A high-strength mineralized aerated building block prepared from solid waste and preparation method thereof
Through the mineralization reaction of calcium solid waste and silicon-aluminum solid waste with carbon dioxide gas, combined with foaming agent and heating agent, the problems of high energy consumption and insufficient strength in the production of aerated blocks are solved, and high efficiency and low carbon are achieved The preparation of mineralized aerated blocks has improved the strength and resource utilization of the product.
Patent Information
- Application Number
- CN202211027383.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-08-25
AI Technical Summary
The processing technology of existing aerated blocks consumes high energy, low production efficiency, and insufficient mineralization and strength, making it difficult to meet the low-carbon and environmental protection requirements of green buildings.
Calcium solid waste and silicon aluminum solid waste are used as the main raw materials to conduct mineralization reactions through contact with carbon dioxide gas, combined with foaming agent and heating agent, and regulate the mineralization process to achieve water without external heating sources and water vapor. Thermal reaction increases the strength and weight gain rate of aerated blocks.
Production of mineralized aerated blocks with light quality and high strength under low energy consumption shortens production time, reduces raw material costs, effectively utilizes solid waste, promotes the low mineralization of aerated blocks, and solves the enterprise solid waste disposal and carbon emission issues.
Smart Images

Figure GDA0004022345420000061 
Figure GDA0004022345420000062 
Figure GDA0004022345420000111
Abstract
Description
Technical Field
[0001] The present invention relates to a high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, and relates to the field of C04B28 / 00, and in particular to the field of building material compositions. Background Art
[0002] Driven by green buildings, environmentally friendly and energy-saving building materials have gradually become the mainstream of the construction industry. Aerated blocks use industrial waste as raw materials, have the characteristics of recycling and environmental protection, are excellent green building materials, and have been increasingly used in prefabricated buildings and green buildings. At present, the processing technology of aerated blocks mainly includes traditional steam curing and natural curing. Steam curing consumes huge energy and takes a long time. The high cement content is not conducive to low carbon. Natural curing is characterized by too long curing age, low production efficiency, and high loss of raw materials.
[0003] Chinese invention patent CN202210408960.6 discloses a lightweight and heat-insulating aerated block and its preparation method. By using acetone as a foaming agent and combining it with a special steam curing process, the pores of the aerated block are evenly distributed and the pore size is even, thereby improving the compressive strength of the block. However, the steam curing time required is long, high energy consumption is required, and a large amount of cement is added to the raw material end, which is not conducive to low-carbon environmental protection. Chinese invention patent CN113698229A discloses a process for curing fly ash aerated blocks by coupling steam and carbon dioxide. The concentration of carbon dioxide introduced in the carbon dioxide mineralization curing is above 80%, the pressure is 0.5MPa~2.0MPa, and the mineralization is 2-4h; after the mineralization curing, the autoclave curing is carried out at a temperature of 170~200℃, a pressure of 0.8MPa~1.6MPa, and the curing is 4-6h. This curing method requires pre-mineralization and then autoclaving. Although it shortens the curing time to a certain extent, the strength is still low and the degree of mineralization is not high. Summary of the invention
[0004] In order to improve the strength of aerated building blocks, increase the weight gain rate and carbon fixation rate of aerated building blocks, and reduce the energy consumption in the aerated building block preparation project, the first aspect of the present application provides a high-strength mineralized aerated building block prepared from solid waste, wherein the mineralized aerated building block is made of basic materials including calcium solid waste, silicon-aluminum solid waste and a foaming agent, and water is added to form a building block; the building block contacts with a carbon dioxide-containing gas to produce a mineralization reaction, and the heat generated by the mineralization reaction is controlled by adjusting the building block formula and the mineralization process, so that the system reaches the environment and temperature required for the hydrothermal reaction in the absence of an external heat source and water vapor, thereby improving the strength of the mineralized aerated building block.
[0005] As a preferred embodiment, the preparation raw materials include solid materials, water and foaming agents. The solid materials include 15-80 parts of calcium solid waste, 40-110 parts of silicon-aluminum solid waste, 0-40 parts of heating agent, 1-50 parts of hardener and 0.1-5 parts of water reducing agent by weight.
[0006] As a preferred embodiment, the solid material includes, by weight, 38-68 parts of calcareous solid waste, 60-90 parts of siliceous and aluminumous solid waste, 20-40 parts of exothermic agent, 30-50 parts of hardener, and 0.1-3 parts of water reducing agent.
