Carbon material for adsorbing carbon monoxide, preparation method thereof, and carbon monoxide adsorption method
By calculating the divalent copper salt, copper carboxylate and lignin under the blending of alkali metal salts, the problems of limited adsorption capacity of carbon monoxide and complex preparation process in the prior art are solved, and high efficiency and low cost are achieved Carbon material preparation and adsorption effect.
Patent Information
- Application Number
- CN202210575970.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-10-27
- Filing Date
- 2022-05-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-05-25
AI Technical Summary
The adsorption capacity of existing materials used to adsorb carbon monoxide is limited, the preparation process is complex and costly, which affects the effective removal of carbon monoxide in hydrogen fuel cells.
The carbon material with cuprous group load is prepared by mixing divalent copper salts, copper carboxylate and lignin with alkali metal salts, and the high carbon content of lignin and the activation of alkali metal salts are used. It can improve the specific surface area and pore structure of the material and enhance the adsorption performance of carbon monoxide.
Carbon materials with high specific surface area and rich pore structure have been achieved, which significantly improves the adsorption capacity of carbon monoxide, is simple in preparation process and cheap raw materials, which reduces the preparation cost and improves the adsorption performance.
Smart Images

Figure CN116020412B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon material preparation, and in particular to a carbon material for adsorbing carbon monoxide, a preparation method thereof, and a method for adsorbing carbon monoxide. Background Art
[0002] Hydrogen fuel cell vehicles are a promising new energy vehicle development direction, with advantages such as zero emissions, high energy conversion efficiency, and a wide range of fuel sources. A stable, reliable, and low-cost hydrogen source is the basic condition for the large-scale application of fuel cell vehicles. The production, storage, and transportation of hydrogen all have the problem of complex impurity gas pollution. Among them, because carbon monoxide can cause irreversible carbon corrosion and other permanent damage to the electrodes in the fuel cell, the carbon monoxide content limit in hydrogen has reached below 200ppb.
[0003] Activated carbon is a black powder or amorphous carbon material in block, granular, or honeycomb form. In addition to carbon, activated carbon also contains oxygen and hydrogen. These elements remain in the carbon due to incomplete carbonization, or during the activation process, foreign non-carbon elements chemically combine with the surface of activated carbon. For example, when activated with water vapor, the surface of activated carbon is oxidized or oxidized by water vapor; the main raw materials of activated carbon can be almost all carbon-rich organic materials, such as coal, wood, fruit shells, coconut shells, walnut shells, apricot shells, jujube shells, etc. These carbon-containing materials are converted into activated carbon through pyrolysis at high temperature and a certain pressure in the activation furnace; activated carbon is widely used in industrial adsorption, catalyst preparation and other fields due to its good specific surface area and its easy access.
[0004] CN1683249A discloses a copper (I) chloride carbon monoxide adsorption material, which loads several copper precursors onto activated carbon and obtains a carbon monoxide adsorption material through high-temperature sintering, wherein the loading amount of the active component copper chloride is greater than 50%, and the carbon monoxide adsorption capacity is only 58 mL / g at normal temperature and pressure.
[0005] Ma J, Li L, Jin R et al. (CO adsorption on activated carbon-supported Cu-based adsorbent prepared by a facile route [J]. Separation & Purification Technology, 2010, 76 (1): 89-93.) used the principle of spontaneous monolayer dispersion to disperse CuCl on the surface of the carrier to prepare an efficient CO adsorbent, mixed CuCl with activated carbon, and calcined it at 350°C for several hours to obtain the adsorbent. Its maximum adsorption capacity for carbon monoxide at room temperature and pressure is only 56 mL / g.
[0006] The adsorbent materials for adsorbing carbon monoxide that have been developed in the prior art are mainly copper chloride (I) loaded on carriers including activated carbon, molecular sieves, alumina, etc., but the adsorption capacity of the above adsorbent materials is limited, which affects the depth of removal of carbon monoxide, and the loading amount of active components is very high, which also affects the economic development of materials. Therefore, it is necessary to develop a carbon-based adsorbent material with high adsorption capacity and simple preparation process. Summary of the invention
[0007] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and to provide a carbon material for adsorbing carbon monoxide and a preparation method thereof and a method for adsorbing carbon monoxide. The carbon material has a better carbon monoxide adsorption capacity, and its preparation process is simple, the raw materials are cheap, and the preparation cost is low.
