A catalytic cracking aid and its preparation method and application
The preparation of phosphate residue by modifying SAPO molecular sieve mother liquor wastewater for use in the preparation of catalytic cracking additives solves the environmental pollution and resource waste problems in the treatment of SAPO molecular sieve mother liquor wastewater and improves the propylene selectivity and yield in the catalytic cracking process.
Patent Information
- Application Number
- CN202111252617.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-27
AI Technical Summary
The treatment of SAPO molecular sieve mother liquor wastewater leads to environmental pollution and resource waste, and existing technologies are unable to effectively utilize the useful resources such as phosphorus, aluminum, and silicon contained therein.
SAPO molecular sieve mother liquor wastewater was modified to prepare phosphate residue, which was then mixed with ZSM-5 molecular sieve, clay and sol. The mixture was then spray-dried and calcined to prepare a catalytic cracking aid, which was used to improve propylene selectivity during catalytic cracking.
This improved the yield and concentration of propylene during catalytic cracking, reduced resource waste, and enabled the resource utilization of wastewater.
Smart Images

Figure RE-GDA0003436707440000111 
Figure RE-GDA0003436707440000121 
Figure RE-GDA0003436707440000131
Abstract
Description
Technical Field
[0001] The invention relates to a catalytic cracking aid for improving the yield and concentration of propylene in liquefied gas, and a preparation method and application thereof. Background Art
[0002] Silicoaluminophosphate molecular sieve (SAPO) plays an important role in the field of heterogeneous catalysis due to its unique properties. For example, it is used in methanol to olefins catalysts to increase the selectivity of light olefins, and in selective catalytic reduction catalysts (NOX-SCR) to reduce NOX emissions. At present, the industrial production of SAPO series molecular sieves mainly adopts the hydrothermal crystallization method, which mixes water, aluminum source, phosphorus source, silicon source and template agent and other raw materials in a certain order, stirs them evenly into a sol state, and then places them in a crystallization kettle with a set temperature for crystallization to form a molecular sieve slurry, and then obtains the molecular sieve product through solid-liquid separation and drying.
[0003] However, in the solid-liquid separation process of SAPO molecular sieve slurry, a large amount of SAPO molecular sieve mother liquor wastewater containing elements such as phosphorus, aluminum, silicon and organic templates will be generated. If it is directly discharged without treatment, it will harm the environment and also lead to the waste of useful resources such as phosphorus, aluminum and silicon. At present, the treatment of SAPO molecular sieve mother liquor wastewater mainly focuses on several aspects: one is to improve the recycling of organic templates, the second is to strengthen the resource utilization of phosphate waste residues, and the third is to directly reuse the mother liquor as a raw material in the preparation of molecular sieves or catalysts. Common methods for treating SAPO molecular sieve mother liquor include: using incineration treatment method, after treatment, the organic amines in the recovered wastewater can be reused in the synthesis of SAPO molecular sieves, and the enriched and recovered phosphates can be used as raw materials for the phosphate industry; using chemical precipitation method, that is, adding a certain amount of certain metal salts or polymers to the wastewater, so that the dissolved phosphate in the sewage forms insoluble salts and precipitates.
[0004] CN109092353A discloses a method for preparing a propylene production-increasing auxiliary agent, comprising the following steps: (1) removing the template agent in the SAPO molecular sieve synthesis mother liquor to obtain a refined mother liquor; (2) mixing the refined mother liquor, a carrier, a ZSM-5 molecular sieve and water to form a slurry, and spraying and solidifying the slurry to obtain the propylene production-increasing auxiliary agent. Summary of the invention
[0005] The present application provides a catalytic cracking aid, which contains, based on the dry weight of the catalytic cracking aid, 20 to 60% by weight of ZSM-5 molecular sieve, 10 to 60% by weight of clay, 10 to 45% by weight of sol and 1 to 30% by weight of phosphate waste residue obtained by treating SAPO molecular sieve mother liquor wastewater;
[0006] Based on the dry weight of the phosphate waste residue, the phosphate waste residue contains 5 to 35 weight % of Al2O3, 20 to 80 weight % of P2O5, 1 to 15 weight % of SiO2 and 2 to 45 weight % of modified metal oxides, wherein the modified metal oxides refer to oxides containing one or more metals selected from Mg, RE, Ti and Zr.
[0007] In one embodiment, the phosphate waste residue contains 5 to 25 wt % of Al2O3, 25 to 75 wt % of P2O5, 2 to 10 wt % of SiO2 and 5 to 40 wt % of modified metal oxides based on the dry weight of the phosphate waste residue.
