Alkoxymagnesium carrier for olefin polymerization, preparation method, catalyst and application

By using a preparation method involving magnesium powder, mixed alcohols, halogenating agents, and chemically modified nanoparticles, the problem of difficult particle size control of alkoxy magnesium supports in existing technologies has been solved, achieving high catalyst activity and high polymer packing density, making it suitable for various polymerization processes.

CN116023536BActive Publication Date: 2024-11-19CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111245248.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-26
Publication Date
2024-11-19
Estimated Expiration
2041-10-26

AI Technical Summary

Technical Problem

Existing technologies struggle to prepare alkoxy magnesium supports with excellent particle shape, adjustable particle size, and narrow particle size distribution, especially when ensuring yield, leading to poor catalyst performance.

Method used

Using magnesium powder, mixed alcohols, halogenating agents, and chemically modified nanoparticles as raw materials, the particle size and shape of alkoxy magnesium carriers are controlled through a specific preparation method. This includes adding halogenating agents and nanoparticles in an inert solvent, adding magnesium powder after cooling, reacting, filtering, washing, and drying to prepare alkoxy magnesium carriers with excellent hydrogen regulation properties.

Benefits of technology

An alkoxy magnesium support with controllable particle size, uniform particle shape, and narrow particle size distribution was prepared. When used to prepare catalysts, it improved the catalytic activity and polymer packing density, making it suitable for different polymerization processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116023536B_ABST
    Figure CN116023536B_ABST
Patent Text Reader

Abstract

The present invention discloses an alkoxy magnesium carrier for olefin polymerization, a preparation method, a catalyst and application. The carrier is prepared from raw materials including the following components: magnesium powder, mixed alcohol, a halogenating agent and nanoparticles with chemically modified surfaces; the shape of the nanoparticles is quasi-spherical or spherical; the average particle size of the nanoparticles is 10 to 1000 nm; preferably 50 to 600 nm; the nanoparticles are at least one of inorganic nanoparticles or organic nanoparticles, preferably at least one of inorganic silicon, magnesium, aluminum, titanium, zirconium, calcium, iron, arsenic and selenium nanoparticles. The alkoxy magnesium carrier of the present invention has excellent particle shape, controllable particle size, uniform particle shape and narrow particle size distribution; the catalyst prepared by using the carrier of the present invention has high activity, excellent hydrogen regulation performance, narrow particle distribution, controllable size and excellent particle shape, and high polymer bulk density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalysts, and more particularly to an alkoxy magnesium carrier for olefin polymerization, a preparation method, a catalyst and application thereof. Background Art

[0002] The core of polyolefin catalyst research is to control the polymerization activity of the catalyst, the particle morphology and particle size distribution of the polymer generated by the catalyst, the hydrogen adjustment sensitivity of the catalyst, the copolymerization performance of the catalyst, etc. on the basis of matching different production process conditions. Among the numerous polyolefin production processes, taking the production process of polyethylene as an example, the requirements of the slurry polymerization process and the gas phase polymerization process for the catalyst are not only activity and hydrogen adjustment performance, but also certain requirements for the particle size and particle size distribution of the catalyst in order to match the device conditions. Therefore, the research on catalysts with excellent particle shape and adjustable particle size has always been the core and key technology of polyolefin catalyst development.

[0003] Catalysts for olefin polymerization are usually prepared by various methods such as dissolution, loading, and spraying. Among them, catalysts with alkoxymagnesium as the loading source occupy an important position in the field of polyolefin catalysis due to their excellent hydrogen regulation performance and particle morphology. It is well known that in the preparation of polyolefin catalysts, the particle morphology of the catalyst can well replicate the particle morphology of the carrier. Therefore, it can be said that catalysts with excellent performance can be achieved by controlling the carrier used to prepare the catalyst.

[0004] In the prior art, a variety of methods for preparing magnesium alkoxides have been disclosed. Chinese patent CN 101906017A introduces a method for preparing magnesium alkoxides using magnesium powder, mixed alcohol and halogen as raw materials; Chinese patents CN104356257A and CN103044585 etc. introduce a method for preparing polyolefin catalyst carriers using silicon dioxide as a dispersion medium, on which the fluidity of the polyethylene powder obtained is significantly improved, but the content of polymerized fine powder is high and the bulk density is low.