[0008] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a carbon material for adsorbing carbon monoxide, the preparation method comprising the following steps:
[0009] (1) In the presence of a solvent, a divalent copper salt, a copper carboxylate, lignin, and an alkali metal salt are mixed to obtain a suspension;
[0010] (2) drying the suspension and then calcining it under an inert atmosphere;
[0011] (3) Washing and then drying the product obtained by calcining in step (2).
[0012] The second aspect of the present invention provides a carbon material for adsorbing carbon monoxide, which is prepared by the preparation method described in the first aspect.
[0013] A third aspect of the present invention provides a method for adsorbing carbon monoxide, the method comprising:
[0014] A gas containing carbon monoxide is brought into contact with a carbon material to adsorb the carbon monoxide contained in the gas onto the carbon material; wherein the carbon material is the carbon material described in the second aspect.
[0015] Through the above technical scheme, the preparation method provided by the present invention uses cheap lignin as a carbon source, utilizes its high carbon content, uniformly mixes divalent copper salt, copper carboxylate and lignin, and roasts and activates them under the mixing of alkali metal salts. This method can obtain a carbon material with a cuprous base load through a single roasting, and the preparation process is simple, the raw materials are cheap, and the preparation cost is low. In addition, due to the addition of alkali metal salts, the carbonization process of lignin is fully activated, which not only improves the dispersion of cuprous base active components in the carbon material, but also the obtained carbon material has a very high specific surface area and rich pore structure, which is more conducive to applications in the fields of adsorption and the like, and has good carbon monoxide adsorption performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 is the N2 adsorption-desorption isotherm of the carbon material prepared in Example 1;
[0017] Figure 2 is the BJH pore size distribution curve of the carbon material prepared in Example 1;
[0018] Figure 3 This is the XPS graph of the carbon material prepared in Example 1. DETAILED DESCRIPTION
[0019] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0020] A first aspect of the present invention provides a method for preparing a carbon material for adsorbing carbon monoxide, the method comprising the following steps:
[0021] (1) In the presence of a solvent, a divalent copper salt, a copper carboxylate, lignin, and an alkali metal salt are mixed to obtain a suspension;
[0022] (2) drying the suspension and then calcining it under an inert atmosphere;
[0023] (3) Washing and then drying the product obtained by calcining in step (2).
[0024] The inventors of the present invention discovered during the research process that lignin is a complex organic polymer that forms an important structural material in the supporting tissues of vascular plants and some algae. Chemically, lignin is a cross-linked phenolic polymer with a relatively high carbon content. In addition, the raw materials are abundant and inexpensive, so it can be used as an excellent raw material for synthesizing activated carbon-based adsorption materials.
[0025] According to some embodiments of the present invention, in step (1), in the presence of a solvent, a divalent copper salt, a copper carboxylate, lignin and an alkali metal salt are mixed to obtain a suspension. As long as a suspension can be obtained, the purpose of the present invention can be achieved, and the order of adding the materials is not particularly limited. In order to further improve the adsorption performance of the obtained carbon material, preferably, the mixing includes:
[0026] (1-1) first mixing a divalent copper salt, a copper carboxylate and a solvent to obtain a precursor solution;
[0027] (1-2) The precursor solution is mixed with lignin and alkali metal salt for a second time to obtain the suspension. The above preferred embodiment is conducive to promoting the dispersion of active components and promoting the dispersion of active components in the subsequent roasting process.
[0028] According to some embodiments of the present invention, preferably, in step (1-1), the first mixing includes heating and stirring; more preferably, the conditions of the heating and stirring include: a temperature of 60-80° C. and a time of 10-20 min.
[0029] According to some embodiments of the present invention, preferably, in step (1-2), the second mixing conditions include: under stirring, at a temperature of 60-80° C., and for 30-60 min.
[0030] According to some embodiments of the present invention, preferably, the molar ratio of the divalent copper salt to the copper carboxylate is 0.5-1.5: 1, preferably 0.85-1.25: 1. The molar ratio of the divalent copper salt to the copper carboxylate is within the above-defined range, which is conducive to promoting the formation of cuprous components.
[0031] According to some embodiments of the present invention, preferably, the divalent copper salt is selected from copper chloride and / or copper bromide.
