A solar-driven glass fiber-based composite MOF block moisture absorbent and its preparation method and application
By constructing a hydrophilic and photothermal conversion coating on a honeycomb glass fiber base and using in-situ synthesis technology to form a composite MOF, the problems of easy shedding of MOF hygroscopic agents and low heat and mass transfer efficiency are solved, achieving efficient water adsorption and Improved stability and performance driven by solar energy.
Patent Information
- Application Number
- CN202211596156.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-13
AI Technical Summary
Existing MOF hygroscopic agents are easy to fall off during use, have low heat and mass transfer efficiency, and have a low solar photothermal conversion rate, resulting in low water adsorption and storage efficiency.
A honeycomb glass fiber base is used as the carrier of MOF, and the hydrophilicity of the base material is improved through hydrophilic polymer material modification, and a polymer photothermal conversion coating is constructed on its surface, combined with in-situ synthesis technology, to form the same aluminum source, The composite MOF hybridized with two organic ligands achieves efficient self-assembly of MOF on the substrate and efficient capture and release of water vapor.
It achieves high load, low-temperature desorption, low energy consumption and high cycle stability of MOF, improves water adsorption capacity and solar-driven adsorption kinetics, avoids pore clogging problems caused by adhesives, and enhances the performance of hygroscopic agents. Water collection capacity.
Smart Images

Figure CN116020423B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solar-driven atmospheric water collection, and in particular relates to a solar-driven glass fiber-based composite MOF block moisture absorbent, and a preparation method and application thereof. Background Art
[0002] As the demand for freshwater resources increases, the sustainable and efficient use of atmospheric water has become a key issue. Atmospheric water is a green water source that can be developed and utilized. The fascinating water collection performance of cactus clusters and Namibian desert beetles proves the versatility and feasibility of atmospheric water collection technology. Therefore, the development of atmospheric water collection technology is conducive to the full utilization of freshwater resources, especially in arid areas, which can reduce the water burden.
[0003] Hygroscopic agents used in atmospheric water harvesting technology by adsorption include metal organic frameworks (MOFs), hydrogels, and traditional silica gel, zeolites, etc. Compared with other adsorbents, MOFs have attracted widespread attention due to their high water absorption capacity, steep water vapor adsorption and desorption curves, and low desorption temperatures. The water adsorption efficiency of MOFs is determined by three adsorption pathways: (i) capillary condensation; (ii) physical adsorption of polar and organic linkers; and (iii) chemical adsorption of inorganic metal units. In order to enable MOFs to capture as much atmospheric water as possible, the introduction of hygroscopic salts into the porous structure of MOFs has been reported as a successful strategy. However, salt-containing MOFs have problems such as salt leakage and corrosion. Considering these shortcomings, researchers have focused on improving the hydrophilicity of MOFs through structural modification methods, such as functional group modification and introduction of hybrid structures. By constructing a composite (hybrid) MOF using two MOFs with different working humidity ranges, its water adsorption isotherm has been cleverly adjusted. Interestingly, the surface area and pore structure parameters of the composite MOF also change because the two MOFs with the same metal source compete for nucleation. If a hybrid MOF with higher specific surface area and pore volume is formed, the competitive nucleation relationship between the two MOFs can be used to design a new generation of MOF adsorbents with higher water absorption activity. In addition, the recovery rate of powdered MOF desiccant in water environment is very low, which will lead to secondary pollution.
[0004] Adsorbent support is an effective way to effectively reduce pollution and increase the actual atmospheric water harvesting. Glass fiber paper (GF) has become an attractive and promising substrate due to its excellent ductility and durability. It is widely used in dehumidification systems, heat pumps, wind turbine blades and other fields. Passive adhesion of MOF powder to a substrate using a polymer adhesive is a common method for preparing MOF-based derivative products. For example, Tao et al. reported that adhesive sodium alginate and Al-fumarate were mixed and applied to a carbon scaffold to prepare an electrically heatable MOF product for atmospheric water harvesting (Tao, L., Wu, Q., Huang, C., Zhu, D., Li, H., 2022. Electrically heatable carbon scaffold accommodated monolithic metal–organic frameworks for energy-efficient atmospheric water harvesting. Chem. Eng. J. 451 (1), 138547. doi: 10.1016 / j.cej.2022.138547.). However, when these types of binders are added, the surface area and pore volume of MOF will be reduced due to pore clogging, which will reduce the water adsorption and storage energy absorption of MOF itself. Therefore, in order to combine GF and powdered MOF, it is necessary to use an in-situ synthesis method to grow MOF directly on the substrate, so as to solve the problem of powdered MOF shedding while effectively avoiding MOF pore clogging. However, the weak interfacial interaction between MOF and GF makes it difficult for MOF to grow on the surface of the substrate. For example, Tan et al. prepared an Al-fumarate monolithic adsorbent based on GF (Tan, B., Luo, Y., Liang, X., Wang, S., Gao, X., Zhang, Z., Fang, Y., 2019. In situ synthesis and performance of aluminum fumarate metal–organic framework monolithic adsorbent for water adsorption. Ind. Eng. Chem. Res. 58 (34), 15712-15720. doi: 10.1021 / acs.iecr.9b03172.), but due to the low loading of MOFs in the monolith (mass fraction less than 20%), the MOF-based product showed unsatisfactory water absorption performance. Therefore, the synthesis of reliable and fine functionalized MOF monolithic adsorbents requires more sophisticated design.
[0005] In addition, after the desiccant is saturated with adsorption, it needs to use external energy such as heat to desorb it in order to achieve the next adsorption-desorption cycle. Solar energy is a green energy, but whether it is MOF desiccant or GF substrate, they have low solar thermal conversion rate. Some polymers such as polydopamine, polypyrrole, polyaniline, etc. have strong photothermal conversion ability. Therefore, adding a polymer photothermal conversion coating on the basis of GF-based composite MOF block desiccant is a feasible technical solution. Summary of the invention
[0006] In order to realize the carrierization of MOF to solve the disadvantages of MOF powder being easy to fall off and agglomerate during use, and at the same time solve the problems of low photothermal conversion efficiency and poor heat and mass transfer efficiency of MOF powder, the purpose of the present invention is to provide a solar-driven glass fiber-based composite MOF block desiccant and its preparation method and application.
