A porous carbon nanofiber material with parallel pore structure and preparation method thereof
By using porous carbon nanofiber materials with an array-like parallel arrangement of pore structures in potassium-ion batteries, the problem of poor cycle stability of anode materials in potassium-ion batteries is solved, and battery performance with high capacity and long life is achieved.
Patent Information
- Application Number
- CN202310059994.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-01-18
AI Technical Summary
The cycle stability of potassium-ion battery anode materials is poor, mainly due to the large ionic radius of potassium ions causing the anode volume to expand. Existing carbon-based anode materials have problems such as high preparation cost, low initial Coulombic efficiency and low reversible capacity, making it difficult to achieve high Controlled synthesis.
Porous carbon nanofiber materials with an array-like parallel arrangement of pores are used to form a spinning liquid in N,N-dimethylformamide through cobalt acetate, polymethyl methacrylate, polyacrylonitrile and polystyrene. After spinning, it is carbonized at high temperature to form porous carbon nanofibers with a diameter of about 50 nm, which can effectively buffer the volume change of the anode material.
It has achieved excellent capacity and ultra-long battery life of the potassium ion battery cathode material, with a capacity of 309mA h g-1 at a current density of 0.2 A g-1 and a reversible capacity of 252mA h g-1 after 3000 cycles, significantly improving cycle stability. .
Smart Images

Figure CN116005299B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon fiber material preparation, and in particular to a porous nanofiber material with a parallel pore structure and a preparation method thereof. Background Art
[0002] Potassium-ion batteries (KIBs) are promising candidates due to their abundant reserves, non-toxic properties, and a “rocking chair” mechanism similar to lithium-ion batteries (LIBs). + / K is -2.93 V, close to the standard reduction potential of LIBs (Li + / Li is -3.04 V), which makes PIBs a powerful alternative to LIBs. However, K + The ionic radius of Li (1.38 nm) is larger than that of Li + (0.76 nm), which will be + The intercalation / deintercalation process leads to volume expansion of the anode, which results in poor cycling stability of the anode material. Therefore, designing suitable anode materials with high reversibility and stable structure for PIBs remains a great challenge.
[0003] Carbon nanomaterials have attracted extensive attention due to their excellent performance. According to existing reports, K ions can be inserted into the graphite interlayer of carbon nanomaterials to form KC8 phase (theoretical capacity is 278 mAh g -1 ). However, due to the large ionic radius of K ions, the (002) plane distance of the graphite layer expands from 0.335nm to 0.532nm during the intercalation process, resulting in a large volume change of the anode material (about 61%), which makes the carbon nanomaterial have poor cycle stability and serious capacity decay. In order to buffer and overcome the huge volume expansion of the anode material, various carbon nanostructures such as soft carbon, hard carbon, graphene, carbon nanotubes (CNT), carbon fiber, carbon foam and amorphous carbon have been developed as KIB anodes in the prior art. However, these carbon-based anode materials still have various disadvantages, including high preparation cost, low initial coulombic efficiency (ICE), low reversible capacity and low cycle stability. For example, the article "Enabling Superior Electrochemical Properties for Highly Efficient Potassium Storage by Impregnating Ultrafine Sb Nanocrystals within Nanochannel-Containing Carbon Nanofibers" published by Xufang Ge et al. improves the capacity of carbon nanofibers by impregnating Sb in carbon nanofibers, and at a current density of 0.2Ag -1 Its capacity reaches 392mAg-1 However, without the infiltration of Sb, the capacity of the prepared carbon nanofibers is only 258 mAg -1 Therefore, the controllable synthesis of ordered porous carbon anode materials remains a great challenge. Summary of the invention
[0004] The present invention aims to provide a porous nanofiber material having an array-like parallel pore structure, which has excellent capacity and cycle stability when used as a positive electrode material for potassium ion batteries (KIBs).
[0005] Another object of the present invention is to provide a method for preparing the above-mentioned porous nanofiber material having an array-like parallel pore structure.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] A porous carbon nanofiber material with a parallel pore structure, characterized in that: the porous carbon nanofiber has a diameter of 50nm, has an array-arranged through-hole structure parallel to the fiber, and the porous carbon fiber is made of cobalt acetate, polymethyl methacrylate (PMMA), polyacrylonitrile (PAN) and polystyrene (PS) dissolved in N,N-dimethylformamide (DMF) to form a spinning solution, which is obtained by electrospinning and then high-temperature carbonization.
[0008] Furthermore, the mass volume ratio of the above-mentioned cobalt acetate, PMMA, PAN, PS and DMF is 0.6-0.7 mg: 0.5 mg: 0.9 g: 0.3 mg: 10 mL.
[0009] Furthermore, the spinning solution is prepared by heating DMF to 50-60° C., then adding cobalt acetate, PMMA, PAN and PS under stirring at 500-600 rpm, and continuously stirring for 10-12 hours.
