072] The metal alloy includes at least one of the following: metallic manganese and ferromanganese.
[0073] The positive effect of controlling the order of adding steel grit aluminum, slag washing material and metal alloy: first add steel grit aluminum for deoxidation, then add slag washing material 1 minute after steel tapping, and use the steel tapping dynamic conditions to fully melt the slag washing material, so that the slag washing material plays a good role in heat preservation and protection between molten steel and air. Finally, add metal alloy to prevent excessive addition during the refining process. For full melting, a large argon flow rate must be opened for stirring to avoid a large amount of nitrogen addition in the refining process.
[0074] Positive effects of metallic manganese and ferromanganese: low-carbon ferromanganese and metallic manganese have low costs, high and stable absorption rates, and low alloy carbon and phosphorus content, meeting low-carbon and low-phosphorus design requirements.
[0075] In some embodiments, before the step of sequentially adding steel grit aluminum, slag washing material and metal alloy to the molten iron after converter smelting for alloying to obtain the first molten steel, the step further comprises:
[0076] Blow argon into the ladle under the condition of set time;
[0077] The setting time is 2min-4min.
[0078] The positive effect of blowing argon into the ladle is to fully fill the ladle with argon inert gas, exhaust the air, and avoid the increase of oxygen and nitrogen in the molten steel.
[0079] The positive effect of controlling the pre-blowing time of argon in the ladle to 2min-4min is: without affecting the temperature drop of the refractory material on the inner wall of the ladle, the ladle is fully filled with argon inert gas, the air is emptied, and the molten steel is prevented from increasing oxygen and nitrogen. If the time is too long, the temperature drop of the refractory material on the inner wall of the ladle will be large to a certain extent, and the refining process conditions cannot be met; if the time is too short, the ladle will not be fully filled with argon inert gas to a certain extent. Specifically, the time can be 2min, 3min, 4min, etc.
[0080] In some embodiments, before performing converter smelting on molten iron and controlling the argon flow rates in the early and late stages of the converter smelting respectively, the method further comprises:
[0081] Under the conditions of set stirring parameters and set slag removal times, KR desulfurization is performed on the molten iron so that the molten iron reaches the target sulfur content;
[0082] The target sulfur content is ≤0.002 wt %;
[0083] The setting stirring parameters include: stirring time ≥ 10min, stirring speed ≤ 140rpm, stirring depth ≥ 1400mm;
[0084] The set scraping times is>2.
[0085] The positive effects of controlling the target sulfur content to ≤ 0.002 wt% are: improving the bonding strength between grains of steel, improving the low-temperature impact toughness and plasticity of steel. If the target sulfur content is too high, the low-temperature impact toughness of steel will be reduced to a certain extent. At the same time, sulfur elements will segregate and enrich in the steel, reducing the corrosion resistance of the steel, and reducing the plasticity and toughness of the steel. Specifically, the target sulfur content can be 0.002 wt%, 0.0015 wt%, 0.001 wt%, etc.
[0086] The positive effect of a stirring time ≥ 10min is to satisfy the time required for the desulfurizer to fully react with the sulfur in the molten iron; the positive effect of a stirring speed ≤ 140rpm is to prevent the molten iron from splashing out of the ladle, resulting in a low molten iron yield; the positive effect of a stirring depth ≥ 1400mm is to promote the desulfurizer to fully react with the molten iron at the bottom of the ladle. A stirring time that is too short, and / or a stirring speed that is too high, and / or a stirring depth that is too low will, to a certain extent, cause the final sulfur content of the molten iron to fail to reach the target value. Specifically, the stirring time can be 10min, 11min, 12min, etc.; the stirring speed can be 140rpm, 142rpm, 144rpm, etc.; the stirring depth can be 1400mm, 1410mm, 1420mm, etc.
[0087] The positive effect of setting the number of slag removal to >2 is that the desulfurized top slag is fully removed from the iron ladle. If the number of slag removal is too small, the desulfurized top slag in the iron ladle cannot be fully emptied to a certain extent, so that the top slag is brought into the converter, and after being fully stirred in the converter, the sulfur in the slag is brought into the molten steel. Specifically, the number of slag removal can be 3, 4, etc.