[0007] The applicant found in the experiment that the weight ratio of calcium solid waste to silicon-aluminum solid waste (20-35): (30-45) can significantly improve the weight gain rate of the prepared mineralized aerated building blocks, and at the same time have excellent compressive strength. The possible reason is that when the weight ratio of calcium solid waste to silicon-aluminum solid waste is within the range of (20-35): (30-45), the contact probability between the building blocks and carbon dioxide increases, the system releases heat significantly, the building blocks have high mineralization efficiency, and the weight gain rate is high. At the same time, the system temperature is relatively excellent, so that a large number of hydrothermal reactions occur in the system, the degree of hydrothermal reaction is high, and the building blocks have high strength. However, when the weight of the calcium solid waste exceeds the preferred weight range, the initial reaction will be violent, the mineralization reaction will occur on the surface, the external pores of the aerated building blocks will be closed, and carbon dioxide cannot enter the interior, which will reduce the weight gain rate.
[0008] As a preferred embodiment, the preparation raw materials also include water and a foaming agent, and the water-to-solid ratio of the water to the solid material is (0.2-0.8):1.
[0009] As a preferred implementation manner, the mass proportion of calcium compounds in the calcareous solid waste is ≥ 80%, and the calcareous solid waste is selected from one or a combination of carbide slag, waste lime, and waste cement.
[0010] As a preferred embodiment, the foaming agent is selected from one or a combination of aluminum powder, hydrogen peroxide, and animal protein. The foaming agent can react with water or decompose itself to generate gases such as hydrogen, so that the volume of the slurry expands, and the dry density and porosity of the product can be adjusted.
[0011] As a preferred embodiment, the silicoaluminous solid waste is selected from one or a combination of fly ash, recycled aggregate, construction waste, yellow phosphorus slag, fly ash, smelting slag, and red mud.
[0012] As a preferred embodiment, the exothermic agent is selected from lime, waste lime, or a combination of the two. The exothermic agent reacts with the water in the system to release heat, providing certain temperature conditions for the foaming and hardening stages.
[0013] As a preferred embodiment, the hardener is selected from one or a combination of silicate cement, aluminate cement, desulfurized gypsum, anhydrous gypsum cement, industrial gypsum, and building gypsum. The crystalline substances generated by the hardener after hydration in the system are interlaced and aggregated together so that the whole material is condensed and hardened, providing excellent initial strength to ensure the demolding of the test block.
[0014] As a preferred embodiment, the water reducer is selected from one or a combination of carboxymethyl cellulose, naphthalene-based water reducer, polycarboxylic acid, and sodium tripolyphosphate. The water reducer disperses the system particles, improves workability, increases slurry fluidity, reduces water consumption, and can effectively reduce the water-to-solid ratio required during preparation and shorten the subsequent pre-curing time.
[0015] As a preferred embodiment, the added weight of the foaming agent is 1-5 parts, preferably 1-3 parts.
[0016] The second aspect of the present invention provides a method for preparing a high-strength mineralized aerated building block prepared from solid waste, comprising the following steps:
[0017] (1) mixing calcium solid waste, silicon aluminum solid waste, a heating agent, and a hardener to obtain a mixed solid material, adding a water reducing agent to part of the water to dissolve the mixture, and then adding the mixture to the mixed solid material, and sending the mixture into a stirring system to mix evenly to obtain a mixed material 1;
[0018] (2) mixing the foaming agent with the remaining water, stirring until uniformly mixed with the mixture 1 to obtain the mixture 2;
[0019] (3) Injecting the second mixture into the mold, placing it in a sealed curing room and allowing it to stand for 1-4 hours to form a block;
[0020] (4) After the formed blocks are demoulded and cut, they are subjected to a precipitation process to adjust the remaining water-to-solid ratio in the blocks;
[0021] (5) After curing, the blocks are turned over and cut, and then put into the reactor. The reactor door is closed, and the air inlet valve is opened to introduce carbon dioxide gas. When the pressure in the reactor reaches the set value, the ventilation is stopped. The mineralization reaction is carried out for a certain period of time, and the gas is exhausted to normal pressure, and the reactor is opened;
[0022] (6) After the reaction kettle is cooled to 50°C, the material is discharged.
[0023] As a preferred embodiment, the volume filling rate of the reactor in step (5) is 5-60%, preferably, the volume filling rate of the reactor in step (5) is 25-55%.
[0024] During the experiment, the applicant found that when the volume filling rate of the reactor was 25-55%, the aerated blocks had a higher weight gain rate and excellent compressive performance. The possible reasons are: when the volume filling rate of the reactor is low, the mineralization reaction releases less heat, the reactor temperature is low, the mineralization degree is low, the weight gain rate is low, and the system releases less heat. The system temperature is not enough to make the blocks undergo hydrothermal reaction, and the compressive strength is low; when the volume filling rate of the reactor is 25-55%, the system can release more heat, increase the disturbance of carbon dioxide, so that the mineralization degree of the blocks is improved, and the weight gain rate of the products is high. At the same time, the higher temperature causes the system to undergo hydrothermal reaction, and the compressive strength of the blocks is high and the carbon fixation rate is high. However, when the volume filling rate of the reactor exceeds 25-55%, the system temperature rises faster and reaches the temperature required for the hydrothermal reaction too early, so that the degree of hydrothermal reaction is high and the strength of the blocks is improved, but the rapid increase in the hydrothermal reaction leads to a rapid decrease in mineralizable substances, which reduces the degree of mineralization reaction and reduces the carbon fixation rate.
