Polyurethane foam containing interpenetrating network structure and preparation method and application thereof

By forming an interpenetrating cross-linked network structure in the polyurethane foam, it solves the existing polyurethane buffer's insufficient resistance to moisture and heat aging and impact resistance, achieves high mechanical strength and good impact energy absorption, and satisfies the requirements at the bottom of the elevator shaft. Buffer application requirements.

CN116023616BActive Publication Date: 2024-10-29SHANGHAI YOUYUE NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202310079293.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-08
Publication Date
2024-10-29
Estimated Expiration
2043-02-08

AI Technical Summary

Technical Problem

In the application of existing polyurethane buffers at the bottom of elevator shafts, their resistance to moisture and heat aging and impact resistance are insufficient, making it difficult to meet the test requirements of GB7588-2020 and TSG7007-2022. Especially in dark and humid environments, the material's mechanics and impact absorption Poor energy capabilities.

Method used

By mixing unsaturated polyester polyol and polyurethane curing agent in a specific ratio, the curing reaction of isocyanate and the free radical curing reaction of carbon-carbon double bonds occur simultaneously to form a polyurethane foam with an interpenetrating cross-linked network structure and enhance the hydrophobicity of the material. properties and cross-linked network strength, improving its performance under impact and damp heat.

Benefits of technology

The polyurethane foam has achieved hydrolysis resistance, high mechanical strength, and excellent cushioning performance. It can meet the requirements of long-term service life and high-frequency impact testing in the elevator pit bottom buffer, and significantly improves the protection ability of property in the car.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116023616B_ABST
    Figure CN116023616B_ABST
Patent Text Reader

Abstract

The present invention provides a polyurethane foam containing an interpenetrating network structure, and a preparation method and application thereof. The preparation method of the polyurethane foam containing an interpenetrating network structure includes: uniformly mixing an unsaturated polyester polyol component and a polyurethane curing agent according to a weight ratio of 1: (1 to 1.2), pouring into a mold for molding, demoulding after curing, and obtaining a polyurethane foam containing an interpenetrating network structure after aging. The microporous elastomeric material of the polyurethane foam containing an interpenetrating network structure prepared by the present invention has hydrolysis resistance, good cushioning performance, and excellent impact resistance. When it is used for the preparation of an elevator pit bottom buffer, it can simultaneously meet the requirements of the new version of GB / 7588‑2020 and the European standard EN81‑20 / 50 for the elevator pit bottom polyurethane buffer, improve the service life of the elevator pit bottom buffer and the ability to absorb and consume impact energy, and ultimately improve the protection of the buffer product to the property in the car.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polymer synthesis and high molecular foaming materials, and specifically relates to a polyurethane foam in which two interpenetrating cross-linking networks are simultaneously present in a polymer by utilizing the simultaneous occurrence of a curing reaction of polyurethane and a cross-linking reaction of free radicals, and a preparation method and application thereof. Background Art

[0002] Polyurethane buffers for elevators are suitable for low-speed elevators with speeds below 1.0m / s. They are the last protective barrier for the property inside the car when the elevator fails and causes the car to fall freely. This requires that the polyurethane buffer has a very good ability to absorb and consume impact energy, and does not suffer a large performance loss due to aging during the entire service life, and the resulting decrease in impact resistance.

[0003] In July 2022, the new version of the inspection regulation TSG7007-2022 was officially released, further clarifying and refining the test specifications and details for polyurethane buffer components in GB7588-2020. That is, after the buffer completes 96h of wet heat aging at 85℃ / 85%RH, the testing agency conducts 10 heavy load and 10 light load impact tests on the buffer at a maximum speed of not less than 1.15m / s. The buffer should have no permanent damage such as cracking. At the same time, it is required that the maximum deceleration of any impact test cannot exceed 6.0g, the rebound speed cannot exceed 1.0m / s, the average deceleration cannot exceed 1.0g, and the time when the deceleration exceeds 2.5g cannot exceed 0.04s, etc. At the same time, it is required to ensure a service life of more than 10 years. This polyurethane buffer must have very high resistance to wet heat aging and the ability to absorb and consume impact energy.