[0010] Furthermore, the electrospinning is performed such that the length of the spinning needle and the collector is 17-20 cm, the feed rate is 1 mL / h, the spinning voltage is 18 kV, and the collected fibers are dried at 60° C. after spinning.
[0011] Furthermore, during the above-mentioned high-temperature carbonization, the dried fiber is carbonized in two stages, specifically, the temperature is raised to 250-260°C at 2°C / min in an air atmosphere, kept warm for 2 hours, then raised to 850-900°C at 5°C / min, and then a mixed gas of H2 and Ar is introduced and kept warm for 2 hours, with a volume ratio of H2 to Ar being 5:95.
[0012] A method for preparing a porous carbon nanofiber material with parallel channels, characterized in that cobalt acetate, polymethyl methacrylate (PMMA), polyacrylonitrile (PAN) and polystyrene (PS) are dissolved in N,N-dimethylformamide (DMF) to form a spinning solution, electrospinning to obtain nanofibers, and then carbonizing at high temperature.
[0013] In the present invention, cobalt acetate is used as a catalyst, PMMA, PAN and PS are used as composite carbon sources, and the composite of different multi-path carbon sources forms a fiber structure with a smaller diameter under the action of the catalyst and the participation of PMMA. PAN and PS form preliminary pores in the fiber, and after decomposition during high-temperature carbonization, parallel pores arranged in an array are formed, and pores with a larger diameter are formed in the fiber with a smaller diameter. When the porous carbon nanofiber with this structure is used as an anode material for potassium ion batteries, K + The embedding and de-embedding of the material can be effectively suppressed.
[0014] Furthermore, the mass volume ratio of the above-mentioned cobalt acetate, PMMA, PAN, PS and DMF is 0.6-0.7 mg: 0.5 mg: 0.9 g: 0.3 mg: 10 mL.
[0015] Furthermore, the spinning solution is prepared by heating DMF to 50-60° C., then adding cobalt acetate, PMMA, PAN and PS under stirring at 500-600 rpm, and continuously stirring for 10-12 hours.
[0016] Furthermore, the electrospinning is performed such that the length of the spinning needle and the collector is 17-20 cm, the feed rate is 1 mL / h, the spinning voltage is 18 kV, and the collected fibers are dried at 60° C. after spinning.
[0017] Furthermore, during the above-mentioned high-temperature carbonization, the dried fiber is carbonized in two stages, specifically, the temperature is raised to 250-260°C at 2°C / min in an air atmosphere, kept warm for 2 hours, then raised to 850-900°C at 5°C / min, and then a mixed gas of H2 and Ar is introduced and kept warm for 2 hours, with a volume ratio of H2 to Ar being 5:95.
[0018] A method for preparing a porous carbon nanofiber material with a parallel pore structure, characterized by following the steps:
[0019] Step 1: Electrospinning to prepare fibers
[0020] (1) Heat DMF to 50-60°C, then add cobalt acetate, PMMA, PAN and PS under stirring at 500-600 rpm, and continue stirring for 10-12 hours to form a spinning solution. The mass volume ratio of cobalt acetate, PMMA, PAN, PS and DMF is 0.6-0.7 mg: 0.5 mg: 0.9 g: 0.3 mg: 10 mL;
[0021] (2) electrospinning the spinning solution, wherein the distance between the spinning needle and the collector is 17-20 cm, the feed rate is 1 mL / h, the spinning voltage is 18 kV, and after the spinning is completed, the collected fibers are dried at 60° C.;
[0022] Step 2: High temperature carbonization treatment
[0023] The dried fiber was heated to 250-260°C at 2°C / min in an air atmosphere, kept warm for 2 hours, then heated to 850-900°C at 5°C / min, and then a mixed gas of H2 and Ar was introduced and kept warm for 2 hours, with a volume ratio of H2 to Ar being 5:95.
[0024] The present invention has the following technical effects:
[0025] The porous carbon nanofiber material with an array of parallel pores prepared by the method of the present invention has a diameter of about 50 nanometers and a length of several tens of micrometers. The parallel pores in its structure are conducive to the infiltration of electrolytes. Therefore, when it is used as a positive electrode material for potassium ion batteries, it has excellent ion conductivity and ultra-long battery life. When the porous carbon nanofiber material with an array of parallel pores is used as a positive electrode material for potassium ion batteries, the current density is 0.2 A g -1 When the capacity is 309mA g -1 After 100 cycles, the reversible capacity is 285 mA h g -1 After 3000 cycles, it has a current of 252 mA hg -1 Reversible capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 : Schematic diagram of the structure of the porous carbon nanofiber material with array-like parallel pore structure prepared by the present invention.
[0027] Figure 2 : Scanning electron microscope image of the porous carbon nanofiber material with array-like parallel pore structure prepared by the present invention.