[0025] As a preferred embodiment, the precipitation process in step (4) can be to reduce the moisture by increasing the block temperature through heating, or to reduce the moisture by increasing air convection.
[0026] As a preferred embodiment, the water-to-solid ratio remaining in the building block after the precipitation process in step (4) is (0.1-0.4):1.
[0027] As a preferred embodiment, the water-to-solid ratio remaining in the block after the precipitation process in step (4) is (0.15-0.3):1.
[0028] As a preferred embodiment, the ventilation rate of the carbon dioxide gas in step (5) is 40-100m / s. 3 / min, the absolute pressure of carbon dioxide is 0.1MPa.
[0029] As a preferred embodiment, the ventilation method of carbon dioxide gas in step (5) is: 30 minutes before the reaction, one-third of the gas volume of the reactor is introduced, and carbon dioxide is continued to be introduced during the reaction until the pressure setting value in the reactor is reached.
[0030] As a preferred embodiment, the pressure of the mineralization reaction in step (5) is 0.1-1.2 MPa, and the time of the mineralization reaction is 1-8 hours.
[0031] During the experiment, the applicant found that when the mineralization pressure was 0.1-1.2MPa and the system temperature was 120-160°C, the aerated blocks had a higher weight gain rate and excellent compressive resistance. The possible reasons are speculated to be: when the system is lower than the preferred mineralization pressure, the mineralization reaction fully occurs on the surface of the block, the mineralization product blocks the surface pores, and carbon dioxide cannot enter the interior of the block to continue the mineralization reaction, resulting in a lower product weight gain rate, and at the same time, the lower temperature also results in lower product strength; when within the preferred mineralization pressure range, the higher pressure allows carbon dioxide to enter the interior of the block, the degree of mineralization increases, the system temperature increases, and the degree of hydrothermal reaction increases; but exceeding the preferred mineralization pressure range, the excessively high gas partial pressure causes the system to reach a certain temperature in a shorter time, more calcium-containing compounds undergo hydrothermal reaction, the product strength is higher, but the mineralization reaction is inhibited, and the block weight gain rate is lower.
[0032] As a preferred embodiment, the water-to-solid ratio after pre-curing in step (4) is 0.1-0.3.
[0033] As a preferred embodiment, the pre-curing method in step (4) is to add a ventilation system in the pre-curing room to evaporate the moisture of the test block through the loss of humidity, thereby controlling the residual water-solid ratio of the system.
[0034] The applicant found in the experiment that after pre-curing, the mass ratio of water to solid components was 0.05-0.35:1, and the aerated blocks had a higher weight gain rate and excellent compressive resistance. The possible reasons are: when the water-solid ratio is low, there are more capillary channels inside the blocks, the water cannot be evenly distributed in the pores, and the amount of carbon dioxide dissolved in the water is less, which makes the degree of mineralization reaction lower, resulting in a lower weight gain rate and lower strength of the product; when the preferred water-solid ratio is reached, the capillary channels inside the blocks are more evenly distributed, carbon dioxide enters the blocks and fully undergoes mineralization reaction, resulting in a high weight gain rate of the blocks, and at the same time, the system temperature is increased, and the good temperature conditions make the blocks undergo hydrothermal reaction, and the strength of the blocks is further improved, and the strength of the blocks is high. When the preferred water-solid ratio is exceeded, there are fewer capillary channels inside the blocks, the channels for carbon dioxide diffusion are blocked, carbon dioxide cannot enter the blocks, the degree of mineralization is low, the system temperature rises slowly, the degree of hydrothermal reaction decreases, and the strength and carbon fixation rate of the blocks are low.
[0035] As a preferred embodiment, the carbon dioxide in step 5 is chemical waste gas, wherein the volume fraction of carbon dioxide is 5%-95%, and the chemical waste gas is selected from one or a combination of flue gas emitted from a coal chemical plant, flue gas from a coal-fired power plant, flue gas from a lime kiln, flue gas from a steel plant, flue gas from a chemical plant, flue gas from a cement plant, and gas after carbon capture and analysis.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) The high-strength mineralized aerated building blocks prepared from solid wastes described in the present invention use calcium solid waste and silicon-aluminum solid waste as main raw materials, and add water to form building blocks. The heat released during the mineralization reaction of the building blocks in contact with carbon dioxide-containing gas increases the temperature of the system. By regulating the building block formula and the mineralization process, the system can reach a temperature that can evaporate the water in the building blocks into water vapor without an external heat source, so that the building blocks can undergo a hydrothermal reaction without the addition of external water vapor, thereby improving the strength of the aerated building blocks, thereby obtaining light-weight and high-strength mineralized aerated building blocks with as low energy consumption as possible.