[0005] Although a variety of strategies for preparing alkoxy magnesium particles have been disclosed, the industrial production of alkoxy magnesium with excellent particle shape is still difficult. In many cases, the quality of the carrier needs to be guaranteed at the expense of yield. In particular, the preparation of alkoxy magnesium particles with adjustable particle size is more complicated and difficult. Therefore, the preparation of alkoxy magnesium with excellent particle shape, adjustable particle size, narrow particle size distribution and high bulk density is of great significance. Summary of the invention

[0006] In order to solve the problems in the prior art, the present invention provides an alkoxy magnesium carrier for olefin polymerization, a preparation method, a catalyst and application. The alkoxy magnesium carrier of the present invention has excellent particle shape, controllable particle size, uniform particle shape and narrow particle size distribution; the catalyst prepared by using the carrier of the present invention has high activity, excellent hydrogen regulation performance, narrow particle distribution, controllable size and excellent particle shape, and high polymer bulk density.

[0007] One of the objects of the present invention is to provide an alkoxy magnesium support for olefin polymerization.

[0008] The carrier is prepared from raw materials including the following components:

[0009] Magnesium powder, mixed alcohol, halogenating agent and surface chemically modified nanoparticles;

[0010] The shape of the nanoparticles is spherical or spherical; the average particle size of the nanoparticles is 10 to 1000 nm; preferably 50 to 600 nm;

[0011] The nanoparticles are at least one of inorganic nanoparticles or organic nanoparticles, preferably at least one of inorganic silicon, magnesium, aluminum, titanium, zirconium, calcium, iron, arsenic, and selenium nanoparticles.

[0012] In a preferred embodiment of the present invention,

[0013] The alkoxy magnesium carrier is in granular form, with an average particle size of 1 to 100 μm, preferably 10 to 70 μm;

[0014] The particle size distribution is 0.5 to 1.5, preferably 0.6 to 1.1,

[0015] The bulk density of the alkoxy magnesium carrier particles is 0.2 to 0.7 g / cm 3 , preferably 0.2 to 0.6 g / cm 3 .

[0016] In a preferred embodiment of the present invention,

[0017] The nanoparticles are selected from at least one of silicon dioxide, titanium dioxide, aluminum oxide, zirconium dioxide, magnesium oxide, and calcium oxide, preferably silicon dioxide.

[0018] In a preferred embodiment of the present invention,

[0019] The surface of the nanoparticles chemically modified is a layer of inorganic substances or organosiloxane attached to the surface of the nanoparticles, or the surface of the nanoparticles contains at least one of amino, hydroxyl, phenolic hydroxyl, carboxyl, thiol, nitro, halogen, ester, amide, urea, guanidine, aldehyde, sulfonic acid, and amine groups. Preferably, the surface of the nanoparticles contains at least one of hydroxyl, amino, and phenolic hydroxyl groups.

[0020] In a preferred embodiment of the present invention,

[0021] The mixed alcohol is a linear or branched monohydric alcohol or polyhydric alcohol, preferably a mixture of C1-C10 alcohols; more preferably a mixture of ethanol and isooctyl alcohol, and / or a mixture of ethanol and butanol; more preferably: the molar content of isooctyl alcohol or butanol in the mixed alcohol is 1% to 20%.

[0022] In a preferred embodiment of the present invention,

[0023] The halogenating agent is at least one of a halogen element or an inorganic halide, preferably at least one of chlorine, bromine, iodine, magnesium chloride, manganese chloride, mercuric chloride, calcium chloride, magnesium bromide, manganese bromide, mercuric bromide, calcium bromide, magnesium iodide, manganese iodide, mercuric iodide, and calcium iodide, more preferably at least one of iodine, magnesium iodide, magnesium chloride, and manganese chloride; and / or,

[0024] The average particle size of the magnesium powder is 50 to 300 μm.

[0025] In a preferred embodiment of the present invention,

[0026] Among the raw materials,

[0027] The molar ratio of the halogenating agent to the magnesium powder is (0.0001-0.5):1, preferably (0.002-0.05):1;

[0028] The molar ratio of the mixed alcohol to the magnesium powder is (1-20):1, preferably (2-15):1;

[0029] The weight ratio of the nanoparticles with chemically modified surfaces to the magnesium powder is (0.0001-2):1, preferably (0.0001-1):1.

[0030] The second object of the present invention is to provide a method for preparing an alkoxy magnesium carrier.

[0031] The method comprises:

[0032] 1) Adding a halogenating agent, a mixed alcohol and nanoparticles with chemically modified surfaces into an inert solvent, stirring for 10 to 120 minutes, and then cooling to -15 to 10°C;

[0033] 2) Add magnesium powder and heat to 60-90°C for reaction;

[0034] 3) filtering, washing and drying to obtain the alkoxy magnesium carrier.