[0032] According to some embodiments of the present invention, preferably, the copper carboxylate is selected from at least one of copper formate, copper acetate and copper citrate.
[0033] According to some embodiments of the present invention, preferably, the divalent copper salt and copper carboxylate are used in an amount such that the content of monovalent copper salt in the prepared carbon material is 20-50% by weight, preferably 25-45% by weight, based on the total weight of the carbon material. Preferably, the monovalent copper salt is selected from CuCl and / or CuBr.
[0034] According to some embodiments of the present invention, there is no particular limitation on the type of the solvent, as long as a suspension can be formed. Preferably, the solvent is water and / or ethanol, more preferably water. There is no particular limitation on the amount of the solvent, as long as a suspension can be formed.
[0035] According to some embodiments of the present invention, the alkali metal salt has a wide selection range, and conventional alkali metal salts in the art can be used. Preferably, the alkali metal salt is a potassium salt and / or a sodium salt, more preferably at least one of potassium chloride, potassium nitrate, potassium sulfate, sodium chloride, sodium nitrate and sodium sulfate, and more preferably potassium chloride. In step (1), the addition of the alkali metal salt helps to activate the carbonization process of lignin, so that it forms a structured material with a high specific surface area, and is also beneficial to increase the dispersion of the cuprous active component in the carbon material, thereby improving the adsorption effect of the carbon material on carbon monoxide.
[0036] According to some embodiments of the present invention, the selection range of the lignin is relatively wide, and conventional lignin in the art can be used. Preferably, the lignin is alkali-washed lignin.
[0037] According to some embodiments of the present invention, preferably, the mass ratio of the divalent copper salt to lignin is 0.2-1:1, preferably 0.25-0.5:1.
[0038] According to some embodiments of the present invention, preferably, the mass ratio of the alkali metal salt to lignin is 0.2-2: 1, preferably 0.5-1: 1. The mass ratio of the alkali metal salt to lignin within the above preferred range can effectively form a rich pore structure in the process of sintering lignin into carbon material.
[0039] According to some embodiments of the present invention, in step (2), the suspension is dried and then calcined under an inert atmosphere. Preferably, the drying is performed by rotary evaporation.
[0040] According to some embodiments of the present invention, preferably, the inert atmosphere is provided by an inert gas, and the inert gas is selected from at least one of nitrogen, helium, argon and neon.
[0041] According to some embodiments of the present invention, preferably, the calcination conditions include: a temperature of 200-950° C. and a time of 2-6 h; preferably, a flow rate of the inert gas is 5-200 mL / min.
[0042] According to some embodiments of the present invention, in step (3), the product obtained by calcining step (2) is washed and then dried. There is no particular limitation on the washing method, and conventional washing methods in the art can be used. Preferably, the washing comprises: dispersing the product obtained by calcining step (2) in an organic solvent.
[0043] According to some embodiments of the present invention, preferably, the organic solvent is selected from at least one of ethanol, methanol and glycerol.
[0044] According to some embodiments of the present invention, the preparation method uses cheap lignin as a carbon source, utilizes its high carbon content, uniformly mixes divalent copper salt, copper carboxylate and lignin, and roasts and activates them under the mixing of alkali metal salts. This method can obtain a carbon material with a cuprous base load through a single roasting, and the preparation process is simple, the raw materials are cheap, and the preparation cost is low. In addition, due to the addition of alkali metal salts, the carbonization process of lignin is fully activated, which is not only beneficial to improve the dispersion of cuprous base active components in the carbon material, but also beneficial to obtain a carbon material with a high specific surface area and a rich pore structure.
[0045] The second aspect of the present invention provides a carbon material for adsorbing carbon monoxide, which is prepared by the preparation method described in the first aspect.
[0046] According to some embodiments of the present invention, preferably, based on the total weight of the carbon material, the carbon content in the carbon material is 40-80% by weight, preferably 50-70% by weight.
[0047] According to some embodiments of the present invention, preferably, based on the total weight of the carbon material, the content of monovalent copper salt in the carbon material is 20-50% by weight, preferably 25-45% by weight; preferably, the monovalent copper salt is selected from CuCl and / or CuBr.
[0048] According to some embodiments of the present invention, preferably, based on the total weight of the carbon material, the content of oxygen in the carbon material is 1-10 wt %, preferably 1-8 wt %.