[0007] The present invention proposes a design technical solution for a solar-driven glass fiber-based composite MOF integral adsorbent (i.e., a solar-driven glass fiber-based composite MOF block hygroscopic agent according to the present invention). First, a honeycomb glass fiber-based embryo is selected as a carrier of MOF. Its uniform honeycomb structure and multi-void skeleton can provide a large attachment area for MOF powder and reduce the heat and mass transfer resistance of the adsorption and desorption process of the adsorbent as much as possible. In order to solve the problem of low interface between the substrate and MOF, a hydrophilic polymer material (hydrophilic coating) is used to modify the surface of the substrate to improve its hydrophilicity, thereby providing growth conditions for the in-situ self-assembly of MOF on its surface. At the same time, a polymer photothermal conversion coating is added to achieve high absorption of sunlight, providing heat for the subsequent adsorbed water to separate from MOF. The composite MOF is a water-absorbing composite MOF hybridized with the same aluminum source and two organic ligands, and a composite MOF with different MOF ratios is obtained by adjusting the ratio of the two organic ligands. Through reasonable design, the composite MOF can have a high specific surface area and pore volume, and has a higher water adsorption capacity than a single MOF monomer. In addition, by using the in-situ synthesis process, the composite MOF is self-assembled on the hydrophilic modified fiber substrate, which can avoid the use of adhesives to cause MOF pore blockage. The composite MOF block desiccant obtained based on the above design concept has the advantages of low energy consumption, high water adsorption, low temperature desorption, and high cycle stability.
[0008] The present invention designs a solar-driven, efficient, and stable integral water adsorbent by loading composite MOFs with functionalized glass fibers. First, a hydrophilic and photothermal conversion polymer coating is constructed on a honeycomb glass fiber substrate to increase the loading capacity of MOFs through electrostatic and hydrophilic effects. Subsequently, a composite MOF composed of the same aluminum source and two MOFs is customized on the surface of the substrate through in-situ synthesis self-assembly technology. Due to the presence of more active adsorption sites, the resulting composite MOF exhibits better water collection capacity and faster adsorption kinetics at low humidity as a whole.
[0009] The technical solution adopted by the present invention is as follows:
[0010] The present invention provides a method for preparing a solar-driven glass fiber-based composite MOF block moisture absorbent, comprising the following steps:
[0011] (1) Preparation of honeycomb glass fiber-based functional embryo body: Under stirring, the honeycomb glass fiber-based embryo body is immersed in a mixed solution containing a photothermal conversion coating and a hydrophilic coating. After stirring, the functional coating embryo body (honeycomb glass fiber-based functional embryo body) containing a hydrophilic coating and a photothermal conversion coating is taken out and dried.
[0012] (2) Preparation of composite MOF reaction solution: according to the metered ratio, two organic dicarboxylic acid ligands and aluminum salt are dissolved in deionized water, heated at a constant temperature, and then NaOH solution is added. A clear and transparent composite MOF reaction solution is obtained by magnetic stirring, and the solution is transferred into a reaction tank;
[0013] (3) Preparation of a solar-driven glass fiber-based composite MOF bulk desiccant: The functionalized coating embryo obtained in step (1) is immersed in a sealed tank containing a mixed MOF reaction solution, and a hydrothermal reaction is performed to obtain a crude product. The crude product is then immersed in water to obtain a solar-driven glass fiber-based composite MOF bulk desiccant.
[0014] Preferably, in step (1), the hydrophilic coating is selected from one of chitosan, carboxymethyl chitosan, cyclodextrin, etc., and the photothermal conversion coating includes one of polydopamine, polyaniline, and polypyrrole, wherein the photothermal conversion coating polymer monomers dopamine, aniline, and pyrrole are polymerized to obtain photothermal conversion coating polydopamine, polyaniline, and polypyrrole, respectively, and the hydrophilic coating coating photothermal conversion coating can be formed by the reaction polymerization of the mixed solution of dopamine, aniline, and pyrrole monomers and the hydrophilic coating. The physical entanglement and hydrogen bonding of the two polymer coatings are used to achieve the coating of the photothermal conversion coating by the hydrophilic coating.
[0015] Further preferably, taking into account factors such as compatibility (dispersibility) between polymer resins, adhesion performance between the coating and the substrate, and price, chitosan is used as the hydrophilic coating, and polydopamine is used as the photothermal conversion coating (that is, dopamine is used as the polymer monomer of the photothermal conversion coating).
[0016] Preferably, in step (1), the method for preparing the mixed solution containing the photothermal conversion coating and the hydrophilic coating is to mix a photothermal conversion coating solution with a concentration of 5-15 mg / mL with a hydrophilic coating solution with a concentration of 5-20 mg / mL.
[0017] Preferably, in step (2), the aluminum salt is one of water-soluble aluminum chloride, aluminum sulfate, aluminum nitrate, aluminum acetate, etc., and the organic dicarboxylic acid ligand includes any two of 2,5-furandicarboxylic acid, fumaric acid, 3,5-pyrazoledicarboxylic acid and isophthalic acid.
[0018] Further preferably, the aluminum salt is aluminum nitrate; it has good solubility and strong coordination with the sodium salt of organic dicarboxylic acid.
[0019] Preferably, in step (2), the organic dicarboxylic acid ligand and NaOH react to obtain an organic dicarboxylic acid sodium salt, wherein the organic dicarboxylic acid sodium salt includes any two of sodium fumarate, sodium 2,5-furandicarboxylate, sodium 3,5-pyrazoledicarboxylate, sodium isophthalate, etc., and the composite MOF is any two of MIL-160 (Al), MOF-303, Al-fumarate, CAU-10-H, etc. synthesized in situ on a glass fiber substrate by an aluminum salt and a corresponding organic dicarboxylic acid sodium salt.
[0020] Further preferably, the organic dicarboxylic acid sodium salt is a combination of sodium 2,5-furandicarboxylate and sodium 3,5-pyrazoledicarboxylate; they can be obtained by reacting sodium hydroxide with an organic dicarboxylic acid (2,5-furandicarboxylic acid, 3,5-pyrazoledicarboxylic acid); the composite MOF desiccant is a combination of MIL-160 (Al) and MOF-303, and MIL-160 (Al) and MOF-303 have similar topological structures, crystallization rates and reaction conditions.