[0008] In one embodiment, based on the dry weight of the catalytic cracking aid, the catalytic cracking aid contains 25-55 wt% of ZSM-5 molecular sieve, 15-50 wt% of clay, 10-40 wt% of sol and 5-25 wt% of phosphate waste residue.
[0009] In one embodiment, the phosphate waste residue is prepared as follows:
[0010] The SAPO molecular sieve mother liquor wastewater and the compound containing the modified metal are mixed, the pH value of the mixed slurry is adjusted to 5-10, the mixed slurry is reacted at 20-90° C. for 30-120 minutes, and then evaporated and dried to obtain the phosphate waste residue obtained by treating the SAPO molecular sieve mother liquor wastewater.
[0011] In one embodiment, the mixing of SAPO molecular sieve mother liquor wastewater and the compound containing modified metals means that, based on the dry weight obtained after mixing, 55-98% of SAPO molecular sieve mother liquor wastewater and 2-45% of the compound containing modified metals are mixed.
[0012] In one embodiment, the pH value of the slurry is 5-10, preferably 6-9; and the reaction temperature is 20-90°C.
[0013] The present application also provides a method for preparing the catalytic cracking aid, comprising:
[0014] The phosphate waste residue obtained by treating ZSM-5 molecular sieve, sol, SAPO molecular sieve mother liquor wastewater, clay and water are mixed to form slurry, and the slurry is spray-dried, formed and calcined to obtain the catalytic cracking aid.
[0015] In one embodiment, the method comprises:
[0016] Mixing the clay, the phosphate waste residue and water to obtain a first slurry;
[0017] Mixing the first slurry, the sol and the molecular sieve to obtain a second slurry;
[0018] The second slurry is spray-dried and calcined to obtain the catalytic cracking aid.
[0019] In one embodiment, the ZSM-5 molecular sieve is selected from HZSM-5 molecular sieve, ZSM-5 molecular sieve containing a modifying element, and a combination thereof, wherein the modifying element in the ZSM-5 molecular sieve containing a modifying element is selected from one or more of phosphorus, iron, rare earth elements, Zn, Cu, Mg, Zr, Ti, and B;
[0020] The clay is selected from one or more of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth, and synthetic clay, wherein one or more of kaolin, metakaolin, and diatomaceous earth are preferred;
[0021] The sol is selected from aluminum sol, silica sol or a mixture of the two.
[0022] In one embodiment, the ZSM-5 molecular sieve containing a modifying element is selected from a phosphorus-containing ZSM-5 molecular sieve, an iron-containing ZSM-5 molecular sieve, and a rare earth element-containing ZSM-5 molecular sieve; preferably, the iron-containing ZSM-5 molecular sieve further contains phosphorus; and the rare earth element-containing ZSM-5 molecular sieve further contains phosphorus.
[0023] The present application also provides the use of the catalytic cracking aid of the present application in catalytic cracking, and a catalytic cracking catalyst system, comprising the catalytic cracking aid of the present application. In one embodiment, the catalytic cracking catalyst system further comprises a catalytic cracking catalyst. In one embodiment, based on the total weight of the catalytic cracking catalyst system, the content of the catalytic cracking aid is 1 to 50% by weight, preferably 5 to 30% by weight.
[0024] The phosphate waste residue contained in the catalytic cracking aid of the present invention is obtained by modifying the SAPO molecular sieve mother liquor, and contains rich phosphorus and modified metal components, which can adjust the activity and selectivity of the catalytic cracking aid to a certain extent, and improve the coke selectivity; at the same time, the phosphate waste residue also contains a small amount of SAPO molecular sieve crystals, which can improve the propylene selectivity of the catalytic cracking aid of the present invention containing the phosphate waste residue to a certain extent. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below through examples. Through these examples, the features and advantages of the present invention will become clearer and more specific.
[0026] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.
[0027] In addition, the technical features involved in different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.
[0028] On the one hand, the present application provides a catalytic cracking aid, which contains, based on the dry weight of the catalytic cracking aid, 20 to 60 wt% of ZSM-5 molecular sieve, 10 to 60 wt% of clay, 10 to 45 wt% of sol and 1 to 30 wt% of phosphate waste residue obtained by treating SAPO molecular sieve mother liquor wastewater;
[0029] Based on the dry weight of the phosphate waste residue, the phosphate waste residue contains 1 to 30 weight % of Al2O3, 30 to 80 weight % of P2O5, 1 to 10 weight % of SiO2 and 5 to 40 weight % of modified metal oxides, wherein the modified metal oxides refer to oxides containing one or more metals selected from Mg, RE, Ti and Zr.