[0049] According to some embodiments of the present invention, the type and content of each component in the carbon material are determined by X-ray photoelectron spectroscopy (XPS). The X-ray photoelectron spectroscopy used is an ESCALab220i-XL X-ray electron spectrometer equipped with Avantage V5.926 software produced by VG Scientific. The X-ray photoelectron spectroscopy analysis test conditions are: the excitation source is monochromatic A1Kα X-ray, the power is 330W, and the basic vacuum during the analysis test is 3×10 -9 In addition, the electron binding energy was calibrated using the C1s peak (284.6 eV), and the subsequent peak separation software was XPSPEAK.
[0050] According to some embodiments of the present invention, preferably, in the pore size distribution curve of the carbon material, there are at least two mesopore distribution peaks; more preferably, in the pore size distribution curve of the carbon material, there is a first mesopore distribution peak at 2-10 nm, and a second mesopore distribution peak at 20-50 nm.
[0051] According to some embodiments of the present invention, preferably, the mesopore volume of the carbon material is 0.2-0.7 cm 3 / g, preferably 0.25-0.65cm 3 / g; preferably, the proportion of the mesopore volume of the carbon material to the total pore volume is greater than 30%, preferably greater than 40%.
[0052] According to some embodiments of the present invention, preferably, the BET specific surface area of the carbon material is 500-1000m 2 / g, preferably 500-900m 2 / g.
[0053] In the present invention, the term "mesopore" is defined as a pore with a pore size in the range of 2-50 nm.
[0054] In the present invention, the term "mesopore distribution peak" refers to a mesopore distribution peak on a pore distribution curve obtained by calculating a desorption curve according to the Barrett-Joyner-Halenda (BJH) method.
[0055] According to some embodiments of the present invention, the pore structure properties of the material are detected by the BET test method. Specifically, the specific surface area and pore volume of the material are obtained by the Brunauer-Emmett-Taller (BET) method, and the mesopore distribution curve is calculated by the desorption curve according to the Barrett-Joyner-Halenda (BJH) method.
[0056] According to some embodiments of the present invention, the carbon material for adsorbing carbon monoxide has a high specific surface area and a rich pore structure, and the cuprous-based active components have a high dispersion in the carbon material, which is more conducive to applications in fields such as adsorption and has good carbon monoxide adsorption performance.
[0057] A third aspect of the present invention provides a method for adsorbing carbon monoxide, the method comprising:
[0058] A gas containing carbon monoxide is brought into contact with a carbon material to adsorb the carbon monoxide contained in the gas onto the carbon material; wherein the carbon material is the carbon material described in the second aspect.
[0059] According to some embodiments of the present invention, preferably, the contacting conditions include: a temperature of 0-80°C and a pressure of 50-150 kPa; more preferably, the contacting is performed at room temperature (25°C) and normal pressure (100 kPa (1 Bar)). During the contacting process, the adsorption of carbon monoxide by the carbon material will cause a pressure drop, and gradually reach adsorption equilibrium, thereby obtaining an adsorbent adsorbed with carbon dioxide.
[0060] According to some embodiments of the present invention, preferably, the adsorption method also includes heating and / or reducing the pressure of the adsorbent adsorbed with carbon dioxide, and the heating and / or reducing the pressure can desorb the carbon monoxide adsorbed on the carbon material, thereby recovering the carbon material and recycling it for the adsorption of carbon monoxide.
[0061] According to some embodiments of the present invention, preferably, the heating conditions include: a temperature of 100-300° C. and a time of 0.5-3 hours.
[0062] According to some embodiments of the present invention, preferably, the decompression conditions include: a pressure of 0-0.01 kPa and a time of 0.5-3 hours.
[0063] According to some embodiments of the present invention, in order to improve the adsorption effect of the carbon material on carbon monoxide, preferably, the adsorption method also includes heating the carbon material in an inert gas environment or a reducing gas environment before the contact, and the heating treatment can remove impurities adsorbed on the surface of the material while ensuring that the metal active components do not undergo oxidation reaction.
[0064] According to some embodiments of the present invention, the carbon material may have an adsorption capacity for carbon monoxide of more than 45 mL / g at room temperature and pressure, and may be as high as 67.8 mL / g.