[0021] Preferably, in step (2), the molar ratio of the sodium hydroxide to the organic dicarboxylic acid ligand is (0.8-2.4):1, the molar ratio of the aluminum salt to the organic dicarboxylic acid ligand is (0.8-1.2):1; the molar ratio of the two MOFs in the composite MOF is (0.2-5):1
[0022] Further preferably, the molar ratio of the two MOFs in the composite MOF is (0.43-2.33):1.
[0023] Further preferably, the molar ratio of the sodium hydroxide to the organic dicarboxylic acid ligand is (1.0-2.0):1; the amount of sodium hydroxide is small, the degree of protonation of the organic dicarboxylic acid is low, and the reaction rate of the system is slow; the amount of sodium hydroxide is large, the reaction rate of the system is fast, and the formed composite MOF is easy to fall off and powder. The molar ratio of the aluminum salt to the organic dicarboxylic acid ligand is (0.9-1.1):1. The amount of aluminum salt is small, the pH of the system is high; the reaction rate is slow; the amount of aluminum salt is large, the pH of the system is low, the reaction rate is fast, the synthesized composite MOF is unevenly dispersed, and it is easy to fall off. In the composite MOF, the molar ratio of MIL-160 (Al) to MOF-303 is 1: (0.3-4). When MIL-160 (Al) is high, the adsorption curve of the composite MOF shifts to the left, which is conducive to adsorption at low humidity (RH = 0-30%), and when MOF-303 is high, the adsorption curve shifts to the right, which is conducive to adsorption in a higher humidity (RH = 60%-100%) environment, and the adsorption amount is large.
[0024] Preferably, in step (2), the temperature of the hydrothermal reaction is 90-120° C., and the time of the hydrothermal reaction is 8-24 h.
[0025] Further preferably, in step (2), the temperature of the hydrothermal reaction is 100° C., and the time of the hydrothermal reaction is 12 h.
[0026] The invention provides a solar-driven glass fiber-based composite MOF block moisture absorbent prepared by the preparation method.
[0027] Preferably, the solar-driven glass fiber-based composite MOF block desiccant is composed of 37% to 45% honeycomb glass fiber-based carrier, 2% to 8% hydrophilic coating, 5% to 10% photothermal conversion coating and 37% to 56% composite MOF, calculated by mass fraction.
[0028] Further preferably, the solar-driven glass fiber-based composite MOF block hygroscopic agent is composed of 38% to 43% honeycomb glass fiber-based carrier, 3% to 7% hydrophilic coating, 6% to 12% photothermal conversion coating and 38% to 53% composite MOF by mass fraction. The substrate ratio is small, the MOF adsorbent loading is small, and the atmospheric water collection is small; the substrate ratio is large, the MOF hygroscopic agent loading is large, and the atmospheric water collection is large; the hydrophilic coating is small, the photothermal conversion coating coating is low, the bonding force with the substrate surface is weak, and the composite MOF is easy to fall off; the hydrophilic coating is large, the photothermal conversion coating coating is high, and the composite MOF has high adhesion to the substrate; the photothermal conversion coating is small, and the solar thermal conversion efficiency is low; the photothermal conversion coating is large, and the solar thermal conversion efficiency is high; the composite MOF ratio is high, and its atmospheric water collection is large, and the composite MOF ratio is low, and its atmospheric water collection is small.
[0029] Preferably, a photothermal conversion polymer coating is coated with a hydrophilic polymer (hydrophilic coating), involving a solar-driven glass fiber-based composite MOF block desiccant formed by layer-by-layer self-assembly of the same aluminum source and two organic dicarboxylic acid sodium salts on a honeycomb glass fiber.
[0030] Preferably, the solar-driven glass fiber-based composite MOF moisture absorber is synthesized in situ by a one-pot hydrothermal method on a honeycomb glass fiber substrate from the same aluminum salt (aluminum ion) and two organic dicarboxylic acid sodium salts.
[0031] The present invention also provides the use of the solar-driven glass fiber-based composite MOF block moisture absorbent in atmospheric water collection.
[0032] The preparation method of the present invention is based on the following working principle:
[0033] First, hydrophilic modification of glass fiber. Hydrophilic polymer materials (hydrophilic coatings) such as chitosan contain a large number of polar groups such as -OH and -NH2. When they are evenly dispersed on the glass fiber substrate, they can improve the hydrophilicity of the substrate and facilitate the attachment of organic carboxylic acid ligands to the substrate and the in-situ synthesis of composite MOF.
[0034] Second, the photothermal conversion of solar energy. By utilizing the π-π* transition of high molecular photothermal conversion coating polymers such as polydopamine, the ultraviolet and visible regions of solar energy can be highly absorbed, that is, the photothermal conversion efficiency is improved, and the water adsorbed by the composite MOF is released efficiently. The hydrophilic coating effectively covers the photothermal conversion coating, which can reduce the loss of the photothermal conversion coating in the reaction system and keep it on the substrate surface to the maximum extent.
[0035] Third, the construction of composite MOF. Two MOFs can be obtained from the same aluminum source and two dicarboxylic acid sodium salts. By adjusting their ratio in the synthesis reaction, composite MOFs with different MOF compositions can be obtained. Different MOFs are designed in the same reaction system (one-pot method), and they will compete with each other for nucleation, thereby affecting their respective crystal morphology and pore structure parameters. By adjusting the ratio of organic ligands in the reaction system, a composite MOF with high specific surface area and pore volume can be obtained, thereby obtaining a higher water adsorption capacity than the original MOF.
[0036] Fourth, in-situ synthesis technology. Traditional MOF is loaded with a binder on the substrate. Not only does the binder itself have no adsorption properties, but it may also block the MOF pores, thereby affecting its adsorption capacity. In-situ synthesis technology utilizes self-assembly on the MOF substrate. This process does not involve the addition of any binder, so it can effectively prevent the occurrence of pore blocking and increase the content of MOF desiccant in the substrate.
[0037] Fifth, the principle of atmospheric water collection. The solar-driven glass fiber-based composite MOF block desiccant uses the porous adsorption characteristics of MOF to automatically capture water and store it in its own MOF pores at night when the relative humidity is high. Then, by utilizing the high solar light absorption characteristics of the photothermal conversion coating, the surface temperature of the entire desiccant is rapidly increased during the day, providing escape heat for the adsorbed water stored in the MOF pores, thereby actively releasing the captured water.