[0030] In the present application, the ZSM-5 molecular sieve may be selected from HZSM-5 molecular sieve, ZSM-5 molecular sieve containing a modifying element and a combination thereof, wherein the modifying element of the ZSM-5 molecular sieve containing a modifying element is selected from one or more of phosphorus, iron, rare earth elements, Zn, Cu, Mg, Zr, Ti, and B. For example, the ZSM-5 molecular sieve containing a modifying element may be a ZSM-5 molecular sieve containing phosphorus, a ZSM-5 molecular sieve containing iron, a ZSM-5 molecular sieve containing a rare earth element, and a ZSM-5 molecular sieve containing other modifying elements or any combination thereof, wherein the other modifying elements may be selected from Zn, Cu, Mg, Zr, Ti, B, and the like. In one embodiment, the ZSM-5 molecular sieve containing a modifying element may be selected from a ZSM-5 molecular sieve containing phosphorus and / or iron, a ZSM-5 molecular sieve containing phosphorus and / or rare earth, a ZSM-5 molecular sieve modified by other elements, or any combination thereof, wherein the other elements may be selected from Zn, Cu, Mg, Zr, Ti, B, etc. In one embodiment, the ZSM-5 molecular sieve containing a modifying element may be selected from a ZSM-5 molecular sieve containing phosphorus, a ZSM-5 molecular sieve containing iron, and a ZSM-5 molecular sieve containing a rare earth element; preferably, the ZSM-5 molecular sieve containing iron may further contain phosphorus; and the ZSM-5 molecular sieve containing a rare earth element may further contain phosphorus.
[0031] In one embodiment, based on the dry weight of the catalytic cracking aid, the ZSM-5 molecular sieve may account for 20 to 60% by weight, in particular, 25 to 55% by weight.
[0032] In the present application, the clay can be selected from one or more of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth, and synthetic clay, wherein one or more of kaolin, metakaolin, and diatomaceous earth are preferred. In one embodiment, the clay can account for 10 to 60% by weight, especially 15 to 50% by weight, based on the dry weight of the catalytic cracking aid.
[0033] In the present application, the sol can be selected from one of aluminum sol and silica sol or a mixture of the two. These sols can be purchased commercially or prepared according to existing methods. For example, the aluminum sol can be aluminum phosphate sol, which can be prepared according to the methods provided in patents CN1008974C and CN1083512A. Silica sol can be prepared according to the methods provided in U.S. Patents US3957689 and US3867308. In one embodiment, based on the dry weight of the catalytic cracking aid, the sol can account for 10 to 45% by weight, especially 10 to 40% by weight.
[0034] In the present application, the catalytic cracking aid also includes phosphate waste residue obtained by treating SAPO molecular sieve mother liquor wastewater. The phosphate waste residue is prepared by modifying SAPO molecular sieve mother liquor wastewater. In one embodiment, based on the dry weight of the phosphate waste residue, the phosphate waste residue contains 5 to 35 weight % of Al2O3, 20 to 80 weight % of P2O5, 1 to 15 weight % of SiO2 and 2 to 45 weight % of modified metal oxide, and the modified metal oxide refers to an oxide containing one or more metals of Mg, RE, Ti, and Zr. In one embodiment, based on the dry weight of the phosphate waste residue, the phosphate waste residue contains 5 to 25 weight % of Al2O3, 25 to 75 weight % of P2O5, 2 to 10 weight % of SiO2 and 5 to 40 weight % of modified metal oxide. In one embodiment, based on the dry weight of the catalytic cracking aid, the phosphate waste residue may account for 1 to 30% by weight, in particular 5 to 25% by weight.
[0035] In one embodiment, the phosphate waste residue can be prepared as follows:
[0036] The SAPO molecular sieve mother liquor wastewater and the compound containing the modified metal are mixed, the pH value of the mixed slurry is adjusted to 5-10, the mixed slurry is reacted at 20-90° C. for 30-120 minutes, and then evaporated and dried to obtain the phosphate waste residue obtained by treating the SAPO molecular sieve mother liquor wastewater.
[0037] In one embodiment, the SAPO molecular sieve mother liquor wastewater is a liquid after solid-liquid separation in the preparation of one or more SAPO molecular sieves having a six-membered ring, an eight-membered ring, a ten-membered ring, and a twelve-membered ring structure. The SAPO molecular sieve having a six-membered ring structure is one or more of SAPO-20, SAPO-25, and SAPO-28; the SAPO molecular sieve having an eight-membered ring structure is one or more of SAPO-17, SAPO-18, SAPO-26, SAPO-33, SAPO-34, SAPO-35, SAPO-39, SAPO-42, SAPO-43, SAPO-44, and SAPO-47; the SAPO molecular sieve having a ten-membered ring structure is one or more of SAPO-11, SAPO-31, and SAPO-41; the SAPO molecular sieve having a twelve-membered ring structure is one or more of SAPO-5, SAPO-36, SAPO-37, SAPO-40, and SAPO-46.