[0035] In a preferred embodiment of the present invention,

[0036] In step 1), the inert solvent is selected from at least one of benzene, toluene, xylene, hexane, heptane, octane, decane, white oil, and paraffin, preferably at least one of toluene, hexane, decane, heptane, and white oil;

[0037] The volume ratio of the inert solvent to the mixed alcohol is (0.02-1):1, preferably (0.05-0.3):1.

[0038] The inert atmosphere is a protective gas that does not participate in the reaction, preferably an inert gas or nitrogen, more preferably argon and nitrogen.

[0039] In a preferred embodiment of the present invention,

[0040] Step 2) The reaction time is 1 to 12 hours.

[0041] A third object of the present invention is to provide a Ziegler-Natta catalyst for olefins.

[0042] A reaction product comprising:

[0043] A) the alkoxy magnesium support according to one of the objects of the present invention;

[0044] B) a titanium-containing compound; wherein the general formula of the titanium-containing compound is Ti(OR) n X 4-n , where R is C 1 ~C 8 Hydrocarbon group, X is a halogen atom, 0≤n≤4

[0045] C) Internal electron donor compounds.

[0046] in,

[0047] The titanium-containing compound is selected from TiCl 4 、TiBr 4 、TiI 4 、Ti(OC 2 H 5 )Cl 3 、Ti(OCH 3 )Cl 3 、Ti(OC 4 H 9 )Cl 3 、Ti(OC 2 H5 )Br 3 、Ti(OC 2 H 5 ) 2 Cl 2 、Ti(OCH 3 ) 2 Cl 2 、Ti(OCH 3 ) 2 I 2 、Ti(OC 2 H 5 ) 3 Cl、Ti(OCH 3 ) 3 Cl and Ti(OC 2 H 5 ) 3 At least one of I; and / or,

[0048] The internal electron donor compound is selected from at least one of esters, ethers, phenols, ketones, carboxylic acids, and organosiloxane compounds; preferably at least one of esters, ethers, and organosiloxane compounds; more preferably at least one of methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, hexyl benzoate, succinate, ethyl ether, butyl ether, tetrahydrofuran, tetramethoxysilane, and tetraethoxysilane.

[0049] The method for preparing olefins using a Ziegler-Natta catalyst adopts a conventional method for preparing a Ziegler-Natta catalyst in the prior art.

[0050] In the present invention, it can be preferably prepared according to the following steps:

[0051] The above-mentioned alkoxy magnesium particles are dispersed in a solvent of hexane and toluene, and are contacted with a titanium compound containing titanium and an internal electron donor, respectively, to obtain the Ziegler-Natta catalyst for olefins.

[0052] A fourth object of the present invention is to provide a catalyst for olefin polymerization.

[0053] The catalyst comprises:

[0054] 1) The catalyst according to the third object of the present invention;

[0055] 2) Organic aluminum compounds;

[0056] The general formula of the organoaluminum compound is AlR m X 3-m , where R is hydrogen or C 1 ~C 20 Hydrocarbon group, X is a halogen atom, 0<m≤3.

[0057] The present invention can specifically adopt the following technical solutions:

[0058] A method for preparing an alkoxy magnesium carrier comprises the following steps:

[0059] 1) Under an inert atmosphere, a halogenating agent, a mixed alcohol and nanoparticles with chemically modified surfaces are added to an inert solvent, and then the temperature is lowered to -15 to 10°C;

[0060] 2) Raise the temperature to 60-90°C, during which time magnesium powder is added once or several times for reaction;

[0061] 3) The reaction is maintained for 1 to 12 hours, filtered and washed 2 to 6 times, and the obtained solid is dried to obtain an alkoxy magnesium carrier.

[0062] Among them, the nanoparticles are preferably selected from inorganic nanoparticles, more preferably selected from at least one of silicon dioxide, titanium dioxide, aluminum oxide, zirconium dioxide, magnesium oxide, and calcium oxide; particularly preferably selected from silicon dioxide; the morphology of the nanoparticles is preferably spherical or spherical; the average particle size of the nanoparticles is preferably 10 to 1000 nm, more preferably 50 to 600 nm.

[0063] The surface of the nanoparticles in the present invention needs to be chemically modified. The surface of the chemically modified nanoparticles has one or more functional groups, which helps the nanoparticles to be well dispersed in the solvent. At the same time, the nanoparticles with chemically modified surfaces can act as effective nucleating agents during the growth of alkoxymagnesium, which helps to generate narrow distribution alkoxymagnesium carrier particles and is conducive to the regulation of the particle size of the alkoxymagnesium carrier particles.