[0038] Compared with the prior art, the technology of the present invention has the following advantages:
[0039] (1) The MOF desiccant was used as a carrier to solve the shortcomings of MOF powder such as easy agglomeration and poor heat and mass transfer.
[0040] (2) Use in-situ synthesis technology to avoid MOF powder pore clogging caused by adding adhesives.
[0041] (3) Add a hydrophilic coating to the substrate to achieve high MOF loading on the substrate and reduce MOF powder loss.
[0042] (4) Adding a photothermal conversion coating to the substrate enhances the capture and conversion of solar energy, creating conditions for achieving low-energy water production in the device.
[0043] (5) A higher water capture capacity was achieved by constructing a solar-driven glass fiber-based composite MOF bulk hygroscopic agent.
[0044] (6) The solar-driven glass fiber-based composite MOF block desiccant prepared by the present invention has a simple preparation process and is green and environmentally friendly. It has the characteristics of large moisture absorption capacity, low-temperature desorption by solar energy and stable performance. It can realize the production of drinking water from air in all weather conditions, especially in low humidity (dry environment). BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 Scanning electron microscope (SEM) images of the honeycomb glass fiber-based embryo body, the honeycomb glass fiber-based functional embryo body and the bulk hygroscopic agent of the solar-driven honeycomb glass fiber-based composite MOF prepared in Example 1.
[0046] Figure 2 This is a comparison chart of X-ray powder diffraction (XRD) of the bulk hygroscopic agents prepared in Comparative Example 1, Comparative Example 2 and Example 1.
[0047] Figure 3 The photothermal curves of the block desiccant prepared in Example 1 and Comparative Example 3 under the irradiation of sunlight.
[0048] Figure 4 It is a water vapor isothermal adsorption curve diagram of the block desiccant prepared in Example 1, Comparative Example 1 and Comparative Example 2 at 25°C.
[0049] Figure 5 This is a cyclic stability curve diagram of the bulk moisture absorbent of the solar-driven honeycomb glass fiber-based composite MOF prepared in Example 1. DETAILED DESCRIPTION
[0050] The following examples are further examples of specific implementations of the present invention, but the embodiments and protection scope of the present invention are not limited thereto.
[0051] Material preparation:
[0052] a: Preparation of 10 mg / mL dopamine hydrochloride solution: Accurately weigh 15.0 g dopamine hydrochloride (purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) and dissolve it in 1500 mL hydrochloric acid buffer solution (1.5 M, pH = 8.8, purchased from Solebow Biotechnology Co., Ltd.) for later use.
[0053] b: Preparation of 15 mg / mL chitosan solution: Accurately weigh 1.50 g chitosan hydrochloride (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) and add it to 1000 mL deionized water. After continuous stirring at 70°C for 20 min, cool it for later use.
[0054] c: Preparation of the honeycomb glass fiber-based embryo body used in Comparative Example 3: The honeycomb glass fiber-based block (also known as corrugated paper, purchased from KeRun (Hangzhou) Environmental Protection Technology Co., Ltd., 2cm×4cm×2cm) was sintered in a 550℃ muffle furnace for 12h to remove organic residues to obtain a honeycomb glass fiber-based embryo body weighing 2.428g.
[0055] d: Preparation of the honeycomb glass fiber-based functional embryo used in the following Examples 1-3, Examples 6-11 and Comparative Examples 1-2: At room temperature and magnetic stirring, take 80 mL of a 10 mg / mL dopamine hydrochloride solution and add it to a 200 mL beaker. Continue stirring for 3 hours, then add 20 mL of a 15 mg / mL chitosan solution (the solvent is water) to the reaction solution to obtain a mixed solution, adjust the pH of the reaction solution to 8.8, and then immerse 2.428 g of the honeycomb glass fiber-based embryo in the mixed solution, continue magnetic stirring for 24 hours, take out and dry in a hot air furnace at 60°C for 12 hours to obtain a honeycomb glass fiber-based functional embryo, weighing 3.085 g.
[0056] Comparative Example 1
[0057] (1) Under magnetic stirring, 3.12 g of 2,5-furandicarboxylic acid (H2FDC, 20 mmol, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) and 7.5 g of aluminum nitrate nonahydrate (Al(NO3)3·9H2O, 20 mmol, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) were accurately weighed and added into a 300 mL beaker, 100 mL of deionized water was added to dissolve, the mixture was heated to 80°C, and 50 mL of 0.6 mmol / mL sodium hydroxide (NaOH, 30 mmol, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) aqueous solution was added dropwise to obtain a transparent composite MOF reaction solution.
[0058] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.082 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. Subsequently, the reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 hours, and the solar-driven honeycomb glass fiber-based MIL-160 (Al) block desiccant was obtained, which was recorded as MIL-160 (Al) functional block desiccant, weighing 5.984 g. By mass fraction, the MIL-160 (Al) loading rate was 48.45%, the honeycomb glass fiber substrate accounted for 40.56%, the functional coating accounted for 10.99%, the hydrophilic coating accounted for 4.12% of the functional coating, and the photothermal conversion coating accounted for 6.87% of the functional coating.
[0059] Comparative Example 2
[0060] (1) Under magnetic stirring, accurately weigh 3.08 g of 3,5-pyrazoledicarboxylic acid (H3PDC, 20 mmol, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) and 7.5 g of aluminum nitrate nonahydrate (Al(NO3)3·9H2O, 20 mmol) into a 300 mL beaker, add 100 mL of deionized water to dissolve, heat to 80 °C, and dropwise add 50 mL of 0.6 mmol / mL sodium hydroxide (NaOH, 30 mmol) aqueous solution to obtain a transparent composite MOF reaction solution.
[0061] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.088 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. Subsequently, the reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 h. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for 12 h to obtain a solar-driven honeycomb glass fiber-based MOF-303 block hygroscopic agent, recorded as MOF-303 functional block hygroscopic agent, weighing 6.023 g. By mass fraction, the MOF-303 loading rate was 48.72%, the honeycomb glass fiber substrate accounted for 40.37%, the functional coating accounted for 10.91%, the hydrophilic coating accounted for 4.09% of the functional coating, and the photothermal conversion coating accounted for 6.82% of the functional coating.