[0038] (2) The high-strength mineralized aerated building blocks prepared from solid waste described in the present invention improve the mineralization efficiency by introducing a foaming agent and a heat-generating agent to cooperate with the calcium solid waste and the silicon-aluminum solid waste, and adjusting the control system temperature, so that the system temperature rises rapidly to cause a hydrothermal reaction, thereby improving the strength of the product, shortening the production time, and improving the product performance, further reducing the cost of raw materials, and reducing process energy consumption.
[0039] (3) The high-strength mineralized aerated building blocks prepared from solid waste described in the present invention use bulk solid waste as raw materials and utilize mixed waste gas containing carbon dioxide for direct mineralization and maintenance, thereby reducing the use of high-carbon raw materials and effectively realizing efficient resource utilization of solid waste. This solves the problems of solid waste disposal and carbon emission in enterprises and plays an important role in promoting the development of low-mineralization aerated building blocks in my country. DETAILED DESCRIPTION
[0040] Raw material composition: The moisture content of carbide slag from chemical enterprises is 2%. Through XRF analysis, its chemical composition and weight percentage are shown in Table 1:
[0041] Table 1
[0042] Elemental composition CaO <![CDATA[SiO2]]> <![CDATA[P2O5]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> <![CDATA[K2O]]> <![CDATA[SO3]]> <![CDATA[Na2O]]> LOSS content / % 89.2 4.28 2.17 1.34 0.45 0.37 0.15 0.1 1.94
[0043] The moisture content of fly ash from chemical enterprises is 1.2%. Through XRF analysis, its chemical composition and weight percentage are shown in Table 2:
[0044] Table 2
[0045]
[0046] The chemical composition and weight percentage of cement produced by the building materials factory are shown in Table 3 through XRF analysis:
[0047] Table 3
[0048]
[0049] The quicklime produced by the building materials factory was analyzed by XRF. Its chemical composition and weight percentage are shown in Table 4:
[0050] Table 4
[0051] Elemental composition CaO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> Fe2O3 MgO <![CDATA[SO3]]> LOSS content / % 96.02 1.81 0.51 0.15 0.77 0.07 0.32
[0052] The gas composition and volume percentage of tail gas from coal chemical plants are shown in Table 5:
[0053] Table 5
[0054] Gas composition <![CDATA[CO2]]> <![CDATA[N2]]> LOSS Steel exhaust 73.2% 26.1% 0.6%
[0055] Example 1
[0056] A high-strength mineralized aerated building block prepared from solid waste, wherein the preparation raw materials include at least solid materials, and the solid materials include, by weight, 52.08 parts of calcareous solid waste, 77.92 parts of silicoaluminate solid waste, 30 parts of heating agent, 40 parts of hardener, 0.2 parts of water reducing agent, and 2 parts of foaming agent.
[0057] The calcareous solid waste is carbide slag; the silicoaluminous solid waste is fly ash; the exothermic agent is lime; the hardener is cement and gypsum in a weight ratio of 3:1; the water reducer is a common commercially available polycarboxylic acid water reducer; and the foaming agent is aluminum powder.
[0058] A method for preparing a high-strength mineralized aerated building block prepared from solid waste, comprising the following steps:
[0059] (1) mixing calcium solid waste, silicon-aluminum solid waste, a heating agent, and a hardener to obtain a mixed solid material, adding a water reducing agent to two-thirds of water to dissolve the mixed solid material, and then adding the mixed solid material to a stirring system to mix evenly to obtain a mixed material 1;
[0060] (2) mixing the foaming agent with the remaining water, stirring until uniformly mixed with the mixture 1 to obtain the mixture 2;
[0061] (3) Mixture 2 was injected into a mold of 4.2 m × 1.2 m × 0.6 m, and placed in a sealed curing room for 2 h to obtain a block;
[0062] (4) After the formed blocks are demoulded and cut, they are placed in front of the kettle and allowed to stand, and the convection of air is increased by a fan to adjust the residual water-to-solid ratio in the blocks to 0.2:1;
[0063] (5) The pre-cured blocks are placed in a reactor with a volume filling rate of 5%. A total of 5.36 tons of blocks are filled in the reactor. The reactor door is closed and the carbon dioxide inlet valve is opened. When the pressure in the reactor reaches the set value, ventilation is stopped. Mineralization is performed for a certain period of time, and the air is exhausted to normal pressure. The reactor is then opened.
[0064] (6) After the reaction kettle is cooled to 50°C, the material is discharged.
[0065] The water-to-solid ratio of water to solid material in step (1) is 0.5:1.