[0064] According to an embodiment of the present invention, the mixed alcohol is a linear or straight-chain monohydric alcohol or polyhydric alcohol, preferably a mixture of C1-C10 alcohols, more preferably a mixture of ethanol and isooctyl alcohol, or a mixture of ethanol and butanol. The molar content of isooctyl alcohol or butanol in the mixed alcohol is 1% to 20%.

[0065] According to an embodiment of the present invention, the weight ratio of the nanoparticles to the magnesium powder is preferably (0.0001-1):1; the molar ratio of the halogenating agent to the magnesium powder is preferably (0.002-0.05):1; the molar ratio of the mixed alcohol to the magnesium powder is preferably (2-15):1; the halogenating agent is preferably at least one selected from elemental iodine, magnesium iodide, magnesium chloride, and manganese chloride.

[0066] According to an embodiment of the present invention, the inert solvent is preferably at least one selected from benzene, toluene, xylene, hexane, heptane, octane, decane, white oil, and paraffin, and more preferably at least one selected from toluene, hexane, decane, heptane, and white oil. The inert solvent can act as a solvent to prevent the aggregation of particles, and can also affect the formation mechanism of alkoxy magnesium and regulate the growth of alkoxy magnesium.

[0067] In the preparation of the alkoxy magnesium carrier provided by the present invention, the average particle size of the magnesium powder is 50 to 300 μm; the shape of the magnesium powder is not particularly limited under the condition of good reaction, and is preferably spherical particles.

[0068] In the preparation of the alkoxy magnesium carrier provided by the present invention, magnesium powder can be added all at once or in portions according to the particle size requirements of the alkoxy magnesium particles.

[0069] In the preparation of the alkoxy magnesium carrier provided by the present invention, the halogenating agent and the magnesium powder can be added to the reaction system separately, or in the form of a solution or a slurry.

[0070] In the preparation of the alkoxy magnesium carrier provided by the present invention, the order of adding the reactants and the reaction temperature can be adjusted according to the product requirements; the degree of reaction is determined according to the emission of hydrogen.

[0071] In the preparation of the alkoxy magnesium carrier provided by the present invention, the form, type and stirring rate of the stirring paddle are not limited, and the form, type and stirring rate of the stirring paddle can be adjusted appropriately according to the requirements of the product.

[0072] In the preparation of the alkoxy magnesium carrier provided by the present invention, the reaction product can be washed with ethanol, mixed alcohol, or any organic solvent, and the washing method is not limited.

[0073] The alkoxy magnesium carrier provided by the present invention can be stored in the form of dry powder or in the form of suspended slurry after being dried.

[0074] A Ziegler-Natta catalyst for olefin polymerization, comprising the reaction product of the following components:

[0075] A) the alkoxy magnesium carrier particles;

[0076] B) a titanium-containing compound; wherein the general formula of the titanium-containing compound is Ti(OR) n X 4-n , where R is C 1 ~C 8 Hydrocarbyl, X is a halogen atom, 0≤n≤4; the titanium compound is selected from TiCl 4 、TiBr 4 、TiI 4 、Ti(OC2 H 5 )Cl 3 、Ti(OCH 3 )Cl 3 、Ti(OC 4 H 9 )Cl 3 、Ti(OC 2 H 5 )Br 3 、Ti(OC 2 H 5 ) 2 Cl 2 、Ti(OCH 3 ) 2 Cl 2 、Ti(OCH 3 ) 2 I 2 、Ti(OC 2 H 5 ) 3 Cl、Ti(OCH 3 ) 3 Cl and Ti(OC 2 H 5 ) 3 At least one of I, preferably TiCl 4

[0077] C) Internal electron donor compounds.

[0078] According to an embodiment of the present invention, the internal electron donor compound is selected from at least one of esters, ethers, phenols, ketones, carboxylic acids, and organosiloxane compounds; preferably at least one of esters, ethers, and organosiloxane compounds; more preferably at least one of methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, hexyl benzoate, succinate, ethyl ether, butyl ether, tetrahydrofuran, tetramethoxysilane, and tetraethoxysilane.

[0079] A catalyst for olefin polymerization, comprising:

[0080] 1) the above-mentioned Ziegler-Natta catalyst;

[0081] 2) Organic aluminum compounds;

[0082] The general formula of the organoaluminum compound is AlR m X 3-m , where R is hydrogen or C 1 ~C 20 Hydrocarbyl, X is a halogen atom, 0<m≤3, the organoaluminum compound can be selected from Al(CH 3 ) 3 、Al(CH2 CH 3 ) 3 、Al(i-Bu) 3 、AlH(CH 2 CH 3 ) 2 、AlH(i-Bu) 2 、AlCl(CH 2 CH 3 ) 2 、Al 2 Cl 3 (CH 2 CH 3 ) 3 、AlCl(CH 2 CH 3 ) 2 and AlCl 2 (CH 2 CH 3 ) at least one of.