[0062] Comparative Example 3
[0063] (1) Under magnetic stirring, 1.56 g H2FDC (10 mmol), 10.54 g 3,5-pyrazoledicarboxylic acid (H3PDC, 10 mmol) and 7.5 g Al(NO3)3·9H2O (20 mmol) were accurately weighed and added into a 300 mL beaker, 100 mL deionized water was added to dissolve, the mixture was heated to 80 °C, and 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution was added dropwise to obtain a transparent composite MOF reaction solution.
[0064] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 2.425 g of unmodified honeycomb glass fiber-based embryo was immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. Subsequently, the reaction tank was sealed and placed in a muffle furnace at 100°C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100°C oven for drying for 12 hours to obtain a honeycomb glass fiber-based composite MOF block hygroscopic agent, recorded as a composite MOF (5) block hygroscopic agent, weighing 3.053 g. By mass fraction, the composite MOF (5) loading rate was 20.57%, and the honeycomb glass fiber substrate was 79.43%.
[0065] Example 1
[0066] (1) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 10.54 g 3,5-pyrazoledicarboxylic acid (H3PDC, 10 mmol) and 7.5 g Al(NO3)3·9H2O (20 mmol) and add them into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and dropwise add 50 mL of 0.6 mmol / mL NaOH (30 mmol) aqueous solution to obtain a transparent composite MOF reaction solution;
[0067] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.085 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. Subsequently, the reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 hours to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, recorded as a composite MOF (5) functional block hygroscopic agent, weighing 6.123 g. By mass fraction, the composite MOF (5) loading rate was 49.62%, the honeycomb glass fiber substrate accounted for 39.65%, the functional coating accounted for 10.73%, the hydrophilic coating accounted for 4.02% of the functional coating, and the photothermal conversion coating accounted for 6.71% of the functional coating.
[0068] Example 2
[0069] (1) Under magnetic stirring, accurately weigh 0.936 g H2FDC (6 mmol), 2.16 g H3PDC (14 mmol), and 7.5 g Al(NO3)3·9H2O (20 mmol) into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and dropwise add 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution to obtain a transparent composite MOF reaction solution;
[0070] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.080 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 hours to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, that is, a solar-driven honeycomb glass fiber-based composite MOF block adsorbent was obtained, which was recorded as a composite MOF (3) functional block hygroscopic agent, weighing 6.144 g. By mass fraction, the composite MOF (3) loading rate was 49.87%, the honeycomb glass fiber substrate accounted for 39.44%, the functional coating accounted for 10.69%, the hydrophilic coating accounted for 4.01% of the functional coating, and the photothermal conversion coating accounted for 6.68% of the functional coating.
[0071] Example 3
[0072] (1) Under magnetic stirring, accurately weigh 2.18 g H2FDC (14 mmol), 0.924 g H3PDC (6 mmol), and 7.5 g Al(NO3)3·9H2O (20 mmol) into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and dropwise add 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution to obtain a transparent composite MOF reaction solution;
[0073] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.078 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 h. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 h, and a solar-driven honeycomb glass fiber-based composite MOF block adsorbent was obtained, which was recorded as a composite MOF (7) functional block desiccant, weighing 6.098 g. By mass fraction, the composite MOF (7) loading rate was 49.52%, the honeycomb glass fiber substrate accounted for 39.71%, the functional coating accounted for 10.77%, the hydrophilic coating accounted for 4.04% of the functional coating, and the photothermal conversion coating accounted for 6.73% of the functional coating.
[0074] Example 4
[0075] Preparation of honeycomb glass fiber-based functional embryos: except that the amount of chitosan solution added was changed to 20 mL of 5 mg / mL chitosan solution, the remaining steps were the same as step d in the above material preparatory process, weighing 2.912 g.
[0076] (1) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 10.54 g H3PDC (10 mmol), and 7.5 g Al(NO3)3·9H2O (20 mmol) into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and dropwise add 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution to obtain a transparent composite MOF reaction solution;
[0077] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 2.912 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 h. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 h to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 5.903 g. By mass fraction, the composite MOF (5) loading rate was 48.98%, the honeycomb glass fiber substrate accounted for 41.13%, the functional coating accounted for 11.47%, the hydrophilic coating in the functional coating accounted for 3.28%, and the photothermal conversion coating in the functional coating accounted for 8.19%.
[0078] Example 5
[0079] Preparation of honeycomb glass fiber-based functional embryos: except that the amount of chitosan solution added was changed to 20 mL of 20 mg / mL chitosan solution, the remaining steps were the same as step d in the above material pre-preparation, weighing 3.152 g.
[0080] (1) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 10.54 g H3PDC (10 mmol), and 7.5 g Al(NO3)3·9H2O (20 mmol) into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and add 50 mL 0.6 mmol / L NaOH (30 mmol) aqueous solution dropwise to obtain a transparent composite MOF reaction solution;
[0081] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.152 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 h. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 h to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 6.303 g. By mass fraction, the composite MOF (5) loading rate was 49.99%, the honeycomb glass fiber substrate accounted for 38.52%, the functional coating accounted for 11.49%, the hydrophilic coating accounted for 4.81% of the functional coating, and the photothermal conversion coating accounted for 6.68% of the functional coating.
[0082] Example 6
[0083] (1) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 1.54 g H3PDC (10 mmol), and 7.5 g Al(NO3)3·9H2O (20 mmol) into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and add 40 mL 0.6 mmol / mL NaOH (24 mmol) aqueous solution dropwise to obtain a transparent composite MOF reaction solution;
[0084] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.085 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 hours to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 5.821 g. By mass fraction, the composite MOF (5) loading rate was 47.0%, the honeycomb glass fiber substrate accounted for 41.71%, the functional coating accounted for 11.29%, the hydrophilic coating in the functional coating accounted for 4.23%, and the photothermal conversion coating in the functional coating accounted for 7.06%.
[0085] Example 7
[0086] (1) Under magnetic stirring, 1.56 g H2FDC (10 mmol), 1.54 g H3PDC (10 mmol), and 7.5 g Al(NO3)3·9H2O (20 mmol) were accurately weighed and added into a 300 mL beaker, 100 mL deionized water was added to dissolve, the mixture was heated to 80 °C, and 60 mL 0.6 mmol / mL NaOH (36 mmol) aqueous solution was added dropwise to obtain a transparent composite MOF reaction solution;
[0087] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.085 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 hours to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 5.777 g. By mass fraction, the composite MOF (5) loading rate was 46.60%, the honeycomb glass fiber substrate was 42.0%, the functional coating accounted for 11.37%, the hydrophilic coating accounted for 4.26% of the functional coating, and the photothermal conversion coating accounted for 7.11% of the functional coating.