[0065] According to some embodiments of the present invention, the carbon monoxide adsorption capacity of the nano-metal composite adsorption material at room temperature and pressure is measured with reference to GB / T 19560-2008 "High-Pressure Isothermal Adsorption Experimental Method for Coal".
[0066] The present invention will be described in detail below by way of examples. In the following examples and comparative examples:
[0067] Unless otherwise specified, all reagents used in the present invention are analytically pure and commercially available.
[0068] The pore structure properties of the material were detected by the BET test method. Specifically, the Quantachrome AS-6B analyzer was used for the determination. The specific surface area and pore volume of the material were obtained by the Brunauer-Emmett-Taller (BET) method, and the mesopore distribution curve was calculated by the desorption curve according to the Barrett-Joyner-Halenda (BJH) method.
[0069] The elements on the surface of the material were detected by X-ray photoelectron spectroscopy (XPS). The X-ray photoelectron spectroscopy used was an ESCALab220i-XL X-ray electron spectrometer produced by VG Scientific and equipped with Avantage V5.926 software. The X-ray photoelectron spectroscopy analysis test conditions were as follows: the excitation source was monochromatic A1Kα X-ray, the power was 330W, and the basic vacuum during the analysis test was 3×10 -9 In addition, the electron binding energy was calibrated using the C1s peak (284.6 eV), and the subsequent peak separation software was XPSPEAK.
[0070] Adsorption and desorption of carbon monoxide: The test was carried out in accordance with GB / T 19560-2008 “High-pressure isothermal adsorption test method for coal”.
[0071] Examples 1-4 are used to illustrate carbon materials for adsorbing carbon monoxide and methods for preparing the same.
[0072] Example 1
[0073] Step 1, dissolving 3 g of copper chloride and 3.8 g of copper formate (the molar ratio of copper chloride to copper formate is 0.9:1) in deionized water, heating to 60° C. and stirring for 20 minutes to obtain a precursor solution;
[0074] Step 2, adding 10 g of lignin and 5 g of potassium chloride to the precursor solution and stirring at 60° C. for 30 minutes, and drying the obtained suspension by rotary evaporation to obtain material 1;
[0075] Step 3, carbonizing material 1 in a tubular furnace under nitrogen protection at 800° C. (nitrogen flow rate is 100 mL / min) for 120 minutes to obtain material 2;
[0076] Step 4: disperse the material 2 in ethanol, wash it, filter it, and dry it to obtain a carbon material for adsorbing carbon monoxide.
[0077] Characterization of materials:
[0078] Figure 1 is the N2 adsorption-desorption isotherm of the carbon material, Figure 2 is the BJH pore size distribution curve of the carbon material. It can be seen from the figure that the carbon material has two mesopore distribution peaks at 3.6nm and 32.1nm. The mesopore volume of the carbon material is 0.28cm 3 / g, accounting for 44% of the total pore volume; the BET specific surface area is shown in Table 1.
[0079] The X-ray photoelectron spectroscopy (XPS) of the carbon material is shown in Figure 3 As shown in the figure, it can be seen that the carbon material clearly has the XPS peak of CuCl. Based on the total weight of the carbon material, the carbon content in the carbon material is 61.7% by weight, the CuCl content is 32% by weight, and the oxygen content is 6.3% by weight.
[0080] Example 2
[0081] Step 1, dissolving 4 g of copper chloride and 4.5 g of copper formate (the molar ratio of copper chloride to copper formate is 1.02:1) in deionized water, heating to 60° C. and stirring for 20 minutes to obtain a precursor solution;
[0082] Step 2: adding 10 g of lignin and 8 g of potassium chloride to the precursor solution and stirring at 60° C. for 30 minutes, and drying the obtained suspension by rotary evaporation to obtain material 1;
[0083] Step 3, carbonizing material 1 in a tubular furnace under nitrogen protection at 800° C. (nitrogen flow rate is 100 mL / min) for 120 minutes to obtain material 2;
[0084] Step 4: disperse the material 2 in ethanol, wash it, filter it, and dry it to obtain a carbon material for adsorbing carbon monoxide.
[0085] Characterization of materials:
[0086] BET test shows that the carbon material has two mesopore distribution peaks at 2.5nm and 37.2nm. The mesopore volume of the carbon material is 0.27cm 3 / g, accounting for 41% of the total pore volume; the BET specific surface area is shown in Table 1.