[0083] Preferably, the organoaluminum compound is selected from Al(CH 2 CH 3 ) 3 and / or Al(i-Bu) 3 .

[0084] The present invention has the following beneficial technical effects:

[0085] 1. The introduction of surface-modified functional nanoparticles is beneficial to improve the particle shape and particle size distribution of the alkoxy magnesium carrier particles; alkoxy magnesium carrier particles with controllable particle size, uniform particle shape and narrow particle size distribution are obtained;

[0086] 2. The alkoxy magnesium carrier particles of the present invention are used to prepare catalysts for olefin polymerization, and the obtained catalysts have high activity, narrow particle distribution, controllable size, excellent particle shape, and high polymer bulk density;

[0087] 3. Catalysts for olefin polymerization of different sizes prepared with alkoxymagnesium carriers are suitable for different polymerization processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0088] Figure 1 is a scanning electron microscope image of inorganic nanoparticles;

[0089] Figure 2 is a scanning electron microscope image of the alkyl magnesium carrier particles of Example 1;

[0090] Figure 3 This is a scanning electron microscope image of the catalyst for olefin polymerization of Example 1:

[0091] Figure 4This is a scanning electron microscope image of the polyethylene powder of Example 6.

[0092] Figure 5 This is a scanning electron microscope image of the alkyl magnesium carrier particles of Comparative Example 1. DETAILED DESCRIPTION

[0093] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.

[0094] In the following examples and comparative examples:

[0095] 1. The content of organic matter in the surface chemically modified nanoparticles (%) = (W1-W0) / W1×100%, where W1 is the weight of W0g of silica after modification.

[0096] 2. Particle size and particle size distribution of alkoxy magnesium carrier and catalyst: Malvern Mastersizer TM2000 laser particle size analyzer was used, wherein Span = (D90-D10) / D50.

[0097] 3. Particle shape of inorganic nanoparticles, alkoxy magnesium carrier and catalyst: A Hitachi S4800 electron scanning microscope was used.

[0098] 4. Bulk density of alkoxy magnesium particles and polymers: measured by the method of loose solid weight per unit volume.

[0099] 5. Preparation method of surface-modified nano-silica: prepare 100 mL of 2 mg / mL dopamine Tris-HCl solution (10 mM, pH 8.5), stir for 1 min, add 1 g (particle size of about 250 nm) of silica microspheres to the above solution, and continue the reaction for 3 h. Filter the clear water, wash with deionized water and ethanol several times, and dry to obtain a brown solid particle powder, in which the modification amount of the polymer is about 5.6%.

[0100] The raw materials used in the remaining embodiments are all commercially available products.

[0101] The present invention will be further described below in conjunction with specific embodiments.

[0102] Example 1

[0103] A reflux condenser was installed in the reactor with a stirrer. A conduit was inserted above the reflux condenser and the other end of the conduit was connected to an oil seal device to facilitate observation of H 2The reactor is fully replaced with high-purity nitrogen.

[0104] (1) Under nitrogen protection, 0.3 g iodine, 120 mL mixed alcohol (ethanol and isooctyl alcohol, ethanol: isooctyl alcohol molar ratio is 2:0.05), 60 mg modified nano-SiO 2 , stirred for 30 min, and then cooled to 0°C;

[0105] (2) Add 6.3 g of magnesium powder, raise the temperature to 75°C, and maintain the reaction at reflux temperature for 4 h;

[0106] (3) Allow to settle, filter the clear water, wash four times with anhydrous ethanol and hexane, separate and dry to obtain a white solid powder (alkoxy magnesium carrier) with good fluidity.

[0107] The particle size and distribution of the product were measured using a particle size distribution instrument. The results are shown in Table 1.

[0108] Embodiment 2-3

[0109] The method is the same as in Example 1, except that: the nano-SiO 2 The amounts were adjusted to 6 mg and 600 mg respectively.

[0110] The particle size and distribution of the product were measured using a particle size distribution instrument. The results are shown in Table 1.

[0111] Embodiment 4-5

[0112] The same method as in Example 1, except that the inorganic nanoparticles are composed of nano-SiO 2 Adjust to titanium dioxide and calcium oxide respectively.

[0113] The particle size and distribution of the product were measured using a particle size distribution instrument. The results are shown in Table 1.