[0038] The modified metal may be selected from one or more of Mg, RE (rare earth metal), Ti, and Zr. The compound containing the modified metal may be a magnesium compound, which may be one or more of magnesium oxide, magnesium carbonate, magnesium hydroxide, magnesium chloride, magnesium sulfate, and magnesium nitrate; the compound containing the modified metal may be a rare earth compound, which may be one or more of rare earth oxide, rare earth carbonate, rare earth chloride, and rare earth nitrate; the compound containing the modified metal may be a titanium compound, which may be one or more of titanium oxide, titanium sulfate, titanium oxysulfate, titanium tetrachloride, titanium trichloride, tetrabutyl titanate, ammonium fluorotitanate, and titanium hydroxide; the compound containing the modified metal may be a zirconium compound, which may be one or more of zirconium oxide, zirconium hydroxide, zirconium tetrachloride, zirconium sulfate, zirconium nitrate, zirconium oxychloride, zirconium acetate, and zirconium isopropoxide.
[0039] In one embodiment, the mixing of SAPO molecular sieve mother liquor wastewater and the compound containing modified metals means that, based on the dry weight obtained after mixing, 55-98% of SAPO molecular sieve mother liquor wastewater and 2-45% of the compound containing modified metals are mixed.
[0040] In one embodiment, the pH value of the slurry is adjusted to 5 to 10, preferably 6 to 9. In one embodiment, the slurry is reacted at a reaction temperature of 20 to 90° C. for a period of time, such as 30 to 120 minutes; then the mixed slurry is evaporated and dried to obtain the phosphate waste residue. In one embodiment, based on the dry weight of the phosphate waste residue, the phosphate waste residue contains 5 to 35 weight % of Al2O3, 20 to 80 weight % of P2O5, 1 to 15 weight % of SiO2 and 2 to 45 weight % of modified metal oxides, wherein the modified metal oxide refers to an oxide containing one or more metals of Mg, RE, Ti, and Zr. In one embodiment, based on the dry weight of the phosphate waste residue, the phosphate waste residue contains 5 to 25 weight % of Al2O3, 25 to 75 weight % of P2O5, 2 to 10 weight % of SiO2 and 5 to 40 weight % of modified metal oxides.
[0041] The evaporation can be performed by evaporation methods well known to those skilled in the art, such as single-effect evaporator or multiple-effect evaporator, concentrating evaporator, falling film evaporation, or reduced pressure dehydration, vacuum drying, etc. The purpose of evaporation is to remove the organic template contained in the mother liquor wastewater and recycle it.
[0042] The drying can be carried out by constant temperature drying, air flow drying, spray drying, vacuum drying, freeze drying, etc., which are well known to those skilled in the art. The purpose of drying is to remove the residual organic matter in the phosphate waste residue. The drying temperature is 80 to 300° C., preferably, the temperature is 100 to 250° C., and the time can be selected according to actual needs, and there is no specific limitation on this.
[0043] The catalytic cracking aid can be prepared as follows, comprising:
[0044] The ZSM-5 molecular sieve, sol, phosphate waste residue, clay and water are mixed to form slurry, and the slurry is spray-dried, shaped and calcined to obtain the catalytic cracking aid.
[0045] In one embodiment, the ZSM-5 molecular sieve, sol, phosphate waste residue, clay and water are mixed to form a slurry, which means that based on the dry weight of the catalytic cracking aid, 20 to 60 weight percent of the ZSM-5 molecular sieve, 10 to 45 weight percent of the sol, 1 to 30 weight percent of the phosphate waste residue, and 10 to 60 weight percent of the clay are mixed in water to form a slurry with a solid content of 10 to 50 weight percent. In one embodiment, when the slurry is mixed to form a slurry, the weight ratio of ZSM-5 molecular sieve: sol: phosphate waste residue: clay can be 20 to 60: 10 to 45: 1 to 30: 10 to 60.
[0046] In one embodiment, the method for preparing a catalytic cracking aid may include: mixing clay, phosphate waste residue and water to obtain a first slurry; mixing the first slurry, sol and the ZSM-5 molecular sieve to form a second slurry; spray drying and calcining the obtained second slurry. The mixing and slurrying time is not specifically limited, for example, it can be 30 to 120 minutes.
[0047] The spray drying is a technique known to those skilled in the art, and the temperature of the spray tail gas can be controlled at 100-250° C. The roasting treatment is also well known to those skilled in the art, and can be carried out in a muffle furnace, for example, and the roasting treatment conditions may include: a temperature of 350-800° C., preferably 400-650° C., a roasting time of 0.5-6 hours, preferably 1-4 hours; the roasting can be carried out in any atmosphere, for example, in air or an inert atmosphere, the inert atmosphere contains an inert gas, and the inert gas may include nitrogen, helium, argon, etc.