[0087] XPS test shows that the carbon material clearly has an XPS peak of CuCl. Based on the total weight of the carbon material, the carbon content of the carbon material is 57.4% by weight, the CuCl content is 41.4% by weight, and the oxygen content is 1.2% by weight.
[0088] Example 3
[0089] Step 1, dissolve 2.5 g of copper chloride and 3 g of copper acetate (the molar ratio of copper chloride to copper acetate is 1.13:1) in deionized water, heat to 60° C. and stir for 20 minutes to obtain a precursor solution;
[0090] Step 2, adding 10 g of lignin and 5 g of sodium chloride to the precursor solution and stirring at 60° C. for 30 minutes, and drying the obtained suspension by rotary evaporation to obtain material 1;
[0091] Step 3, carbonizing material 1 in a tubular furnace under nitrogen protection at 500° C. (nitrogen flow rate is 100 mL / min) for 120 minutes to obtain material 2;
[0092] Step 4: disperse the material 2 in ethanol, wash it, filter it, and dry it to obtain a carbon material for adsorbing carbon monoxide.
[0093] Characterization of materials:
[0094] BET test shows that the carbon material has two mesopore distribution peaks at 2nm and 24.6nm. The mesopore volume of the carbon material is 0.31cm 3 / g, accounting for 45% of the total pore volume; the BET specific surface area is shown in Table 1.
[0095] XPS test shows that the carbon material clearly has an XPS peak of CuCl. Based on the total weight of the carbon material, the carbon content of the carbon material is 66.5% by weight, the CuCl content is 27.1% by weight, and the oxygen content is 6.4% by weight.
[0096] Example 4
[0097] Step 1, dissolving 3 g of copper bromide and 4.5 g of copper citrate (the molar ratio of copper bromide to copper citrate is 1.25:1) in deionized water, heating to 60° C. and stirring for 20 minutes to obtain a precursor solution;
[0098] Step 2, adding 10 g of lignin and 2 g of potassium chloride to the precursor solution and stirring at 60° C. for 30 minutes, and drying the obtained suspension by rotary evaporation to obtain material 1;
[0099] Step 3, carbonizing material 1 in a tubular furnace under nitrogen protection at 700° C. (nitrogen flow rate is 100 mL / min) for 120 minutes to obtain material 2;
[0100] Step 4: disperse material 2 in glycerol, wash it, filter it, and dry it to obtain a carbon material for adsorbing carbon monoxide.
[0101] Characterization of materials:
[0102] BET test shows that the carbon material has two mesopore distribution peaks at 2.1nm and 46.5nm. The mesopore volume of the carbon material is 0.25cm 3 / g, accounting for 57% of the total pore volume; the BET specific surface area is shown in Table 1.
[0103] XPS test shows that the carbon material clearly has an XPS peak of CuBr. Based on the total weight of the carbon material, the carbon content of the carbon material is 68.7% by weight, the CuBr content is 28.1% by weight, and the oxygen content is 3.2% by weight.
[0104] Comparative Example 1
[0105] Step 1, dissolving 3 g of copper chloride and 3.8 g of copper formate (the molar ratio of copper chloride to copper formate is 0.9:1) in deionized water, heating to 60° C. and stirring for 20 minutes to obtain a precursor solution;
[0106] Step 2: adding 10 g of lignin and 8 g of potassium chloride to the precursor solution and stirring at 60° C. for 30 minutes, and drying the obtained suspension by rotary evaporation to obtain material 1;
[0107] Step three, carbonizing material 1 in a tubular furnace under nitrogen protection at 800° C. (nitrogen flow rate is 100 mL / min) for 120 minutes to obtain a carbon material for adsorbing carbon monoxide.
[0108] Characterization of materials: The BET specific surface area of the carbon material is shown in Table 1. XPS test shows that the carbon material clearly has an XPS peak of CuCl. Based on the total weight of the carbon material, the carbon content in the carbon material is 40.6% by weight.