[0004] The polyurethane buffer is installed at the bottom of the elevator shaft, and the working environment is dark and humid. From the perspective of microscopic molecular structure, the polyurethane buffer should meet the following requirements: (1) The polymer chain segment structure is hydrophobic or contains a large number of hydrophobic groups; (2) The strength of the polymer cross-linking network is large enough to withstand 20 impact tests; (3) The molecular chain is relatively rough, and during the compression and recovery process caused by the impact, most of the impact energy can be consumed by friction between the molecular chains in the form of heat.

[0005] Most existing buffers are adipic acid polyester or polypropylene oxide ether polyurethane foam systems. Except for polyadipate neopentyl glycol diol-based polyurethane foam, the polyesters of the other structures are easily hydrolyzed and do not have good resistance to wet heat aging; although the latter has good anti-aging properties, its mechanical and impact resistance are poor. In addition, the polyurethane foams of the above two systems are difficult to meet the test requirements of GB7588-2020 and TSG7007-2022 in terms of consuming impact energy.

[0006] Patent publication number CN110698625A discloses a method for preparing a viscoelastic microporous elastomer, which prepares an IPN-structured microporous elastomer by hybridizing a polyurethane resin and an epoxy resin to form a large number of polyurethane networks with excellent deformation recovery ability. The special network structure inside the polymer can consume a large amount of external impact energy and has excellent deformation recovery ability. However, the mechanical properties of the technology disclosed in this patent are difficult to meet the requirements of polyurethane buffers for elevators. Summary of the invention

[0007] In order to overcome the defects of the materials used in the elevator pit bottom buffer in the above-mentioned prior art, such as poor resistance to moisture and heat aging and impact resistance, the first purpose of the present invention is to provide a method for preparing a polyurethane foam containing an interpenetrating network structure, the second purpose of the present invention is to provide a polyurethane foam containing an interpenetrating network structure obtained by the preparation method, and the third purpose of the present invention is to provide the use of the polyurethane foam containing an interpenetrating network structure as a microporous elastomeric material in the preparation of an elevator pit bottom buffer; the material is resistant to hydrolysis, has high mechanical strength and good buffering performance.

[0008] The purpose of the present invention is achieved by the following technical means:

[0009] In one aspect, the present invention provides a method for preparing a polyurethane foam containing an interpenetrating network structure, comprising the following steps:

[0010] The unsaturated polyester polyol component and the polyurethane curing agent are uniformly mixed in a weight ratio of 1: (1-1.2), poured into a mold for molding, demoulded after curing, and a polyurethane foam containing an interpenetrating network structure is obtained after aging.

[0011] In the above preparation method, preferably, in parts by weight, the unsaturated polyester polyol component comprises:

[0012]

[0013]

[0014] In the above preparation method, preferably, the first polymer diol is selected from one or more combinations of polypropylene oxide ether diol, polytetramethylene glycol ether diol, polyneopentyl adipate, polyneopentyl terephthalate, polyneopentyl phthalate, polyneopentyl isophthalate, polycaprolactone diol and polytetramethylene glycol ether-caprolactone copolymer diol, but is not limited thereto.

[0015] In the above preparation method, preferably, the average molecular weight of the first polymer diol is 2000 g / mol.

[0016] In the above preparation method, preferably, the polyether triol is a polypropylene oxide ether triol obtained by a polyaddition reaction between propylene oxide and glycerol as an initiator, and has a molecular weight of 300 to 700 g / mol.

[0017] In the above preparation method, preferably, the functional monomer is a small molecule compound containing both a hydroxyl group and a carbon-carbon double bond, selected from a combination of one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate, but not limited thereto.

[0018] In the above preparation method, preferably, the chain extender is selected from one or more combinations of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol and 1,6-hexanediol, but is not limited thereto.

[0019] In the above preparation method, preferably, the foam leveling agent is silicone oil selected from Evonik B8547 and / or Momentive DC193, but not limited thereto.

[0020] In the above preparation method, preferably, the promoter is a cobalt salt selected from cobalt naphthenate and / or cobalt isooctanoate, but not limited thereto.

[0021] In the above preparation method, preferably, the catalyst is an organic tin catalyst selected from dibutyltin dilaurate and / or stannous octoate, but not limited thereto.