[0114] Example 6

[0115] A reflux condenser was installed in the reactor with a stirrer. A conduit was inserted above the reflux condenser and the other end of the conduit was connected to an oil seal device to facilitate observation of H 2 The reactor is fully replaced with high-purity nitrogen.

[0116] (1) Under nitrogen protection, 0.13 g iodine, 200 mL mixed alcohol (ethanol and isooctyl alcohol, the amount of isooctyl alcohol added is 2 mL), 60 mg modified nano-SiO 2 , stirred for 30 min, and then cooled to -15 °C;

[0117] (2) Add 6.3 g of magnesium powder (particle size 70 μm), heat to 60 °C, and maintain the reflux temperature for 4 h;

[0118] (3) Allow to settle, filter the clear water, wash four times with anhydrous ethanol and hexane, separate and dry to obtain a white solid powder (alkoxy magnesium carrier) with good fluidity.

[0119] The particle size and distribution of the product were measured using a particle size distribution instrument. The results are shown in Table 1.

[0120] Example 7

[0121] A reflux condenser was installed in the reactor with a stirrer. A conduit was inserted above the reflux condenser and the other end of the conduit was connected to an oil seal device to facilitate observation of H 2 The reactor is fully replaced with high-purity nitrogen.

[0122] (1) Under nitrogen protection, 0.66 g iodine, 50 mL mixed alcohol (ethanol and isooctyl alcohol, the amount of isooctyl alcohol added is 10 mL), and 60 mg modified nano-SiO 2 , stirred for 90 min, and then cooled to 10 °C;

[0123] (2) Add 6.3 g of magnesium powder (particle size is 300 μm), raise the temperature to 90° C., and maintain the reaction at reflux temperature for 8 h;

[0124] (3) Allow to settle, filter the clear water, wash four times with anhydrous ethanol and hexane, separate and dry to obtain a white solid powder (alkoxy magnesium carrier) with good fluidity.

[0125] The particle size and distribution of the product were measured using a particle size distribution instrument. The results are shown in Table 1.

[0126] Comparative Example 1

[0127] A reflux condenser was installed in the reactor with a stirrer. A conduit was inserted above the reflux condenser and the other end of the conduit was connected to an oil seal device to facilitate observation of H 2 The reactor is fully replaced with high-purity nitrogen.

[0128] (1) Under nitrogen protection, add 0.3 g iodine, 120 mL mixed alcohol, and 30 mL toluene, stir for 30 min, and then cool to 0°C;

[0129] (2) Add 6.3 g of magnesium powder, raise the temperature to 75°C, and maintain the reaction at reflux temperature for 4 h;

[0130] (3) Allow to settle, filter the clear liquid, wash it four times with anhydrous ethanol and hexane, separate and dry it to obtain a white solid powder.

[0131] The particle size and distribution of the product were measured using the same method as in Example 1. The results are shown in Table 1.

[0132] Comparative Example 2

[0133] A reflux condenser was installed in the reactor with a stirrer. A conduit was inserted above the reflux condenser and the other end of the conduit was connected to an oil seal device to facilitate observation of H 2 The reactor is fully replaced with high-purity nitrogen.

[0134] (1) Under nitrogen protection, add 0.3 g iodine, 120 mL mixed alcohol, 30 mL toluene, 60 mg unmodified nano-SiO 2 , then cool down to 0℃;

[0135] (2) Add 6.3 g of magnesium powder, raise the temperature to 75°C, and maintain the reaction at reflux temperature for 4 h;

[0136] (3) Allow to settle, filter the clear liquid, wash it four times with anhydrous ethanol and hexane, separate and dry it to obtain a white solid powder.

[0137] The particle size and distribution of the product were measured using the same method as in Example 1. The results are shown in Table 1.

[0138] Example 8

[0139] In a 300 mL nitrogen-purified 5-mouth stirred reactor, 4 g of the diethoxy magnesium support prepared in Example 1 and 40 mL of toluene were added, the temperature was lowered to -15 °C, and 20 mL of TiCl was slowly added dropwise under stirring. 4 , it takes 1 hour; heat to 100℃, keep constant temperature for 2 hours, let it stand and settle, decant the supernatant, and add 30mL of TiCl 4 and 3 mL of tetraethoxysilane, keep the temperature constant for 1 hour, let it stand and settle, filter the clear water, wash it with 100 mL of hexane at 60°C for several times and then dry it to obtain a solid catalyst with good fluidity.