[0088] Example 8
[0089] (1) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 1.54 g H3PDC (10 mmol), and 6.75 g Al(NO3)3·9H2O (18 mmol) into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and dropwise add 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution to obtain a transparent composite MOF reaction solution;
[0090] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.085 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 hours to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 5.855 g. By mass fraction, the composite MOF (5) loading rate was 47.31%, the honeycomb glass fiber substrate accounted for 41.47%, the functional coating accounted for 11.22%, the hydrophilic coating in the functional coating accounted for 4.21%, and the photothermal conversion coating in the functional coating accounted for 7.01%.
[0091] Example 9
[0092] (1) Under magnetic stirring, 1.56 g H2FDC (10 mmol), 1.54 g H3PDC (10 mmol) and 9.0 g Al(NO3)3·9H2O (24 mmol) were accurately weighed and added into a 300 mL beaker, 100 mL deionized water was added to dissolve, the mixture was heated to 80 °C, and 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution was added dropwise to obtain a transparent composite MOF reaction solution;
[0093] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.085 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 hours to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 6.107 g. By mass fraction, the composite MOF (5) loading rate was 49.48%, the honeycomb glass fiber substrate accounted for 39.76%, the functional coating accounted for 10.76%, the hydrophilic coating accounted for 4.03% of the functional coating, and the photothermal conversion coating accounted for 6.73% of the functional coating.
[0094] Example 10
[0095] (1) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 1.54 g H3PDC (10 mmol), and 7.5 g Al(NO3)3·9H2O (20 mmol) into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and add 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution dropwise to obtain a transparent composite MOF reaction solution;
[0096] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.085 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 90°C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100°C oven for drying for 12 hours to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 5.651 g. By mass fraction, the composite MOF (5) loading rate was 45.40%, the honeycomb glass fiber substrate accounted for 42.97%, the functional coating accounted for 11.63%, the hydrophilic coating accounted for 4.51% of the functional coating, and the photothermal conversion coating accounted for 7.12% of the functional coating.
[0097] Embodiment 11
[0098] (1) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 1.54 g 3,5-pyrazoledicarboxylic acid (H3PDC, 10 mmol) and 7.5 g Al(NO3)3·9H2O (20 mmol) and add them into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and add 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution dropwise to obtain a transparent composite MOF reaction solution;
[0099] (2) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.085 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 120°C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100°C oven for drying for 12 hours to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 5.702 g. By mass fraction, the composite MOF (5) loading rate was 45.90%, the honeycomb glass fiber substrate accounted for 42.58%, the functional coating accounted for 11.52%, the hydrophilic coating in the functional coating accounted for 4.32%, and the photothermal conversion coating in the functional coating accounted for 7.2%.
[0100] Example 12
[0101] (1) Preparation of honeycomb glass fiber-based functional embryos: except that the chitosan solution was changed to carboxymethyl chitosan solution (the solvent was water, and carboxymethyl chitosan was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), the remaining steps were the same as step d in the above material preparatory process. Weigh 2.912 g.
[0102] (2) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 1.54 g H3PDC (10 mmol) and 7.5 g Al(NO3)3·9H2O (20 mmol) and add them into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and add 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution dropwise to obtain a transparent composite MOF reaction solution;
[0103] (3) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 2.912 g of honeycomb glass fiber-based functional embryo was immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 hours to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 4.787 g. By mass fraction, the composite MOF (5) loading rate was 39.17%, the honeycomb glass fiber substrate accounted for 42.88%, the functional coating accounted for 17.95%, the hydrophilic coating accounted for 6.89% of the functional coating, and the photothermal conversion coating accounted for 11.06% of the functional coating.
[0104] Embodiment 13
[0105] (1) Preparation of honeycomb glass fiber-based functional embryos: except that the chitosan solution was replaced with a cyclodextrin solution (the solvent was water, and cyclodextrin was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), the remaining steps were the same as step d in the above material preparatory process. The weight was 3.192 g.
[0106] (2) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 1.54 g H3PDC (10 mmol) and 7.5 g Al(NO3)3·9H2O (20 mmol) and add them into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and add 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution dropwise to obtain a transparent composite MOF reaction solution;
[0107] (3) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.192 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 h. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 h to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 5.431 g. By mass fraction, the composite MOF (5) loading rate was 41.23%, the honeycomb glass fiber substrate accounted for 41.36%, the functional coating accounted for 17.41%, the hydrophilic coating in the functional coating accounted for 6.94%, and the photothermal conversion coating in the functional coating accounted for 10.47%.
[0108] Embodiment 14
[0109] (1) At room temperature and magnetic stirring, 0.8 g of polyaniline powder (purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) was accurately weighed and ultrasonically separated into 80 mL of hydrochloric acid buffer solution (1.5 M, pH = 8.8), and stirred for 3 h. Then, 20 mL of 15 mg / mL chitosan solution (solvent is water) was added to the reaction solution to obtain a mixed solution. The pH of the reaction solution was adjusted to 8.8, and the honeycomb glass fiber-based embryo (pre-treated according to step c in the above material pre-preparation) was immersed in the mixed solution. The magnetic stirring was continued for 24 h, and the honeycomb glass fiber-based functional embryo was taken out and dried in a hot air furnace at 60°C for 12 h to obtain a honeycomb glass fiber-based functional embryo weighing 3.234 g.
[0110] (2) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 1.54 g H3PDC (10 mmol) and 7.5 g Al(NO3)3·9H2O (20 mmol) and add them into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and add 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution dropwise to obtain a transparent composite MOF reaction solution;
[0111] (3) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.234 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 hours to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 5.627 g. By mass fraction, the composite MOF (5) loading rate was 42.53%, the honeycomb glass fiber substrate accounted for 41.57%, the functional coating accounted for 15.90%, the hydrophilic coating accounted for 6.98% of the functional coating, and the photothermal conversion coating accounted for 8.92% of the functional coating.