[0109] Comparative Example 2
[0110] Step 1, dissolving 3 g of copper chloride and 3.8 g of copper formate (the molar ratio of copper chloride to copper formate is 0.9:1) in deionized water, heating to 60° C. and stirring for 20 minutes to obtain a precursor solution;
[0111] Step 2, adding 10 g of lignin to the precursor solution and stirring at 60° C. for 30 minutes, and drying the obtained suspension by rotary evaporation to obtain material 1;
[0112] Step 3: Carbonize material 1 in a tubular furnace under nitrogen protection at 800° C. (nitrogen flow rate is 100 mL / min) for 120 minutes to obtain material 2.
[0113] Step 4: disperse material 2 in glycerol, wash it, filter it, and dry it to obtain a carbon material for adsorbing carbon monoxide.
[0114] Characterization of materials: The BET specific surface area of the carbon material is shown in Table 1. XPS test shows that the carbon material clearly has an XPS peak of CuCl. Based on the total weight of the carbon material, the carbon content in the carbon material is 52.1% by weight.
[0115] Test Case
[0116] (a) Adsorption of carbon monoxide: The carbon materials prepared in Examples 1-4 were respectively filled in the adsorption cylinder of the BSD-PH high-pressure gas analyzer (with an inner diameter of 10 mm, a height of 100 mm, and a filling length of 55 mm), and then 100% of carbon monoxide gas was supplied to the adsorption cylinder at 25°C and 100 kPa (1 Bar). The adsorption of gas by the adsorbent will cause a pressure drop. After reaching adsorption equilibrium, the equilibrium pressure of the gas is measured, and the adsorption capacity is calculated based on the pressure change of the system before and after adsorption to obtain the adsorption capacity of carbon monoxide gas per unit adsorbent (mL / g);
[0117] (b) Desorption of carbon monoxide: After reaching adsorption equilibrium in step (a), the adsorption cylinder is heated at 300° C. for 3 hours in a near vacuum to desorb carbon monoxide from the adsorbent.
[0118] The above carbon monoxide adsorption test and desorption test were repeated 5 times, and the average value was taken. The results are shown in Table 1.
[0119] Comparative test example
[0120] The carbon monoxide adsorption test and desorption test were carried out according to the method of the test example, except that the adsorbent was replaced by the carbon material prepared in Comparative Examples 1-2, respectively. The results are shown in Table 1.
[0121] Table 1
[0122]
[0123] The above results show that the carbon material prepared by the preparation method provided by the present invention has good CO adsorption performance. Its adsorption capacity for carbon monoxide at room temperature and pressure can reach more than 45 mL / g, and the highest can reach 67.8 mL / g; the BET specific surface area reaches 530 m 2 / g or above, and can adsorb carbon monoxide very well.
[0124] Comparative Example 1 is based on Example 1 minus the washing step, resulting in a significant decrease in the specific surface area of the carbon material and the lack of the ability to adsorb carbon monoxide.
[0125] Comparative Example 2 is based on Example 1 without adding alkali metal salt, so that the specific surface area of the carbon material is greatly reduced, and the carbon monoxide adsorption capacity is also affected.
[0126] It can be seen that in the preparation method provided by the present invention, the addition of alkali metal salt helps to activate the carbonization process of lignin, so that it forms a structured material with a high specific surface area, and also improves the dispersion of cuprous active components in the carbon material, thereby improving the adsorption effect of the carbon material on carbon monoxide.
[0127] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a carbon material for adsorbing carbon monoxide, the method comprising the following steps: (1) in the presence of a solvent, mixing a divalent copper salt, copper carboxylate, lignin and an alkali metal salt to obtain a suspension; the divalent copper salt is selected from copper chloride and / or copper bromide; (2) drying the suspension and then calcining it under an inert atmosphere; (3) washing the product obtained by calcining in step (2) and then drying; The washing comprises: dispersing the product obtained by calcining in step (2) in an organic solvent.
2. The preparation method according to claim 1, wherein In step (1), the mixing comprises: (1-1) first mixing a divalent copper salt, a copper carboxylate and a solvent to obtain a precursor solution; (1-2) The precursor solution is mixed with lignin and an alkali metal salt for a second time to obtain the suspension.
3. The preparation method according to claim 2, wherein In step (1-1), the first mixing includes stirring at elevated temperature.
4. The preparation method according to claim 3, wherein The conditions for heating and stirring include: temperature of 60-80° C. and time of 10-20 min.
5. The preparation method according to claim 2, wherein: In step (1-2), the second mixing conditions include: under stirring, at a temperature of 60-80° C., and for 30-60 min.