[0088] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0089] The chemical composition of the molten steel obtained in each embodiment and comparative example is shown in Table 1:
[0090] Table 1
[0091]
[0092] The process parameters of the preparation methods of various embodiments and comparative examples are shown in Table 2:
[0093] Table 2
[0094]
[0095]
[0096] By controlling the bottom blowing argon flow rate of the converter, alloying the molten steel, controlling the bottom blowing argon flow rate of the LF furnace refining process and low nitrogen ferro-titanium alloy or pure titanium wire, the nitrogen content in the molten steel is reduced. The content of this application solves the technical problem that it is difficult to reduce the nitrogen content in the molten steel in the prior art. The final N content in the molten steel is obtained from Table 1. The change of the N content in each molten steel smelting stage is obtained from Table 2.
[0097] Secondly, by controlling the bottom blowing gas supply mode in the converter process to be divided into two stages with different flow rates, and then by limiting the temperature range of the slag making material added in the early slag making and dephosphorization of the converter and the converter auxiliary gun probe TSC and TSO, the removal of harmful elements in the converter steelmaking process can be accurately controlled. At the same time, the sequence of the steelmaking alloying process can be controlled, and the removal of harmful elements in the molten steel and the stability of other components can be further controlled, thereby achieving stable control of the composition of the steel.
[0098] The stirring, stirring speed and stirring depth of KR stirring paddle will affect the desulfurization effect. By adopting the stirring method of KR stirring paddle and controlling the stirring speed and stirring depth as well as the bottom blowing argon flow rate of the LF furnace process, the kinetic conditions for molten steel desulfurization can be achieved and the purpose of deep desulfurization can be achieved. The deep dephosphorization effect can be achieved by controlling the amount of slag material added to the converter and the temperature range of the converter auxiliary gun probe TSC and TSO.
[0099] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for smelting molten steel, characterized in that: The method comprises: Perform converter smelting on molten iron, and respectively control the argon flow rate in the early and late stages of the converter smelting, and control the process parameters of slag making and dephosphorization in the converter smelting; Alloying the molten iron after converter smelting to obtain first molten steel; Performing LF furnace refining on the first molten steel, and controlling the early temperature rising process, the alloy fine-tuning process and the late argon gas flow rate of the LF furnace refining respectively; Under the condition of setting the argon gas flow rate, adding low-nitrogen ferrotitanium and or pure titanium wire to the first molten steel after being refined in the LF furnace, and feeding calcium wire after waiting for a set time to obtain molten steel; The early stage of converter smelting is the dephosphorization and desiliconization stage of steelmaking, from the start of oxygen blowing to 5 minutes of oxygen blowing, and the late stage of converter smelting is the last 5 minutes near the end of oxygen blowing. The argon flow rate in the early stage of converter smelting is 800NL / min-1000NL / min, and the argon flow rate in the late stage of converter smelting is 400NL / min-550NL / min. The process parameters of slag making and dephosphorization include: the distance between the oxygen lance position and the molten iron in the early stage of the converter smelting is 210mm-230mm; the proportion of slag making material: 40kg-44kg of lime and 16kg-20kg of light burning are added to each ton of molten steel; the temperature of the converter auxiliary lance probe TSC is ≤1580℃, and the temperature of the converter auxiliary lance probe TSO is 1610℃-1640℃; the amount of ore added is 800kg-1000kg; The argon flow rate in the early heating process of the LF furnace refining is 150NL / min-300NL / min, the argon flow rate in the fine-tuning alloy process of the LF furnace refining is 400NL / min-600NL / min, the argon flow rate in the later stage of the LF furnace refining is 30NL / min-100NL / min, the set argon flow rate is 20NL / min-40NL / min, and the set time is 1min-3min.
2. The method according to claim 1, characterized in that Alloying the molten iron after converter smelting to obtain first molten steel, comprising: sequentially adding steel grit aluminum, slag washing material and metal alloy to the molten iron after converter smelting to alloy the molten iron to obtain first molten steel; The metal alloy includes at least one of the following: manganese and ferromanganese.
3. The method according to claim 2, characterized in that Before the steel sand aluminum, slag washing material and metal alloy are sequentially added to the molten iron after converter smelting for alloying to obtain the first molten steel, the method further comprises: Blow argon into the ladle under the condition of set time; The setting time is 2min-4min.
4. The method according to claim 1, characterized in that Before performing converter smelting on molten iron and respectively controlling the argon flow rate in the early stage and the late stage of the converter smelting, the method further includes: Under the conditions of set stirring parameters and set slag removal times, KR desulfurization is performed on the molten iron so that the molten iron reaches the target sulfur content; The target sulfur content is ≤0.002% by weight; The setting stirring parameters include: stirring time ≥ 10min, stirring speed ≤ 140rpm, stirring depth ≥ 1400mm; The set scraping times is>2.