[0112] Embodiment 15
[0113] (1) At room temperature and magnetic stirring, accurately weigh 0.8 g of polypyrazole powder (purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) and ultrasonically separate it into 80 mL of hydrochloric acid buffer solution (1.5 M, pH = 8.8), and continue stirring for 3 h. Then, add 20 mL of 15 mg / mL chitosan solution (solvent is water) to the reaction solution to obtain a mixed solution, adjust the pH of the reaction solution to 8.8, and then immerse the honeycomb glass fiber-based embryo (pre-treated according to step c in the above material pre-preparation) in the mixed solution, continue magnetic stirring for 24 h, take out and dry in a hot air furnace at 60°C for 12 h to obtain a honeycomb glass fiber-based functional embryo, weighing 3.104 g.
[0114] (2) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 1.54 g H3PDC (10 mmol) and 7.5 g Al(NO3)3·9H2O (20 mmol) and add them into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and add 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution dropwise to obtain a transparent composite MOF reaction solution;
[0115] (3) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.104 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 hours to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 5.418 g. By mass fraction, the composite MOF (5) loading rate was 42.71%, the honeycomb glass fiber substrate accounted for 42.98%, the functional coating accounted for 14.31%, the hydrophilic coating accounted for 6.89% of the functional coating, and the photothermal conversion coating accounted for 7.42% of the functional coating.
[0116] Example 16
[0117] (1) Preparation of honeycomb glass fiber-based functional embryos: The remaining steps are the same as step d in the above material preparatory process, except that the amount of dopamine hydrochloride solution added is changed to 80 mL of 5 mg / mL dopamine hydrochloride solution. The weight is 2.612 g.
[0118] (2) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 1.54 g H3PDC (10 mmol) and 7.5 g Al(NO3)3·9H2O (20 mmol) and add them into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and add 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution dropwise to obtain a transparent composite MOF reaction solution;
[0119] (3) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 2.612 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 h. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 h to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 4.342 g. By mass fraction, the composite MOF (5) loading rate was 39.84%, the honeycomb glass fiber substrate accounted for 42.04%, the functional coating accounted for 18.12%, the hydrophilic coating in the functional coating accounted for 6.95%, and the photothermal conversion coating in the functional coating accounted for 11.17%.
[0120] Embodiment 17
[0121] (1) Preparation of honeycomb glass fiber-based functional embryos: The remaining steps are the same as step d in the above material preparatory process, except that the amount of dopamine hydrochloride solution added is changed to 80 mL of 15 mg / mL dopamine hydrochloride solution. The weight is 3.269 g.
[0122] (2) Under magnetic stirring, accurately weigh 1.56 g H2FDC (10 mmol), 1.54 g H3PDC (10 mmol) and 7.5 g Al(NO3)3·9H2O (20 mmol) and add them into a 300 mL beaker, add 100 mL deionized water to dissolve, heat to 80 °C, and add 50 mL 0.6 mmol / mL NaOH (30 mmol) aqueous solution dropwise to obtain a transparent composite MOF reaction solution;
[0123] (3) The composite MOF reaction solution was transferred to a 250 mL reaction tank lined with polytetrafluoroethylene, and 3.269 g of honeycomb glass fiber-based functional embryos were immersed in the reaction tank containing the MOF reaction solution and cooled naturally to room temperature. The reaction tank was sealed and placed in a muffle furnace at 100 ° C for hydrothermal reaction for 12 hours. After cooling to room temperature, the block sample was taken out and washed with deionized water three times, and then placed in a 100 ° C oven for drying for 12 hours to obtain a solar-driven honeycomb glass fiber-based composite MOF block hygroscopic agent, weighing 6.362 g. By mass fraction, the composite MOF (5) loading rate was 48.62%, the honeycomb glass fiber substrate accounted for 40.06%, the functional coating accounted for 11.32%, the hydrophilic coating in the functional coating accounted for 3.12%, and the photothermal conversion coating in the functional coating accounted for 8.20%.
[0124] Test conditions and methods
[0125] The morphology of the samples was investigated using a field emission scanning electron microscope (FESEM, Meilin, Zeiss, Germany). X-ray diffraction (XRD) patterns of the samples were obtained using an X-ray powder diffractometer (D8 ADVANCE, Bruker, Germany) under Cu-K radiation. The power density was 100 mW / cm 2 A xenon lamp (CEL-HXF300, Ceaulight, China) was used to carry out the photothermal conversion experiment.
[0126] Moisture adsorption test
[0127] The water absorption isotherms of the prepared samples were measured using a moisture sorption analyzer (Aquadyne DVS, Quanta chrome, USA). Before testing, all samples were dried at 150 °C for 12 h.
[0128] Cyclic test: The sample selected 25°C and 30% relative humidity (30% RH) as the water absorption environment; 60°C and 30% relative humidity as the desorption environment, and the stability of the solar-driven honeycomb glass fiber-based composite MOF bulk desiccant prepared in Example 1 was subjected to 100 cycles of adsorption and desorption tests.
[0129] Results Analysis
[0130] In order to maximize the exposure of MOF to the air, a glass fiber-based MOF support process was adopted. Figure 1 The scanning electron microscope (SEM) images of the honeycomb glass fiber-based embryo, the honeycomb glass fiber-based functional embryo, and Example 1 ( Figure 1 a in the figure is a honeycomb glass fiber based embryo. Figure 1 b in the figure is a honeycomb glass fiber based functional embryo. Figure 1 c and d in the figure are the bulk moisture absorbents of the solar-driven honeycomb glass fiber-based composite MOF prepared in Example 1). Figure 1 As shown in a, the microstructure of the honeycomb glass fiber embryo (GF) is formed by countless fiber rods with smooth surfaces connected to each other. In order to improve the interfacial properties of the glass fiber substrate to MOF, a chitosan coating was first constructed on the GF as a hydrophilic material, and polydopamine was used as a photothermal conversion coating. Figure 1 b in the figure shows that the surface of the glass fiber rod is covered with a rough and compact polymer coating (hydrophilic coating encapsulating the photothermal conversion coating), which is conducive to the contact of organic ligands and the growth of MOF on the surface. After the solar-driven honeycomb glass fiber-based composite MOF bulk hygroscopic agent prepared in Example 1 successfully constructed a hybrid composite MOF on the substrate, a large number of uniform and dense crystals ( Figure 1 c and Figure 1d) in the figure, and is tightly bonded to the substrate, so that the MOF grains will not fall off. Figure 2 The X-ray diffraction (XRD) patterns of the bulk hygroscopic agents prepared in Example 1, Comparative Example 1 and Comparative Example 2 are shown. Among them, the XRD diffraction peaks presented in Example 1 match the intensity peaks of MIL-160 (Al) prepared in Comparative Example 1 and MOF-303 prepared in Comparative Example 2, further proving that the composite MOF grown on the honeycomb glass fiber-based functional embryo body of the present invention is composed of MIL-160 (Al) and MOF-303. It is worth noting that the glass fiber proposed in the present invention has a certain spatial distance, which can avoid the agglomeration of MOF grains and increase the contact area between MOF and air moisture.