[0066] The ventilation rate of carbon dioxide gas in step (5) is 60m 3 / min, the absolute pressure of carbon dioxide is 0.1MPa; the ventilation method of carbon dioxide gas is: 30 minutes before the reaction, one-third of the gas volume of the reactor is introduced, and carbon dioxide is continued to be introduced during the reaction until the pressure setting value in the reactor is reached.
[0067] The pressure of the mineralization reaction in step (5) is 0.3 MPa, and the time of the mineralization reaction is 4 hours.
[0068] The carbon dioxide in step (5) is chemical waste gas, wherein the volume fraction of carbon dioxide is 73.2%.
[0069] The initial temperature of the mineralization reaction in step (5) is room temperature 25°C, and the temperature of the system after the reaction is 64.88°C.
[0070] Example 2
[0071] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, wherein the specific steps are the same as those in Example 1, except that the volume filling rate of the reactor is 15%, and a total of 16.09 tons of building blocks are filled, and the initial temperature of the mineralization reaction in step (5) is room temperature 25°C, and the temperature of the system after the reaction is 105.48°C.
[0072] Example 3
[0073] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, wherein the specific steps are the same as those in Example 1, except that the volume filling rate of the reactor is 25%, and a total of 26.81 tons of building blocks are filled, the initial temperature of the mineralization reaction in step (5) is room temperature 25°C, and the temperature of the system after the reaction is 120.8°C.
[0074] Example 4
[0075] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, the specific steps are the same as those in Example 1, the difference is that the volume filling rate of the reactor is 35%, and a total of 37.54t of building blocks are filled, the initial temperature of the mineralization reaction in step 5 is room temperature 25°C, and the temperature of the system after the reaction is 128.35°C.
[0076] Example 5
[0077] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, the specific steps are the same as those in Example 1, the difference is that the volume filling rate of the reactor is 45%, and a total of 48.26 tons of building blocks are filled, the initial temperature of the mineralization reaction in step 5 is room temperature 25°C, and the temperature of the system after the reaction is 137.72°C.
[0078] Example 6
[0079] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, the specific steps are the same as those in Example 1, the difference is that the volume filling rate of the reactor is 48%, and a total of 51.48 tons of building blocks are filled, the initial temperature of the mineralization reaction in step 5 is room temperature 25°C, and the temperature of the system after the reaction is 140.72°C.
[0080] Example 7
[0081] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, the specific steps are the same as those in Example 1, the difference is that the volume filling rate of the reactor is 54%, and a total of 57.92t of building blocks are filled, the initial temperature of the mineralization reaction in step 5 is room temperature 25°C, and the temperature of the system after the reaction is 151.46°C.
[0082] Example 8
[0083] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, the specific steps are the same as those in Example 1, the difference being that the volume filling rate of the reactor is 60%, and a total of 64.35 tons of building blocks are filled, the initial temperature of the mineralization reaction in step 5 is room temperature 25°C, and the temperature of the system after the reaction is 161.74°C.
[0084] Example 9
[0085] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, wherein the specific steps are the same as those of Example 6, except that 24.80 parts by weight of calcareous solid waste and 105.2 parts by weight of silicoaluminate solid waste are used, and the amounts of the remaining substances are the same as those of Example 1. In the step (5), the initial temperature of the mineralization reaction is room temperature 25°C, and the temperature of the system after the reaction is 82.03°C.
[0086] Example 10
[0087] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, wherein the specific steps are the same as those of Example 6, except that 34.72 parts by weight of calcareous solid waste and 95.28 parts by weight of silicoaluminate solid waste are used, and the amounts of the remaining substances are the same as those of Example 1. In the step (5), the initial temperature of the mineralization reaction is room temperature 25°C, and the temperature of the system after the reaction is 104.52°C.
[0088] Embodiment 11
[0089] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, wherein the specific steps are the same as those of Example 6, except that 42.16 parts by weight of calcareous solid waste and 87.84 parts by weight of silicoaluminate solid waste are used, and the amounts of the remaining substances are the same as those of Example 1. In the step (5), the initial temperature of the mineralization reaction is room temperature 25°C, and the temperature of the system after the reaction is 121.06°C.
[0090] Example 12
[0091] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, wherein the specific steps are the same as those of Example 6, except that 60.76 parts by weight of calcareous solid waste and 69.24 parts by weight of silicoaluminate solid waste are used, and the amounts of the remaining substances are the same as those of Example 1. In the step (5), the initial temperature of the mineralization reaction is room temperature 25°C, and the temperature of the system after the reaction is 157.29°C.
[0092] Embodiment 13
[0093] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, wherein the specific steps are the same as those of Example 6, except that 79.36 parts by weight of calcareous solid waste and 50.64 parts by weight of silicoaluminate solid waste are used, and the amounts of the remaining substances are the same as those of Example 1. In the step (5), the initial temperature of the mineralization reaction is room temperature 25°C, and the temperature of the system after the reaction is 199.97°C.