[0048] The present invention also provides the use of the catalytic cracking aid of the present claim in the catalytic cracking of heavy oil.
[0049] According to the present invention, when the catalytic cracking aid of the present invention is used in a catalytic cracking process, it can be mixed with a catalytic cracking catalyst before use. In a specific embodiment, based on the total amount of the catalytic cracking aid and the cracking catalyst, the content of the catalytic cracking aid provided by the present invention is 1 to 50% by weight, preferably 5 to 30% by weight.
[0050] The present invention also relates to a catalytic cracking catalyst system, comprising the catalytic cracking aid and the catalytic cracking catalyst of the present application. In one embodiment, based on the total weight of the catalytic cracking catalyst system, the content of the catalytic cracking aid is 1 to 50 weight %, preferably 5 to 30 weight %.
[0051] The catalytic cracking catalyst that can be used in the present application can be various catalytic cracking catalysts commonly used in the art. For example, based on the total weight of the catalyst, the catalytic cracking catalyst can include 15 to 65% by weight of natural minerals, 10 to 30% by weight of inorganic oxides, and 25 to 75% by weight of zeolite. The zeolite, as an active component, can be selected from one or more mixtures of Y zeolite, mordenite, beta zeolite, and zeolite with MFI structure (e.g., ZRP zeolite). Natural minerals can be selected from one or more of kaolin, halloysite, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite, and rectorite. The inorganic oxide can be selected from one or more of silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, and amorphous silicon aluminum. These catalytic cracking catalysts may be catalysts described in CN1064098A, CN1064499A, CN107149917A, CN107973313A, etc., or may be purchased, for example, from Sinopec Catalyst Co., Ltd., etc.
[0052] The present invention is further described below by way of examples, but the present invention is not limited thereto.
[0053] SAPO molecular sieve mother liquor wastewater comes from the mother liquor wastewater generated in the production of SAPO molecular sieves. The ICP element analysis results are as follows: P content 28000ug / g, Al content 7800ug / g, Si content 700ug / g, solid content 14 weight%.
[0054] Kaolin was produced by Suzhou Kaolin Company with a solid content of 76% by weight;
[0055] The silica sol was produced by Qingdao Micro-Nano Silica Gel Technology Co., Ltd., with a solid content of 27% by weight and a pH of 2-3;
[0056] Aluminum phosphate sol was produced by Sinopec Catalyst Co., Ltd., with a solid content of 30% and a P / Al molar ratio of 2.5;
[0057] The hydrogen-type ZSM-5 zeolite was produced by Sinopec Catalyst Co., Ltd., with a molar ratio of SiO2 to Al2O3 of 42, a Na2O content of 3.5% by weight, and a solid content of 80% by weight;
[0058] Phosphorus-modified ZSM-5 zeolite was produced by Sinopec Catalyst Co., Ltd., with a SiO2 to Al2O3 molar ratio of 45, a Na2O content of 0.12 wt%, a P2O5 content of 2.1 wt%, and a solid content of 83 wt%;
[0059] The ASAP 2405N V1.01 automatic adsorption instrument from Micromeritics of the United States was used, and the low-temperature static nitrogen adsorption capacity method was used. The sample was heated to 1.33×10-2 Pa, vacuum degassing at 300 ° C for 4 h, using N2 as the adsorption medium, and measuring the adsorption-desorption isotherm of the sample at 77.4 K. The specific surface area (SBET) of the sample was calculated according to the BET formula, and the volume of N2 adsorbed by the sample at the relative pressure p / p0 = 0.98 was measured and converted into liquid nitrogen volume, i.e., pore volume;
[0060] The composition of the samples was determined by X-ray fluorescence spectroscopy (XRF).
[0061] Preparation Example - Preparation of Phosphate Waste Slag
[0062] Preparation Example 1
[0063] 1000 g of SAPO molecular sieve mother liquor wastewater and 71 g of magnesium oxide were weighed and mixed, the slurry pH was adjusted to 10, and the mixed slurry was reacted at 25° C. for 60 min; the mixed slurry was then evaporated and dried to obtain the phosphate waste residue A1 of the present invention, which contained 15.3 wt % Al2O3, 65.5 wt % P2O5, 1.6 wt % SiO2 and 17.6 wt % MgO on a dry basis.