[0022] In the above-mentioned preparation method, preferably, the preparation method of the polyurethane curing agent comprises:

[0023] The second polymer diol is evacuated at 110-130°C for 1.5-3h, cooled to 50-60°C, isocyanate is added, and reacted at this temperature for 2-3h to obtain a polyurethane prepolymer; the temperature is further cooled to 30-40°C, 2 parts of benzoyl peroxide (BPO, calculated based on 100 parts by weight of the polyurethane prepolymer) are added, and stirred evenly to obtain a polyurethane curing agent.

[0024] In the above preparation method, preferably, the isocyanate group (NCO) content of the polyurethane prepolymer is 16.4% to 22.8%.

[0025] In the above preparation method, preferably, the second polymer diol is selected from one or more combinations of polypropylene oxide ether diol, polytetramethylene ether diol, polyneopentyl adipate, polyneopentyl terephthalate, polyneopentyl phthalate, polyneopentyl isophthalate, polycaprolactone diol and polytetramethylene ether-caprolactone copolymer diol, but is not limited thereto.

[0026] In the above preparation method, preferably, the average molecular weight of the first polymer diol is 2000 g / mol.

[0027] In the above preparation method, preferably, the isocyanate is selected from 4,4-diphenylmethane diisocyanate (MDI-100), a mixture of 2,4-diphenylmethane diisocyanate and 4,4-diphenylmethane diisocyanate by half weight (MDI-50), and a combination of one or more of polyphenylmethane polyisocyanate (polymeric MDI), but is not limited thereto.

[0028] On the other hand, the present invention also provides a polyurethane foam containing an interpenetrating network structure, which is prepared by the above-mentioned preparation method.

[0029] Preferably, the density of the polyurethane foam containing the interpenetrating network structure is 500-800 kg / m 3 .

[0030] On the other hand, the present invention also provides the use of the above-mentioned polyurethane foam containing an interpenetrating network structure as a microporous elastomer material in the preparation of an elevator pit bottom buffer.

[0031] In the present invention, the selected polyol is either polypropylene oxide ether diol or polytetramethylene glycol ether diol, which are naturally hydrophobic; or polyester diol containing neopentyl glycol, the two methyl groups on the molecular structure of which can significantly improve the hydrophobicity of the material; or polycaprolactone polyester diol, which is also naturally hydrophobic. The polyurethane material prepared with the polyol selected in the present invention can fully meet the application requirements of the buffer in terms of hydrolysis resistance.

[0032] The functional monomers used in the unsaturated polyurethane polyol component can be connected with the isocyanate group in the prepolymer through the hydroxyl group on the molecular structure, thereby introducing double bonds into the polyurethane molecular chain. When the unsaturated polyurethane polyol component and the polyurethane curing agent are mixed, the curing reaction of the isocyanate can occur simultaneously, and under the catalysis of the cobalt salt accelerator, the BPO decomposes to trigger the free radical curing reaction of the carbon-carbon double bond. The two curing reactions occur simultaneously, and two different cross-linked networks of polyurethane and polyacrylate can be formed in the cured product, thereby forming an interpenetrating network structure (IPN). During the compression and recovery process caused by impact, the polymer with the IPN structure will not only have friction within the molecular chain within the same cross-linked network and between the molecular chains due to relative slip caused by deformation, but also friction between the molecular chains of different networks, thereby consuming most of the impact energy and converting it into heat energy. The rosin in the unsaturated polyurethane polyol component is cheap, and the carboxyl group in its structure can react with isocyanate to generate carbon dioxide to achieve foaming. When rosin is added to the formula, even water can be omitted to avoid the hydrolysis of the organic tin catalyst that may occur due to the presence of water. In addition, the conjugated double bonds in the rosin structure can participate in the curing of free radicals, thereby linking the polycyclic structure of rosin to the polyacrylate cross-linked network. This polycyclic structure can not only greatly increase the roughness of the molecular chains in the cross-linked network, and increase the friction force during relative slippage within and between molecular chains, but also significantly improve the mechanical properties and UV resistance of the foam.

[0033] Beneficial effects of the present invention:

[0034] The microporous elastomeric material containing polyurethane foam with an interpenetrating network structure prepared by the present invention has hydrolysis resistance, good buffering performance and excellent impact resistance. When it is used in the preparation of elevator pit bottom buffers, the service life of the elevator pit bottom buffers and the ability to absorb and consume impact energy can be improved, and ultimately the protection of the buffer products to the property in the car can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a typical impact test curve of the polyurethane foam containing an interpenetrating network structure prepared in Example 1 of the present invention.