[0094] Embodiment 14
[0095] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, wherein the specific steps are the same as those of Example 6, except that the pressure of the mineralization reaction in step (5) is 0.2 MPa, the initial temperature of the mineralization reaction in step 5 is room temperature 25°C, and the temperature of the system after the reaction is 127.32°C.
[0096] Embodiment 15
[0097] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, wherein the specific steps are the same as those of Example 6, except that the pressure of the mineralization reaction in step (5) is 0.6 MPa, the initial temperature of the mineralization reaction in step 5 is room temperature 25°C, and the temperature of the system after the reaction is 156.49°C.
[0098] Example 16
[0099] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, wherein the specific steps are the same as those of Example 6, except that in step (4), the residual water-solid ratio in the building block is regulated to be 0.1:1, the initial temperature of the mineralization reaction in step 5 is room temperature 25°C, and the temperature of the system after the reaction is 167.16°C.
[0100] Embodiment 17
[0101] A high-strength mineralized aerated building block prepared from solid waste and a preparation method thereof, wherein the specific steps are the same as those of Example 6, except that in step (4), the residual water-solid ratio in the building block is regulated to be 0.35:1, the initial temperature of the mineralization reaction in step 5 is room temperature 25°C, and the temperature of the system after the reaction is 125.45°C.
[0102] Performance Testing
[0103] 1. Carbon fixation rate / weight gain rate test:
[0104] 1) Take 1 / 4 of the volume of the finished bricks prepared in Example 1-17, crush them all into powder, and test the carbon fixation rate of the test block;
[0105] 2) Use a crusher to crush the sample for the carbon fixation rate test of the test block. After crushing, take 50g of the sample and dry it in a 105℃ oven for 12h. Do not evacuate during drying. Keep the oven airtight and place NaOH particles in the oven. After drying, take out 5g of the sample, grind it in a mortar until there is no particle feeling, and put it in a small ziplock bag.
[0106] 3) Place the prepared sample in the sample chamber, set the experimental atmosphere to N2, the temperature range to room temperature to 1000°C, and the heating rate to 10°C / min. Use the TGA2 thermogravimetric analyzer manufactured by the American company (METTLER TOLEDO) for testing and analysis;
[0107] 4) After the test, the TG / DTG thermogravimetric analysis curve is obtained. Note: The present invention uses the CO2 absorption rate to evaluate the carbon absorption effect of the sample, which is the percentage of the mass of CO2 absorbed by the solid waste to the mass of the test block. The content of CO2 absorbed by the solid waste is obtained by testing the TG / DTG thermogravimetric analysis curve of the mineralized product. The content of carbon dioxide absorbed by the mineralized product is the mass increase at 605-820℃, and the mass of the test block is the mass of the mineralized product at 105℃. Weight gain rate = m (矿化反应后) -m (矿化反应前) / m (矿化反应前) ×100%.
[0108] 2. Compressive strength test: Measured in accordance with GB / T 11969-2020 "Test method for autoclaved aerated blocks", the strength of the test block is measured after natural air drying for 24 hours.
[0109] 1. Test steps
[0110] 1. Check the appearance of the test block, measure the length and width of the connecting surface or the pressure surface of each test piece, take the average value, accurate to 0.1mm, and calculate the pressure area A.
[0111] 2. Place the specimen at the center of the lower pressure plate of the material testing machine. The pressure direction of the specimen should be perpendicular to the gas emission direction of the product.
[0112] 3. Start the testing machine. When the upper pressure plate is close to the test piece, adjust the ball seat to make the contact balanced.
[0113] 4. Apply load continuously and evenly at a rate of (2.0±0.5) kN / s until the specimen fails and record the failure load F.
[0114] 2. Calculation of test results
[0115] 1. Calculate the compressive strength of 10 bricks according to the following formula, accurate to 0.1MPa.
[0116] f_cc=F / A
[0117] Where f- cc —compressive strength (MPa);
[0118] F—maximum failure load (N);
[0119] A—Length of the pressure surface (connection surface) (mm);
[0120] Calculate the average compressive strength of three to five test blocks. If the difference between the measured values and their average value is no more than 15%, use the average value as the compressive strength; if the difference between a certain value and the average value is greater than 15%, this value should be discarded and the average value should be calculated with the remaining values.
[0121] 3. Dry density: test the dry density of the block, dry density = mass / volume.
[0122] The test results are shown in Table 1.