[0028] Figure 3 : Transmission electron micrograph of the porous carbon nanofiber material with array-like parallel pore structure prepared by the present invention.
[0029] Figure 4 : X-ray diffraction pattern of the porous carbon nanofiber material with array-like parallel pore structure prepared by the present invention.
[0030] Figure 5 : Rate-cycle performance comparison curve of the porous carbon nanofiber material with array-like parallel pore structure prepared by the present invention and the solid carbon nanofiber prepared in Comparative Example 1 at different current densities.
[0031] Figure 6 : Comparison of the cyclic stability of the porous carbon nanofiber material with array-like parallel pore structure prepared by the present invention and the solid carbon nanofiber prepared by comparison 1.
[0032] Figure 7 : Rate-cycle performance comparison curve of the porous carbon nanofiber material with array-like parallel pore structure prepared by the present invention and the solid carbon nanofiber prepared in Comparative Example 2 at different current densities.
[0033] Figure 8 : Comparison of the cyclic stability of the porous carbon nanofiber material with array-like parallel pore structure prepared by the present invention and the solid carbon nanofiber prepared by comparison 2. Implementation
[0034] The present invention is described in detail below through examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above-mentioned contents of the present invention. Example
[0035] A method for preparing a porous carbon nanofiber material with a parallel pore structure, characterized by following the steps:
[0036] Step 1: Electrospinning to prepare fibers
[0037] (1) DMF was heated to 50°C, and then cobalt acetate, PMMA, PAN and PS were added under stirring at 600 rpm and continued to stir for 12 h to form a spinning solution. The mass volume ratio of cobalt acetate, PMMA, PAN, PS and DMF was 0.7 mg: 0.5 mg: 0.9 g: 0.3 mg: 10 mL;
[0038] (2) electrospinning the spinning solution, wherein the length of the spinning needle and the collector is 17 cm, the feed rate is 1 mL / h, the spinning voltage is 18 kV, and after the spinning is completed, the collected fibers are dried at 60 ° C;
[0039] Step 2: High temperature carbonization treatment
[0040] The dried fiber was heated to 260°C at 2°C / min in an air atmosphere and kept warm for 2 hours. Then, the temperature was raised to 900°C at 5°C / min, and a mixed gas of H2 and Ar was introduced and kept warm for 2 hours. The volume ratio of H2 and Ar was 5:95.
[0041] Figure 1 Schematic diagram of the structure of the porous carbon nanofiber with array-arranged parallel pore structure prepared by the present invention, such as Figure 2 and Figure 3 As shown, the average diameter of the carbon nanofibers prepared by the present invention is 50 nm, and the fibers have channels parallel to the fibers to form an array arrangement, and the channel diameter is large, which is beneficial to K + Effectively relieve K + The volume deformation caused by the embedding and unembedding process. The X-ray diffraction pattern of the carbon nanofiber prepared by the present invention is as follows Figure 4 As shown, the present invention forms a pure carbon material without any residual carbon raw material and cobalt acetate as a catalyst.
[0042] Comparative Example 1:
[0043] Compared with Example 1, PMMA was not added when preparing the spinning solution, and the remaining steps were consistent with Example 1.
[0044] Although the carbon nanofibers prepared in Comparative Example 1 also formed a parallel pore structure, the diameter of the carbon nanofibers was larger, with an average diameter of 500 nm, and the pore size was smaller than that in Example 1, which was not conducive to K + A large number of embedding, K + The embedding and unembedding process can easily cause a large volume change in the carbon nanofiber material. Figure 5 and Figure 6 As shown in the figure, when the carbon nanofibers prepared in Comparative Example 1 and Example 1 are used as positive electrode materials for potassium ion batteries, the current density is 0.2 A g -1 309 mAh g -1 After 100 cycles, its reversible capacity is 285 mA h g -1 After 3000 cycles, it has a capacitance of 252 mA hg -1 The reversible capacity of carbon nanofibers prepared in Comparative Example 1 was 0.2 A g -1 When the -1 After 3000 cycles, the capacity decayed severely and was only 22 mA h g -1 Reversible capacity.