[0140] A 2L stainless steel reactor was fully replaced with high-purity nitrogen, and then 1L of hexane and 1.0mL of 1M triethylaluminum were added, and then the solid catalyst component prepared by the above method (containing 0.6mg of titanium) was added. The temperature was raised to 70°C, hydrogen was introduced to make the pressure in the reactor reach 0.28MPa, and ethylene was introduced to make the total pressure in the reactor reach 0.73MPa, and polymerization was carried out at 80°C for 2 hours.

[0141] The polymer properties were evaluated using a particle size distribution analyzer and polymerization characterization, and the results are shown in Table 2.

[0142] Examples 9-10, Comparative Example 3

[0143] The method is the same as that of Example 6, except that the alkoxy magnesium used is from Examples 2-3 and Comparative Example 1, respectively.

[0144] The polymer properties were evaluated using a particle size distribution analyzer and polymerization characterization, and the results are shown in Table 2.

[0145] Table 1

[0146] serial number Nanoparticles Mg / % D50 / μm Span <![CDATA[BD / g / cm 3 ]]> Example 1 <![CDATA[SiO 2 ]]> 21.34 35.88 0.70 0.37 Example 2 <![CDATA[SiO 2 ]]> 21.14 60.32 0.82 0.32 Example 3 <![CDATA[SiO 2 ]]> 21.32 10.23 0.69 0.56 Example 4 <![CDATA[TiO 2 ]]> 21.16 38.78 0.88 0.36 Example 5 CaO 21.33 38.93 0.98 0.35 Example 6 <![CDATA[SiO 2 ]]> 22.03 33.71 1.10 0.31 Example 7 <![CDATA[SiO 2 ]]> 21.26 41.20 1.07 0.29 Comparative Example 1 none 21.12 45.46 1.40 0.27 Comparative Example 2 <![CDATA[Ordinary SiO 2 > 21.29 43.76 1.46 0.28

[0147] Table 2

[0148] serial number D50 / μm Span Ac / KgPE / gCat <![CDATA[BD / g / cm 3 ]]> <![CDATA[MI 2.16 / g / 10min]]> Example 8 35.21 0.69 33 0.33 2.01 Example 9 59.96 0.82 31 0.29 1.92 Example 10 10.15 0.70 36 0.38 2.15 Comparative Example 3 44.32 1.02 28 0.24 1.89

[0149] As can be seen from Tables 1 to 2 and the scanned photos, compared with the comparative example, the introduction of chemically modified nanoparticles in the embodiment of the present invention can effectively control the particle size of the alkoxymagnesium particles, the particle size distribution of the particles is narrow, and the bulk density of the alkoxymagnesium particles is slightly higher; the olefin polymerization catalyst prepared using this as a carrier has high activity, narrow particle distribution, controllable size and excellent particle shape, and the polymer obtained by polymerization has a high bulk density. Therefore, the introduction of modified nanoparticles is conducive to improving the comprehensive performance of the alkoxymagnesium particles and their catalysts.

[0150] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. An alkoxy magnesium carrier for olefin polymerization, characterized in that: The carrier is prepared from raw materials including the following components: Magnesium powder, mixed alcohol, halogenating agent and surface chemically modified nanoparticles; The shape of the nanoparticles is quasi-spherical or spherical; the average particle size of the nanoparticles is 10 to 1000 nm; The nanoparticles are selected from at least one of silicon dioxide, titanium dioxide, aluminum oxide, zirconium dioxide, magnesium oxide, and calcium oxide; The surface of the nanoparticles chemically modified is a layer of inorganic substances or organic siloxane attached to the surface of the nanoparticles, or the surface of the nanoparticles contains at least one of hydroxyl, amino, carboxyl, thiol, aldehyde, amide, guanidine, sulfonic acid, and halogen atoms; The bulk density of the alkoxy magnesium carrier particles is 0.2 to 0.7 g / cm 3 ; The mixed alcohol is a mixture of ethanol and isooctyl alcohol.

2. The alkoxy magnesium support for olefin polymerization according to claim 1, characterized in that: The average particle size of the nanoparticles is 50-600 nm.

3. The alkoxy magnesium support for olefin polymerization according to claim 1, characterized in that: The alkoxy magnesium carrier is in granular form with an average particle size of 1 to 100 μm; The particle size distribution of the alkoxy magnesium carrier is 0.5 to 1.5; The bulk density of the alkoxy magnesium carrier particles is 0.2 to 0.6 g / cm 3 .

4. The alkoxy magnesium support for olefin polymerization according to claim 3, characterized in that: The alkoxy magnesium carrier is in granular form with an average particle size of 10 to 70 μm; The particle size distribution of the alkoxy magnesium carrier is 0.6-1.

1.