[0123] Table 1
[0124]
[0125]
[0126] It can be seen from Examples 1-8 that when the block formula is the same and the filling rate is different, the compressive strength and weight gain rate of the prepared aerated blocks are changed. Among them, since the filling rate of Example 1 is only 5%, the weight gain rate and compressive strength are both low, 4.75% and 1.7MPa respectively. As the filling rate increases, the weight gain of the test block first increases and then decreases, and the compressive strength gradually increases. This is because when the block filling rate in the reactor is low, the heat released by the mineralization reaction is less, the temperature of the reactor is low, the disturbance effect on the carbon dioxide-containing gas is not obvious, the degree of mineralization is low, and the weight gain rate is low; on the other hand, the system releases less heat and the system temperature is not enough to cause the test block to undergo a hydrothermal reaction, so the compressive strength is low. With the increase of the filling rate, when the system filling rate reaches a certain level, the system releases more heat, increases the disturbance of carbon dioxide, increases the degree of mineralization of the test block, and the weight gain rate of the product is high. At the same time, the higher temperature causes the system to undergo a hydrothermal reaction, and the compressive strength of the test block is high and the carbon fixation rate is high. As the filling rate continues to increase, the excessively high filling rate causes the system temperature to rise rapidly, reaching the hydrothermal temperature prematurely, resulting in a high degree of hydrothermal reaction and increased specimen strength, while the degree of mineralization reaction decreases, the carbon fixation rate decreases, and the specimen strength is high but the carbon fixation rate is low.
[0127] It can be seen from Example 6 and Examples 9-13 that an appropriate calcium content helps to obtain higher compressive strength and weight gain rate. The weight gain of the test block first increases and then decreases, and the compressive strength gradually increases. In Examples 6, 14, and 15, as the gas partial pressure increases, the weight gain of the test block first increases and then decreases, and the compressive strength is significantly improved. In Examples 6, 16, and 17, as the water-solid ratio increases after curing, the weight gain of the test block first increases and then decreases, and the compressive strength gradually decreases. Among them, the weight gain rate of Example 6 and Examples 11-12 reaches 7.32-11.32%, and the compressive strength reaches 2.9-4.2MPa, and the carbon fixation effect and block strength are both excellent. When the calcium solid waste content in Examples 9-10 is low, the weight gain rate is only 4.89-5.72%, and the compressive strength is only 1.9-2.0MPa; when the calcium solid waste content in Example 13 is high, although the compressive strength reaches 5.0MPa, the weight gain rate is only 3.87%, and the carbon fixation effect is significantly reduced. This shows that only by controlling the content of calcium solid waste within an appropriate range can both the carbon fixation effect and the strength of the blocks be ensured. This is because the increase in calcium content increases the probability of contact with carbon dioxide, which in turn increases the degree of mineralization reaction, increases the weight gain rate, and at the same time improves the strength to a certain extent; with the increase in calcium content, when the calcium content reaches a certain value, the system releases heat significantly, the test block has high mineralization efficiency and high weight gain rate, and at the same time, the excellent system temperature causes a large number of hydrothermal reactions in the system, the degree of hydrothermal reaction is high, and the strength of the test block is high; when the calcium content is too high, the initial reaction is violent, and the mineralization reaction occurs on the surface, which closes the external pores of the product, and carbon dioxide cannot enter the interior, which reduces the weight gain rate, and when the temperature rises to a certain level, there are more hydration products, which improves the strength of the product.
[0128] From Example 6, Example 14-15, it can be seen that when the pressure of Example 14 during the mineralization reaction dropped to 0.2MPa, the compressive strength of the prepared aerated block dropped from 3.7MPa in Example 6 to 2.9MPa, and the carbon fixation rate dropped from 11.32% in Example 6 to 7.83%. This is because at low mineralization pressure, the surface of the test block fully undergoes mineralization reaction, and the mineralization product blocks the surface pores. Even after the pressure rises, carbon dioxide cannot enter the interior of the test block to continue the mineralization reaction, resulting in a low product weight gain rate, and at the same time, the low temperature also makes the product strength low. When the pressure of Example 15 during the mineralization reaction rises to 0.6MPa, although the compressive strength of the prepared aerated block rises from 3.7MPa in Example 6 to 4.3MPa, the carbon fixation rate drops from 11.32% in Example 6 to 7.62%. This is because as the gas partial pressure increases, the greater pressure allows carbon dioxide to enter the interior of the test block, thereby increasing the degree of mineralization. At the same time, the system temperature rises, which increases the degree of hydration. However, excessively high gas partial pressure causes the system to reach a certain temperature in a shorter period of time, causing more calcium-containing compounds to undergo hydration reactions, resulting in higher product strength. However, the mineralization reaction is suppressed, and the weight gain rate of the test block is lower.