[0045] Comparative Example 2
[0046] Compared with Example 1, the difference is that PAN and PS are not added when preparing the spinning solution, and the other steps are consistent with Example 1. The prepared carbon nanofibers are solid structures without array-arranged parallel channels inside. Figure 7 and Figure 8 As shown, the carbon nanofibers prepared in Comparative Example 2 were -1 When the -1 After 100 cycles, the reversible capacity is 67 mA h g -1 . Example
[0047] A method for preparing a porous carbon nanofiber material with a parallel pore structure, characterized by following the steps:
[0048] Step 1: Electrospinning to prepare fibers
[0049] (1) DMF was heated to 55°C, and then cobalt acetate, PMMA, PAN and PS were added under stirring at 550 rpm and stirred for 11 h to form a spinning solution. The mass volume ratio of cobalt acetate, PMMA, PAN, PS and DMF was 0.65 mg: 0.5 mg: 0.9 g: 0.3 mg: 10 mL;
[0050] (2) electrospinning the spinning solution, wherein the length of the spinning needle and the collector is 18 cm, the feed rate is 1 mL / h, the spinning voltage is 18 kV, and after the spinning is completed, the collected fibers are dried at 60 ° C;
[0051] Step 2: High temperature carbonization treatment
[0052] The dried fiber was heated to 255°C at 2°C / min in an air atmosphere and kept at this temperature for 2 hours. Then, the temperature was raised to 880°C at 5°C / min, and a mixed gas of H2 and Ar was introduced and kept at this temperature for 2 hours. The volume ratio of H2 to Ar was 5:95.
[0053] When the carbon nanofibers prepared in this example are used as the positive electrode material of potassium ion batteries, the current density is 0.2 A g -1 305 mA hg -1 After 3000 cycles, it has a capacity of 260 mA hg -1 Reversible capacity. Example
[0054] A method for preparing a porous carbon nanofiber material with a parallel pore structure, characterized by following the steps:
[0055] Step 1: Electrospinning to prepare fibers
[0056] (1) DMF was heated to 60°C, and then cobalt acetate, PMMA, PAN and PS were added under stirring at 500 rpm and continued to stir for 10 h to form a spinning solution. The mass volume ratio of cobalt acetate, PMMA, PAN, PS and DMF was 0.6 mg: 0.5 mg: 0.9 g: 0.3 mg: 10 mL;
[0057] (2) electrospinning the spinning solution, wherein the length of the spinning needle and the collector is 20 cm, the feed rate is 1 mL / h, the spinning voltage is 18 kV, and after the spinning, the collected fibers are dried at 60 °C;
[0058] Step 2: High temperature carbonization treatment
[0059] The dried fiber was heated to 250°C at 2°C / min in an air atmosphere and kept warm for 2 hours. Then, the temperature was raised to 850°C at 5°C / min, and a mixed gas of H2 and Ar was introduced and kept warm for 2 hours. The volume ratio of H2 and Ar was 5:95.
[0060] When the carbon nanofibers prepared in this example are used as the positive electrode material of potassium ion batteries, the current density is 0.2 A g -1 316 mA hg -1 After 3000 cycles, it has a capacity of 251mA hg -1 Reversible capacity.
Claims
1. A porous carbon nanofiber material with a parallel pore structure, characterized in that: The porous carbon nanofiber has a diameter of 50nm and has an array-arranged through-hole structure parallel to the fiber. The porous carbon nanofiber is prepared by dissolving cobalt acetate, polymethyl methacrylate (PMMA), polyacrylonitrile (PAN) and polystyrene (PS) in N,N-dimethylformamide (DMF) to form a spinning solution, and then high-temperature carbonization is performed after electrospinning. The mass volume ratio of the cobalt acetate, PMMA, PAN, PS and DMF is 0.6-0.7mg:0.5mg:0.9g:0.3mg:10mL. The high-temperature carbonization is a two-stage carbonization of the dried fiber, specifically, heating to 250-260°C at 2°C / min in an air atmosphere, keeping the temperature for 2h, then heating to 850-900°C at 5°C / min, and then introducing a mixed gas of H2 and Ar, keeping the temperature for 2h, and the volume ratio of H2 to Ar is 5:
95.
2. A method for preparing the porous carbon nanofiber material with parallel pore structure as claimed in claim 1, characterized in that: Cobalt acetate, polymethyl methacrylate (PMMA), polyacrylonitrile (PAN) and polystyrene (PS) are dissolved in N,N-dimethylformamide (DMF) to form a spinning solution, which is then electrospun to obtain nanofibers and then carbonized at high temperature.
3. The method for preparing a porous carbon nanofiber material having a parallel pore structure according to claim 2, characterized in that: The mass volume ratio of the cobalt acetate, PMMA, PAN, PS and DMF is 0.6-0.7 mg: 0.5 mg: 0.9 g: 0.3 mg: 10 mL.
4. The method for preparing a porous carbon nanofiber material having a parallel pore structure according to claim 2 or 3, characterized in that: The spinning solution is prepared by heating DMF to 50-60° C., then adding cobalt acetate, PMMA, PAN and PS under stirring at 500-600 rpm, and continuously stirring for 10-12 hours.
5. The method for preparing a porous carbon nanofiber material having a parallel pore structure according to claim 4, characterized in that: The electrospinning process is performed at a distance of 17-20 cm between the spinning needle and the collector, a feed rate of 1 mL / h, a spinning voltage of 18 kV, and after spinning, the collected fibers are dried at 60° C.