[0064] Preparation Example 2
[0065] 1000 g of SAPO molecular sieve mother liquor wastewater and 186 ml of 270 g / l RECl3 solution were weighed and mixed, the slurry pH was adjusted to 9.5, and the mixed slurry was reacted at 40° C. for 90 min; then the mixed slurry was evaporated and dried to obtain the phosphate waste residue A2 of the present invention, which contained 13.7 wt % of Al2O3, 58.6 wt % of P2O5, 1.4 wt % of SiO2 and 23.6 wt % of rare earth oxide on a dry basis.
[0066] Preparation Example 3
[0067] 1000 g of SAPO molecular sieve mother liquor wastewater and 157 g of zirconium oxychloride were weighed and mixed, the slurry pH was adjusted to 10.0, and the mixed slurry was reacted at room temperature for 120 min; then the mixed slurry was evaporated and dried to obtain the phosphate waste residue A3 of the present invention, which contained 13.0 wt% of Al2O3, 55.7 wt% of P2O5, 1.3 wt% of SiO2 and 22.5 wt% of zirconium oxide on a dry basis.
[0068] Preparation Example 4
[0069] 1000 g of SAPO molecular sieve mother liquor wastewater and 42 g of titanium tetrachloride were weighed and mixed, the slurry pH was adjusted to 9.5, and the mixed slurry was reacted at room temperature for 60 min; then the mixed slurry was evaporated and dried to obtain the phosphate waste residue A4 of the present invention, which contained 16.4 wt % of Al2O3, 70.5 wt % of P2O5, 1.7 wt % of SiO2 and 11 wt % of titanium oxide on a dry basis.
[0070] Examples 1 to 6 are examples of preparing catalytic cracking aids, and Comparative Examples 1 and 2 are examples of preparing catalytic cracking aids.
[0071] Example 1
[0072] 164 g of kaolin, 100 g of phosphate waste residue A1 and 861 g of deionized water were mixed in a slurrying tank and slurried for 60 minutes, and then 333 g of aluminum phosphate sol and 93 g of silica sol were added, and the slurry formed by slurrying of 188 g of hydrogen-type ZSM-5 molecular sieve and 241 g of deionized water was added, and stirred for 30 minutes. The obtained slurry was then spray-dried and formed, and calcined at 500°C for 2 hours to obtain the catalytic cracking aid C1 provided by the present invention.
[0073] Example 2
[0074] 197 g of kaolin, 75 g of phosphate waste A2 and 853 g of deionized water were mixed in a slurrying tank and slurried for 60 minutes, and then 333 g of aluminum phosphate sol and 93 g of silica sol were added, and the slurry was continued for 30 minutes. Finally, 188 g of hydrogen ZSM-5 molecular sieve and 241 g of deionized water were added to form a slurry, stirred for 30 minutes, and then the obtained slurry was spray-dried and formed, and calcined at 500°C for 2 hours to obtain the catalytic cracking aid C2 provided by the present invention.
[0075] Example 3
[0076] 263 g of kaolin, 25 g of phosphate waste A3 and 837 g of deionized water were mixed in a slurrying tank and slurried for 60 minutes, and then 333 g of aluminum phosphate sol and 93 g of silica sol were added, and the slurry was continued for 30 minutes. Finally, 188 g of hydrogen ZSM-5 molecular sieve and 241 g of deionized water were added to form a slurry, stirred for 30 minutes, and then the obtained slurry was spray-dried and formed, and calcined at 500°C for 2 hours to obtain the catalytic cracking aid C3 provided by the present invention.
[0077] Example 4
[0078] 99 g of kaolin, 417 g of aluminum phosphate sol and 185 g of silica sol were mixed in a slurrying tank and slurried for 90 minutes. Then, 241 g of phosphorus-modified ZSM-5 molecular sieve, 50 g of phosphate waste residue A4 and 423 g of deionized water were added to form a slurry, stirred for 60 minutes, and then the obtained slurry was spray-dried and formed, and calcined at 550° C. for 1.5 hours to obtain the catalytic cracking aid C4 provided by the present invention.
[0079] Example 5
[0080] 178 g of kaolin, 250 g of aluminum phosphate sol and 148 g of silica sol were mixed in a slurrying tank and slurried for 90 minutes. Then, 151 g of phosphorus-modified ZSM-5 molecular sieve, 125 g of phosphate waste residue A1 and 439 g of deionized water were added to form a slurry, stirred for 60 minutes, and then the obtained slurry was spray-dried and formed, and calcined at 550° C. for 1.5 hours to obtain the catalytic cracking aid C5 provided by the present invention.
[0081] Example 6
[0082] A slurry formed by beating 86 grams of kaolin, 25 grams of phosphate waste residue A1 and 339 grams of deionized water is stirred for 60 minutes; then a slurry formed by beating 313 grams of phosphorus-modified ZSM-5 molecular sieve and 345 grams of deionized water is added, and stirring is continued for 30 minutes; finally, 500 grams of aluminum phosphate sol and 37 grams of silica sol are added, and beating is continued for 30 minutes. The obtained slurry is then spray-dried and formed, and calcined at 500°C for 2 hours to obtain the catalytic cracking aid C6 provided by the present invention.