5. The alkoxy magnesium support for olefin polymerization according to claim 1, characterized in that: The nanoparticles are silicon dioxide.

6. The alkoxy magnesium support for olefin polymerization according to claim 1, characterized in that: The halogenating agent is at least one of a halogen element or an inorganic halide; and / or, The average particle size of the magnesium powder is 50 to 300 μm.

7. The alkoxy magnesium support for olefin polymerization according to claim 6, characterized in that: The halogenating agent is selected from at least one of chlorine, bromine, iodine, magnesium chloride, manganese chloride, mercuric chloride, calcium chloride, magnesium bromide, manganese bromide, mercuric bromide, calcium bromide, magnesium iodide, manganese iodide, mercuric iodide, and calcium iodide.

8. The alkoxy magnesium support for olefin polymerization according to claim 7, characterized in that: The halogenating agent is selected from at least one of iodine, magnesium iodide, magnesium chloride and manganese chloride.

9. The alkoxy magnesium support for olefin polymerization according to claim 1, characterized in that: Among the raw materials, The molar ratio of the halogenating agent to the magnesium powder is (0.0001-0.5):1; The molar ratio of the mixed alcohol to the magnesium powder is (1-20):1; The weight ratio of the nanoparticles with chemically modified surfaces to the magnesium powder is (0.0001-2):

1.

10. The alkoxy magnesium support for olefin polymerization according to claim 9, characterized in that: Among the raw materials, The molar ratio of the halogenating agent to the magnesium powder is (0.002-0.05):1; The molar ratio of the mixed alcohol to the magnesium powder is (2-15):1; The weight ratio of the nanoparticles with chemically modified surfaces to the magnesium powder is (0.0001-1):

1.

11. A method for preparing an alkoxy magnesium carrier according to any one of claims 1 to 10, characterized in that The method comprises: 1) Under the protection of an inert atmosphere, a halogenating agent, a mixed alcohol and nanoparticles with chemically modified surfaces are added to an inert solvent, stirred for 10 to 120 minutes, and then cooled to -15 to 10°C; 2) Add magnesium powder and heat to 60-90°C for reaction; 3) filtering, washing and drying to obtain the alkoxy magnesium carrier.

12. The preparation method according to claim 11, characterized in that: In step 1), the inert solvent is selected from at least one of benzene, toluene, xylene, hexane, heptane, octane, decane, white oil, and paraffin; The volume ratio of the inert solvent to the mixed alcohol is (0.02-1):

1.

13. The preparation method according to claim 12, characterized in that: In step 1), the inert solvent is selected from at least one of toluene, hexane, decane, heptane and white oil; The volume ratio of the inert solvent to the mixed alcohol is (0.05-0.3):

1.

14. The preparation method according to claim 11, characterized in that: Step 2) The reaction time is 1 to 12 hours.

15. A Ziegler-Natta catalyst for olefin polymerization, characterized in that: A reaction product comprising: A) the alkoxy magnesium support according to any one of claims 1 to 10; B) a titanium-containing compound; wherein the general formula of the titanium-containing compound is Ti(OR) n X 4-n , wherein R is a C1-C8 hydrocarbon group, X is a halogen atom, 0≤n≤4; C) Internal electron donor compounds.

16. The Ziegler-Natta catalyst according to claim 15, characterized in that: The titanium-containing compound is selected from at least one of TiCl4, TiBr4, TiI4, Ti(OC2H5)Cl3, Ti(OCH3)Cl3, Ti(OC4H9)Cl3, Ti(OC2H5)Br3, Ti(OC2H5)2Cl2, Ti(OCH3)2Cl2, Ti(OCH3)2I2, Ti(OC2H5)3Cl, Ti(OCH3)3Cl and Ti(OC2H5)3I; and / or, The internal electron donor compound is selected from at least one of esters, ethers, phenols, ketones, carboxylic acids, and organosiloxane compounds.

17. The Ziegler-Natta catalyst according to claim 16, characterized in that: The internal electron donor compound is selected from at least one of esters, ethers and organosiloxane compounds.

18. The Ziegler-Natta catalyst according to claim 17, characterized in that: The internal electron donor compound is selected from at least one of methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, hexyl benzoate, succinate, ethyl ether, butyl ether, tetrahydrofuran, tetramethoxysilane, and tetraethoxysilane.

19. A catalyst for olefin polymerization, characterized in that The catalyst comprises: 1) The catalyst according to any one of claims 15 to 18; 2) Organic aluminum compounds; The general formula of the organoaluminum compound is AlR m X 3-m , where R is hydrogen or C1~C 20 Hydrocarbon group, X is a halogen atom, 0<m≤3.