[0129] It can be seen from Example 6 and Examples 16-17 that when the water-solid ratio after pre-curing in Example 16 is 0.1:1, the compressive strength of the prepared aerated block decreases from 3.7MPa in Example 6 to 3.1MPa, and the weight gain rate decreases from 11.32% in Example 13 to 5.30%. This is because at a low water-solid ratio, the water distribution inside the test block is less, and the solubility of carbon dioxide is lower, resulting in a lower degree of mineralization reaction and a lower weight gain rate of the test block. At the same time, the low degree of mineralization makes the system temperature insufficient to support the full progress of the hydrothermal reaction, and the test block strength is lower. When the water-solid ratio after pre-curing in Example 17 is 0.35:1, the compressive strength of the prepared aerated block decreases from 3.7 MPa in Example 13 to 2.8 MPa, and the weight gain rate also decreases from 11.32% in Example 13 to 2.71%. This is because the higher moisture content occupies the internal channels of the block, so that carbon dioxide can only undergo mineralization reaction on the surface, the degree of mineralization reaction is low, the temperature rise of the system is limited, and the degree of hydrothermal reaction is low, thereby reducing the weight gain rate and compressive strength of the block.
Claims
1. A high-strength mineralized aerated building block prepared from solid waste, characterized in that: The mineralized aerated building blocks are made of calcium solid waste, silicon-aluminum solid waste and a foaming agent as basic materials, and water is added to form the building blocks; the building blocks are in contact with carbon dioxide-containing gas to undergo a mineralization reaction, and the heat generated by the mineralization reaction is controlled by adjusting the building block formula and the mineralization process, so that the system reaches the environment and temperature required for the hydrothermal reaction without an external heat source and water vapor, thereby improving the strength of the mineralized aerated building blocks; The method for preparing the high-strength mineralized aerated building blocks prepared from solid waste comprises the following steps: (1) mixing calcium solid waste, silicon-aluminum solid waste, a heating agent, and a hardener to obtain a mixed solid material, adding a water reducing agent to part of the water to dissolve the mixture, and then adding the mixture to the mixed solid material, and sending the mixture into a stirring system to mix evenly to obtain a mixed material 1; (2) Mix the foaming agent and the remaining water, stir until uniformly mixed, and then mix with the mixture 1 to obtain the mixture 2; (3) Inject the second mixture into the mold and place it in a sealed curing room for 1-4 hours to obtain a block; (4) After the formed blocks are demoulded and cut, they are subjected to a dewatering process to adjust the remaining water-to-solid ratio in the blocks; (5) The pre-cured blocks are turned over and cut and then put into the reactor. The reactor door is closed and the air inlet valve is opened to introduce carbon dioxide gas. When the pressure in the reactor reaches the set value, the gas is stopped. The mineralization reaction is allowed to proceed for a certain period of time, and then the gas is exhausted to normal pressure and the reactor is opened. (6) After the reaction kettle is cooled to 50°C, the material is discharged; The volume filling rate of the reactor in step (5) is 25-55%; The raw materials for preparing the mineralized aerated building blocks include solid materials, water and foaming agents. The solid materials include 15-80 parts of calcium solid waste, 40-110 parts of silicon-aluminum solid waste, 0-40 parts of heating agent, 1-50 parts of hardener and 0.1-5 parts of water reducing agent by weight. The water-to-solid ratio of water to solid materials in the raw materials is (0.2-0.8):
1. The pressure of the mineralization reaction in step (5) is 0.1-1.2 MPa, and the time of the mineralization reaction is 1-8 hours; After the dewatering process in step (4), the remaining water-to-solid ratio in the block is (0.1-0.4):
1.
2. The high-strength mineralized aerated building block prepared from solid waste according to claim 1, characterized in that: The mass proportion of calcium compounds in the calcareous solid waste is ≥80%, and the calcareous solid waste is selected from one or a combination of carbide slag, waste lime, and waste cement.
3. The high-strength mineralized aerated building block prepared from solid waste according to claim 1, characterized in that: The foaming agent is selected from one or a combination of aluminum powder, hydrogen peroxide, and animal protein.
4. The high-strength mineralized aerated building block prepared from solid waste according to claim 1, characterized in that: The ventilation rate of the carbon dioxide-containing gas in step (5) is 40-100 m / s. 3 / min; the ventilation method of the carbon dioxide-containing gas in step (5) is: 30 minutes before the reaction, one-third of the gas volume of the reactor is introduced, and carbon dioxide is continued to be introduced during the reaction until the pressure setting value in the reactor is reached.
5. The high-strength mineralized aerated building block prepared from solid waste according to claim 1, characterized in that: The carbon dioxide-containing gas in step (5) is chemical waste gas, wherein the volume fraction of carbon dioxide is 5%-95%, and the chemical waste gas is selected from the group consisting of flue gas emitted from coal chemical plants, flue gas from coal-fired power plants, flue gas from lime kilns, flue gas from steel plants, flue gas from chemical plants, flue gas from cement plants, and gas after carbon capture and analysis, or a combination of several of them.