[0036] Figure 2 This is a transmission electron micrograph of the interpenetrating network of the polyurethane foam containing an interpenetrating network structure prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0037] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical scheme of the present invention is now described in detail below, but it should not be construed as limiting the scope of implementation of the present invention; the raw materials used in the following examples are all commercially available in the art unless otherwise specified; the methods used are all conventional preparation methods in the art unless otherwise specified.

[0038] Embodiment 1:

[0039] This embodiment provides a polyurethane foam containing an interpenetrating network structure and a preparation method thereof. The specific preparation method of the polyurethane foam containing an interpenetrating network structure is as follows:

[0040] (1) The unsaturated polyester polyol components are as follows:

[0041]

[0042] (2) Preparation of polyurethane curing agent:

[0043] 100 g of polycaprolactone diol was evacuated at 120° C. for 2 h, cooled to 60° C., 180 g of polyphenylmethane polyisocyanate (polymeric MDI) was added, and reacted at this temperature for 2 h to obtain a polyurethane prepolymer with an NCO content of 18.75%; the temperature was further reduced to 40° C., 5.6 g of benzoyl peroxide was added, and the mixture was stirred evenly to obtain a polyurethane curing agent.

[0044] (3) Preparation of polyurethane foam containing interpenetrating network structure:

[0045] The unsaturated polyester polyol components were mixed with the polyurethane curing agent in a weight ratio of 1:1.2 using a low-pressure two-component foaming machine with a high-speed rotating stirring function, and then poured into a mold for molding. The heat released by the polyurethane reaction and the cobalt salt catalyst were used to initiate the decomposition of BPO to achieve initial curing and demoulding. After further post-aging, a density of 800g / cm 3 Polyurethane foam containing an interpenetrating network structure.

[0046] Embodiment 2:

[0047] This embodiment provides a polyurethane foam containing an interpenetrating network structure and a preparation method thereof. The specific preparation method of the polyurethane foam containing an interpenetrating network structure is as follows:

[0048] (1) The unsaturated polyester polyol components are as follows:

[0049]

[0050] (2) Preparation of polyurethane curing agent:

[0051] 100 g of polytetramethylene glycol was evacuated at 120° C. for 2 h, cooled to 60° C., 250 g of 4,4-diphenylmethane diisocyanate (MDI-100) was added, and reacted at the same temperature for 2 h to obtain a polyurethane prepolymer with an NCO content of 22.80%; the temperature was further reduced to 40° C., 7 g of benzoyl peroxide was added, and the mixture was stirred evenly to obtain a polyurethane curing agent.

[0052] (3) Preparation of polyurethane foam containing interpenetrating network structure:

[0053] The unsaturated polyester polyol components were mixed with the polyurethane curing agent in a weight ratio of 1:1.13 using a low-pressure two-component foaming machine with a high-speed rotating stirring function, and then poured into a mold for molding. The heat released by the polyurethane reaction and the cobalt salt catalyst were used to initiate the decomposition of BPO to achieve initial curing and demoulding. After further post-aging, a density of 500 g / cm 3 Polyurethane foam containing an interpenetrating network structure.

[0054] Embodiment 3:

[0055] This embodiment provides a polyurethane foam containing an interpenetrating network structure and a preparation method thereof. The specific preparation method of the polyurethane foam containing an interpenetrating network structure is as follows:

[0056] (1) The unsaturated polyester polyol components are as follows:

[0057]

[0058] (2) Preparation of polyurethane curing agent:

[0059] 100 g of polytetramethylene glycol-caprolactone copolymer was evacuated at 120° C. for 2 h, cooled to 60° C., 120 g of 4,4-diphenylmethane diisocyanate (MDI-100) was added, and reacted at the same temperature for 2 h to obtain a polyurethane prepolymer with an NCO content of 16.40%; the temperature was further reduced to 40° C., 4.4 g of benzoyl peroxide was added, and the mixture was stirred evenly to obtain a polyurethane curing agent.