[0083] Comparative Example 1
[0084] According to the method of Example 1, a catalytic cracking aid DC1 free of phosphate waste residue was prepared.
[0085] 296 g of kaolin, 333 g of aluminum phosphate sol and 93 g of silica sol were mixed and slurried for 90 minutes, and finally slurry formed by slurrying 188 g of hydrogen-type ZSM-5 molecular sieve and 207 g of deionized water was added, and stirring was continued for 30 minutes. The obtained slurry was then spray-dried and formed, and calcined at 500°C for 2 hours to obtain the catalytic cracking aid DC1 provided by the present invention.
[0086] Comparative Example 2
[0087] Catalytic cracking aid DC2 was prepared according to the method of Example 3 of CN109092353A.
[0088] The SAPO molecular sieve synthesis mother liquor is distilled to obtain the distillation residue of the SAPO molecular sieve synthesis mother liquor. Under stirring conditions, water (controlling the final slurry solid content of 41%), the distillation residue of the SAPO molecular sieve synthesis mother liquor, and kaolin are added to the stirring kettle, stirred for 45 minutes, and then H-ZSM-5 molecular sieve is added, stirred for 90 minutes, and the mixing ratio is kaolin: the distillation residue of the SAPO molecular sieve synthesis mother liquor (on a dry basis): ZSM-5 molecular sieve = 38:23:39, based on the dry basis of the catalytic cracking aid, the slurry is sprayed after gelation, and the obtained spray microspheres are roasted at 450°C for 5 hours to obtain the catalytic cracking aid DC2 provided by the present invention.
[0089] Table 1 Composition of additives
[0090]
[0091] Test Case
[0092] The catalytic cracking aids C1-C6 prepared in Examples 1-6 of the present invention, the catalytic cracking aids DC1-DC2 prepared in Comparative Examples 1-2 and the industrial catalyst (provided by Qilu Branch of Sinopec Catalyst Co., Ltd., trade name HSC catalyst, main properties are shown in Table 2) were mixed into a catalyst mixture in a weight ratio of 10:90, and the catalyst mixture was aged at 800°C and 100% water vapor for 17 hours in a fixed bed aging device. Then, the catalyst mixture was evaluated on an ACE device, and the properties of the raw oil used for evaluation are shown in Table 3. The reaction temperature was 500°C, the catalyst-oil ratio was 6.02, and the evaluation results were listed in Table 4.
[0093] Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield; propylene concentration in liquefied gas = propylene yield / liquefied gas yield.
[0094] Table 2 Properties of industrial catalysts
[0095] name Chemical composition / % <![CDATA[RE2O3]]> 3.4 <![CDATA[Al2O3]]> 52.3 <![CDATA[Na2O]]> 0.16 Physical properties <![CDATA[Specific surface area / (m 2 ×g -1 )]]> 269 <![CDATA[Pore volume / (mL×g -1 )]]> 0.38 <![CDATA[Bulk density / (g×cm -3 )]]> 0.75 Screening mass composition / % 0~20mm 1.5 0~40mm 12.8 0~149mm 90.1 APS mm 76.8 Wear index / (%) 1.2 MA(800℃ / 4h) 78
[0096] Table 3 Raw oil properties
[0097]
[0098]
[0099] The results in Table 4 show that, compared with Comparative Examples 1 and 2, the additives containing phosphate waste residue prepared in Examples 1 to 6 of the present invention have a higher propylene yield, and the propylene concentration in the liquefied gas is significantly increased, indicating that the catalytic cracking additive containing phosphate waste residue (modified SAPO molecular sieve synthesis mother liquor) has a stronger propylene selectivity.
[0100] The present application has been described above in conjunction with preferred embodiments, but these embodiments are only exemplary and serve only as an illustration. On this basis, various replacements and improvements may be made to the present application, all of which fall within the scope of protection of the present application.