6. The preparation method according to claim 1 or 2, wherein: The molar ratio of the divalent copper salt to the copper carboxylate is 0.5-1.5:
1.
7. The preparation method according to claim 6, wherein: The molar ratio of the divalent copper salt to the copper carboxylate is 0.85-1.25:
1.
8. The preparation method according to claim 1 or 2, wherein: The copper carboxylate is selected from at least one of copper formate, copper acetate and copper citrate.
9. The preparation method according to claim 1 or 2, wherein: The mass ratio of the alkali metal salt to the lignin is 0.2-2:
1.
10. The preparation method according to claim 9, wherein: The mass ratio of the alkali metal salt to the lignin is 0.5-1:
1.
11. The preparation method according to claim 1 or 2, wherein: The alkali metal salt is a potassium salt and / or a sodium salt.
12. The preparation method according to claim 11, wherein The alkali metal salt is selected from at least one of potassium chloride, potassium nitrate, potassium sulfate, sodium chloride, sodium nitrate and sodium sulfate.
13. The preparation method according to claim 12, wherein: The alkali metal salt is potassium chloride.
14. The preparation method according to claim 1 or 2, wherein: The lignin is alkali-washed lignin.
15. The preparation method according to claim 1 or 2, wherein: The mass ratio of the divalent copper salt to the lignin is 0.2-1:
1.
16. The preparation method according to claim 15, wherein: The mass ratio of the divalent copper salt to lignin is 0.25-0.5:
1.
17. The preparation method according to claim 1 or 2, wherein: In step (2), the drying is performed by rotary evaporation.
18. The preparation method according to claim 1 or 2, wherein: The inert atmosphere is provided by an inert gas, and the inert gas is selected from at least one of nitrogen, helium, argon and neon.
19. The preparation method according to claim 1 or 2, wherein: The calcination conditions include: temperature of 200-950° C. and time of 2-6 hours.
20. The preparation method according to claim 1 or 2, wherein: The flow rate of the inert gas is 5-200 mL / min.
21. The preparation method according to claim 1 or 2, wherein: The organic solvent is selected from at least one of ethanol, methanol and glycerol.
22. A carbon material for adsorbing carbon monoxide obtained by the preparation method according to any one of claims 1 to 21.
23. The carbon material according to claim 22, wherein Based on the total weight of the carbon material, the carbon content of the carbon material is 40-80 weight %, the monovalent copper salt content is 20-50 weight % and the oxygen content is 1-10 weight %.
24. The carbon material according to claim 23, wherein Based on the total weight of the carbon material, the carbon content of the carbon material is 50-70 weight %, the monovalent copper salt content is 25-45 weight % and the oxygen content is 1-8 weight %.
25. The carbon material according to claim 23 or 24, wherein The monovalent copper salt is selected from CuCl and / or CuBr.
26. The carbon material according to claim 22, wherein In the pore size distribution curve of the carbon material, there are at least two mesopore distribution peaks.
27. The carbon material according to claim 26, wherein In the pore size distribution curve of the carbon material, there is a first mesopore distribution peak at 2-10 nm, and a second mesopore distribution peak at 20-50 nm.
28. The carbon material according to claim 22, wherein The mesopore volume of the carbon material is 0.2-0.7 cm 3 / g.
29. The carbon material according to claim 28, wherein The mesopore volume of the carbon material is 0.25-0.65 cm 3 / g.
30. The carbon material according to claim 22, wherein The proportion of the mesopore volume of the carbon material to the total pore volume is greater than 30%.
31. The carbon material according to claim 30, wherein The proportion of the mesopore volume of the carbon material to the total pore volume is greater than 40%.
32. The carbon material according to claim 22, wherein The BET specific surface area of the carbon material is 500-1000 m 2 / g.
33. The carbon material according to claim 32, wherein The BET specific surface area of the carbon material is 500-900 m 2 / g.
34. A method for adsorbing carbon monoxide, the method comprising: A gas containing carbon monoxide is brought into contact with a carbon material to adsorb the carbon monoxide contained in the gas onto the carbon material; wherein the carbon material is the carbon material according to any one of claims 22 to 33.
35. The adsorption method according to claim 34, wherein: The adsorption method further comprises, before the contacting, heating the carbon material in an inert gas environment or a reducing gas environment.