[0060] (3) Preparation of polyurethane foam containing interpenetrating network structure:

[0061] The unsaturated polyester polyol components were mixed with the polyurethane curing agent in a weight ratio of 1:1 using a low-pressure two-component foaming machine with a high-speed rotating stirring function, and then poured into a mold for molding. The heat released by the polyurethane reaction and the cobalt salt catalyst were used to induce the decomposition of BPO to achieve initial curing and demoulding. After further post-aging, the density of 620 g / cm 3 Polyurethane foam containing an interpenetrating network structure.

[0062] Test experiment:

[0063] The polyurethane foam containing an interpenetrating network structure prepared in the above Examples 1 to 3 was aged at 85°C / 85% RH for 96 hours and placed at room temperature for 24 hours before testing. During the test, a heavy load (700kg) weight and a light load (200kg) weight were used to perform 10 free fall impact tests on the same sample (20 times for each sample in total). A velocity sensor, an acceleration sensor and a displacement sensor were fixed on the weight to record the relevant data changes during the process. The test was conducted at the National Elevator Testing Center of Shanghai Jiao Tong University.

[0064] The test method is as follows: raise the weight to a height of 85mm directly above the sample (make sure that the weight impacts directly above the sample and the speed when it contacts the sample is not less than 1.15m / s), release the external force of the weight to make it fall freely and impact the sample, and lift the weight again after each impact. The test time interval is 30min to ensure that the sample can return to its original height after the impact test is completed.

[0065] The test data of heavy load impact is shown in Table 1, and the test data of light load impact is shown in Table 2. As a typical impact test curve, the test curve of Example 1 is shown in Figure 1 As shown, the upper coordinate in the figure is acceleration, corresponding to the curve with a peak value between -4 and -6, and the lower coordinate is velocity, corresponding to the curve with a peak value at -8. Figure 2 shown.

[0066] Table 1: Heavy load impact test data

[0067]

[0068]

[0069] Table 2: Light load impact test data

[0070]

[0071]

[0072] Table 1 shows the test results of the maximum load impact (700 kg) of the three samples of Examples 1, 2 and 3 according to the above method. Table 2 shows the test results of the minimum load impact (200 kg) of the three samples of Examples 1, 2 and 3 according to the above method.

[0073] Test results Table 1 and Figure 1It can be seen that when the microporous elastomeric material of the polyurethane foam containing an interpenetrating network structure provided by the present invention is used for the elevator pit bottom buffer, the average deceleration is less than 1.0g, the maximum deceleration is less than 6.0gn, the deceleration time above 2.5gn is less than 40ms, the car rebound speed is less than 1.0m / s, and the sample has no permanent deformation after the test. All data well meet the requirements of GB7588-2020h and EN81-20 / 50 for elevator pit bottom buffers.

[0074] Depend on Figure 2 It can be seen that: the polyurethane curing agent component is dyed with OsO4. The bright part in the figure is the polyurethane phase area after OsO4 dyeing. It can be seen that (1) there are very few polyurethane agglomeration areas and acrylate polymer agglomeration areas at the microscopic level, distributed as follows Figure 2 As shown in the middle circles (above) and (below); (2) most of the area is gray, indicating that the polyurethane network and the acrylic polymer network are well interpenetrated and fused to form a uniform interpenetrating network structure.

[0075] In order to further investigate the anti-hygrothermal aging performance of the polyurethane buffer prepared by the present invention, this test extends the aging time at 85°C / 85%RH from 96h to 720h on the basis of GB7588-2020 and TSG7007-2022. After the aging, impact tests with a heavy load of 700kg and a light load of 200kg are carried out. The test results are shown in Table 3.

[0076] Table 3: Impact test data after aging for 720h at 85℃ / 85%RH

[0077] Test items Overload Light load Action speed 1.22 1.25 Average deceleration (G) 0.35 0.47 Maximum acceleration (G) 4.59 3.67 Duration above 2.5G (seconds) 0.032 0.031 Rebound speed (m / s) 0.69 0.67

[0078] It can be seen from the experimental results in Table 3 that all the data meet the requirements of GB7588-2020h and EN81-20 / 50 for elevator pit bottom buffers. Currently, no commercially available buffers using similar technology can meet the above standards.

[0079] It should be particularly pointed out that the above embodiments are only examples for clear description, and are not limitations on the implementation methods. For professionals in this field, many changes can be derived on the basis of the above description. It is not necessary and impossible to enumerate all the changes here. However, those changes that are obviously derived from them are still within the scope of protection of the present invention.