[0131] Figure 3 The photothermal curves of Example 1 and Comparative Example 3 under sunlight irradiation are shown in FIG. Figure 3 As shown, the maximum temperature of the bulk hygroscopic agent of the honeycomb glass fiber-based composite MOF prepared from the honeycomb glass fiber-based embryo without polydopamine modification in Comparative Example 3 is only 46.51°C. In comparison, the surface temperature of the bulk hygroscopic agent of the solar-driven honeycomb glass fiber-based composite MOF prepared in Example 1 increases with time under sunlight irradiation and reaches the critical temperature (70.89°C) within 3 minutes, which further proves the advantage of the polydopamine proposed in the present invention as a photothermal conversion material for the water collection of the composite MOF bulk hygroscopic agent.
[0132] Figure 4 The water vapor isothermal adsorption curves of the block moisture absorbents prepared in Example 1, Comparative Example 1 and Comparative Example 2 at 25°C are shown in FIG. Figure 4 As shown, the bulk hygroscopic agent loaded with MIL-160 (Al) and the bulk hygroscopic agent loaded with MOF-303 both have type I adsorption isotherms, and the water absorption inflection point is within the 10% to 20% RH atmosphere. The saturated water absorption rates of the bulk hygroscopic agents prepared in Comparative Example 1 and Comparative Example 2 are 0.26 g / g and 0.29 g / g at 25°C, respectively. Similar to the steep adsorption curves of MIL-160 (Al) and MOF-303, the steep adsorption humidity atmosphere of the bulk hygroscopic agent of the solar-driven honeycomb glass fiber-based composite MOF prepared in Example 1 did not change significantly. However, the bulk hygroscopic agent of the solar-driven honeycomb glass fiber-based composite MOF of Example 1 exhibits better water adsorption energy absorption than Comparative Example 1 and Comparative Example 2. The saturated adsorption capacity of the bulk hygroscopic agent of the solar-driven honeycomb glass fiber-based composite MOF prepared in Example 1 reached 0.37 g / g at 25°C, showing a significant water collection advantage.
[0133] Figure 5This is a curve chart of 100 adsorption and desorption cycles of the bulk moisture absorbent of the solar-driven honeycomb glass fiber-based composite MOF prepared in Example 1. Figure 5 It can be seen that the water adsorption performance of the bulk desiccant of the solar-driven honeycomb glass fiber-based composite MOF prepared by the present invention has hardly degraded, indicating that the in-situ synthesis scheme of the bulk desiccant of the solar-driven honeycomb glass fiber-based composite MOF proposed by the present invention does not destroy the operating stability of the original MOF.
Claims
1. A method for preparing a solar-driven glass fiber-based composite MOF block moisture absorbent, characterized in that: The steps include: (1) Preparation of a honeycomb glass fiber-based functional embryo body: immersing the honeycomb glass fiber-based embryo body in a mixed solution containing a photothermal conversion coating and a hydrophilic coating under stirring, and taking out and drying the functional coating embryo body in which the hydrophilic coating is coated with the photothermal conversion coating after stirring; the photothermal conversion coating comprises one of polydopamine, polyaniline, and polypyrrole; (2) Preparation of composite MOF reaction solution: dissolving two organic dicarboxylic acid ligands and aluminum salt in water, heating at a constant temperature, adding NaOH solution, stirring to obtain a composite MOF reaction solution, and transferring it into a reaction tank; the two organic dicarboxylic acid ligands are 2,5-furandicarboxylic acid and 3,5-pyrazoledicarboxylic acid; and the molar ratio of the two organic dicarboxylic acid ligands is 1:1; (3) Preparation of solar-driven glass fiber-based composite MOF bulk desiccant: The functional coating embryo obtained in step (1) is immersed in a tank containing a composite MOF reaction solution and sealed, and a hydrothermal reaction is performed to obtain a crude product. After the crude product is washed and dried, a solar-driven glass fiber-based composite MOF bulk desiccant is obtained.
2. The method for preparing the solar-driven glass fiber-based composite MOF block moisture absorbent according to claim 1, characterized in that: In step (1), the hydrophilic coating is selected from one of chitosan, carboxymethyl chitosan and cyclodextrin.
3. The method for preparing the solar-driven glass fiber-based composite MOF block moisture absorbent according to claim 1, characterized in that: In step (1), the method for preparing the mixed solution containing the photothermal conversion coating and the hydrophilic coating is to mix a photothermal conversion coating solution with a concentration of 5-15 mg / mL with a hydrophilic coating solution with a concentration of 5-20 mg / mL.
4. The method for preparing the solar-driven glass fiber-based composite MOF block moisture absorbent according to claim 1, characterized in that: In step (2), the aluminum salt is one of aluminum chloride, aluminum sulfate, aluminum nitrate and aluminum acetate.
5. The method for preparing the solar-driven glass fiber-based composite MOF block moisture absorbent according to claim 1, characterized in that: In step (2), the molar ratio of sodium hydroxide to the organic dicarboxylic acid ligand is (0.8-2.4):
1.
6. The method for preparing the solar-driven glass fiber-based composite MOF block moisture absorbent according to claim 1, characterized in that: In step (2), the molar ratio of the aluminum salt to the organic dicarboxylic acid ligand is (0.8-1.2):
1.
7. The method for preparing the solar-driven glass fiber-based composite MOF block moisture absorbent according to claim 1, characterized in that: In step (3), the temperature of the hydrothermal reaction is 90-120° C., and the time of the hydrothermal reaction is 8-24 h.
8. A solar-driven glass fiber-based composite MOF block desiccant prepared by the preparation method according to any one of claims 1 to 7.