Claims
1. A catalytic cracking aid, which comprises, based on the dry weight of the catalytic cracking aid, 20-60 wt % of ZSM-5 molecular sieve, 10-60 wt % of clay, 10-45 wt % of sol and 1-30 wt % of phosphate waste residue obtained by treating SAPO molecular sieve mother liquor wastewater; Based on the dry weight of the phosphate waste residue, the phosphate waste residue contains 5 to 35 weight % of Al 2 O 3 , 20~80 wt% P 2 O 5 , 1~15 wt% SiO 2 and 2 to 45 wt % of a modified metal oxide, wherein the modified metal oxide refers to an oxide containing one or more metals selected from Mg, RE, Ti, and Zr; The phosphate waste residue obtained by treating the SAPO molecular sieve mother liquor wastewater is prepared as follows: Mixing SAPO molecular sieve mother liquor wastewater and a compound containing a modified metal, adjusting the pH value of the mixed slurry to 5-10, reacting the mixed slurry at 20-90° C. for 30-120 min, and then evaporating and drying the mixed slurry to obtain a phosphate waste residue obtained by treating the SAPO molecular sieve mother liquor wastewater; The sol is selected from aluminum sol, silica sol or a mixture of the two.
2. The catalytic cracking aid according to claim 1, in, Based on the dry weight of the phosphate waste residue, the phosphate waste residue contains 5 to 25 weight % of Al 2 O 3 , 25~75 wt% P 2 O 5 , 2~10 wt% SiO 2 and 5 to 40 wt % of a modified metal oxide.
3. The catalytic cracking aid according to claim 1 or 2, in, Based on the dry weight of the catalytic cracking aid, the catalytic cracking aid contains 25-55 wt % of ZSM-5 molecular sieve, 15-50 wt % of clay, 10-40 wt % of sol and 5-25 wt % of phosphate waste residue obtained by treating SAPO molecular sieve mother liquor wastewater.
4. The catalytic cracking aid according to claim 1, in, The mixing of SAPO molecular sieve mother liquor wastewater and the modified metal-containing compound means that, based on the dry weight obtained after mixing, 55-98% of SAPO molecular sieve mother liquor wastewater and 2-45% of the modified metal-containing compound are mixed.
5. The catalytic cracking aid according to claim 1, in, The pH value of the slurry is 6-9.
6. A method for preparing the catalytic cracking aid according to any one of claims 1 to 5, include: The phosphate waste residue obtained by treating ZSM-5 molecular sieve, sol, SAPO molecular sieve mother liquor wastewater, clay and water are mixed to form slurry, and the slurry is spray-dried, formed and calcined to obtain the catalytic cracking aid.
7. The method according to claim 6, in, The method comprises: Mixing the clay, the phosphate waste residue and water to obtain a first slurry; Mixing the first slurry, the sol and the molecular sieve to obtain a second slurry; The second slurry is spray-dried and calcined to obtain the catalytic cracking aid.
8. The method according to claim 6, in, The ZSM-5 molecular sieve is selected from HZSM-5 molecular sieve, ZSM-5 molecular sieve containing modified elements and combinations thereof, wherein the modified elements in the ZSM-5 molecular sieve containing modified elements are selected from one or more of phosphorus, iron, rare earth elements, Zn, Cu, Mg, Zr, Ti and B; The clay is selected from one or more of kaolin, metakaolin, bentonite, montmorillonite, sepiolite, attapulgite, diatomaceous earth and synthetic clay.
9. The method according to claim 6, in, The clay is selected from one or more of kaolin, metakaolin, and diatomaceous earth; The sol is selected from aluminum sol, silica sol or a mixture of the two.
10. The method according to claim 8, in, The ZSM-5 molecular sieve containing modified elements is selected from ZSM-5 molecular sieve containing phosphorus, ZSM-5 molecular sieve containing iron, and ZSM-5 molecular sieve containing rare earth elements.
11. The method according to claim 10, in, The iron-containing ZSM-5 molecular sieve further contains phosphorus; the rare earth element-containing ZSM-5 molecular sieve further contains phosphorus.
12. Use of the catalytic cracking aid according to any one of claims 1 to 5 and the catalytic cracking aid obtained by the method according to any one of claims 6 to 11 in catalytic cracking.
13. A catalytic cracking catalyst system, comprising the catalytic cracking aid according to any one of claims 1 to 5 or the catalytic cracking aid obtained by the method according to any one of claims 6 to 11, and a catalytic cracking catalyst.
14. The catalytic cracking catalyst system according to claim 13, in, Based on the total weight of the catalytic cracking catalyst system, the content of the catalytic cracking aid is 1 to 50 weight %.
15. The catalytic cracking catalyst system according to claim 13, in, Based on the total weight of the catalytic cracking catalyst system, the content of the catalytic cracking aid is 5-30% by weight.
Citation Information
Patent Citations
Hydrocarbon catalytic cracking catalyst compositions and method therefor
CN1008974B
Cracking and catalytic agent
CN1064098A
Rare-earth Y molecular sieve cracking catalyst and preparation thereof
CN1064499A
Alumina sol, preparation method and application thereof, catalytic cracking catalyst, preparation method of catalyst
CN107149917A
Mesopore-rich Y molecular sieve and preparation method thereof
CN107973313A