Claims

1. A method for preparing a polyurethane foam containing an interpenetrating network structure, wherein The following steps are involved: The unsaturated polyester polyol component and the polyurethane curing agent are uniformly mixed in a weight ratio of 1: (1-1.2), poured into a mold for molding, demoulded after curing, and matured to obtain a polyurethane foam containing an interpenetrating network structure; In parts by weight, the components for preparing the unsaturated polyester polyol include: Wherein, the weight portions of water and rosin are not both 0; The functional monomer is a small molecule compound containing both a hydroxyl group and a carbon-carbon double bond, and is selected from a combination of one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate; The preparation method of the polyurethane curing agent comprises: The second polymer diol is evacuated at 110-130°C for 1.5-3h, cooled to 50-60°C, isocyanate is added, and reacted at this temperature for 2-3h to obtain a polyurethane prepolymer; the temperature is further reduced to 30-40°C, and 2 parts of benzoyl peroxide are then added based on 100 parts by weight of the polyurethane prepolymer, and the mixture is stirred evenly to obtain a polyurethane curing agent.

2. The preparation method according to claim 1, It is characterized in that The first polymer diol is selected from one or more combinations of polypropylene oxide ether diol, polytetramethylene ether diol, polyneopentyl adipate, polyneopentyl terephthalate, polyneopentyl phthalate anhydride, polyneopentyl isophthalate, polycaprolactone diol and polytetramethylene ether-caprolactone copolymer diol.

3. The preparation method according to claim 2, It is characterized in that The average molecular weight of the first polymer diol is 2000 g / mol.

4. The preparation method according to claim 1, It is characterized in that The polyether triol is a polypropylene oxide ether triol obtained by using glycerol as an initiator and carrying out a polyaddition reaction with propylene oxide, and has a molecular weight of 300 to 700 g / mol.

5. The preparation method according to claim 1, It is characterized in that The chain extender is selected from one or more combinations of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol and 1,6-hexanediol.

6. The preparation method according to claim 1, It is characterized in that The foam leveling agent is silicone oil selected from Evonik B8547 and / or Momentive DC193.

7. The preparation method according to claim 1, It is characterized in that The promoter is a cobalt salt selected from cobalt naphthenate and / or cobalt isooctanoate.

8. The preparation method according to claim 1, It is characterized in that The catalyst is an organic tin catalyst selected from dibutyltin dilaurate and / or stannous octoate.

9. The preparation method according to claim 1, It is characterized in that The isocyanate content of the polyurethane prepolymer is 16.4% to 22.8%.

10. The preparation method according to claim 1, It is characterized in that The second polymer diol is selected from one or more combinations of polypropylene oxide ether diol, polytetramethylene ether diol, polyneopentyl adipate, polyneopentyl terephthalate, polyneopentyl phthalate anhydride, polyneopentyl isophthalate, polycaprolactone diol and polytetramethylene ether-caprolactone copolymer diol.

11. The preparation method according to claim 10, It is characterized in that The average molecular weight of the second polymer diol is 2000 g / mol.

12. The preparation method according to claim 1, It is characterized in that The isocyanate is selected from one or more combinations of 4,4'-diphenylmethane diisocyanate, a mixture of 2,4'-diphenylmethane diisocyanate and 4,4'-diphenylmethane diisocyanate in half by weight, and polyphenylmethane polyisocyanate.

13. A polyurethane foam containing an interpenetrating network structure, which is prepared by the preparation method according to any one of claims 1 to 12.

14. The polyurethane foam containing an interpenetrating network structure according to claim 13, It is characterized in that The density of the polyurethane foam containing the interpenetrating network structure is 500-800 kg / m 3 .

15. Use of the polyurethane foam containing an interpenetrating network structure as claimed in claim 13 or 14 as a microporous elastomeric material in the preparation of an elevator pit bottom buffer.

Citation Information

Patent Citations

  • Preparation method of viscoelastic microporous elastomer

    CN110698625A

  • Interpenetrating polymer network structure and polishing pad and processes for producing them

    CN101501112A

  • Flame retardant polyurethane composition, flame retardant polyurethane foam material and method for preparing same

    CN102585140A

Cited By

  • Polyurethane-epoxy hybrid microporous elastomer as well as preparation method and application thereof

    CN120309866A