A nano-scale fluorescent antibacterial polymer material and its preparation method and application

By reacting maleic anhydride copolymer with zinc salt under shear stirring conditions, nano-scale fluorescent antibacterial polymer materials were prepared, which solved the problems of poor dispersion of antibacterial agents and excessive particle size in the prior art, and achieved nano-sized Combination of grade fluorescence and antibacterial properties, and has good industrial application potential.

CN116041617BActive Publication Date: 2024-11-19CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111264850.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-28
Publication Date
2024-11-19
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

In the prior art, there are problems with the dispersion effect and minimum addition amount of nano-level antibacterial agents in plastics, and the particle size of maleic anhydride copolymer derivatives is mainly above the micron level, and the combination of nano-level fluorescence and antibacterial properties is not achieved. .

Method used

After fully reacting the maleic anhydride copolymer with alkali metal hydroxide solution, it is added to the zinc saline solution with shear stirring in the form of liquid droplets or liquid lines, and the complexing reaction is carried out to form a nano-scale fluorescent antibacterial polymer material. The particle size is between 10 and 800 nm, the weight fraction of zinc element is 10% to 70%, the excitation wavelength is 325 to 550 nm, and the strongest fluorescence emission range is 350 to 600 nm.

Benefits of technology

It has realized the preparation of nano-level fluorescent antibacterial polymer materials, with a simple process flow, easy to industrial promotion, small particle size, good dispersion, long-lasting antibacterial effect, suitable for dispersion of multiple substrates, and can be quickly distinguished by fluorescence testing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116041617B_ABST
    Figure CN116041617B_ABST
Patent Text Reader

Abstract

The present invention relates to a fluorescent antibacterial polymer material in the field of polymer materials, and a preparation method and application thereof. The fluorescent antibacterial polymer material is a zinc salt derivative of a maleic anhydride copolymer, and the particle size is 10 to 800 nm, preferably 100 to 800 nm. The antibacterial rate of the fluorescent antibacterial polymer material against Escherichia coli and Staphylococcus aureus is greater than 99%. The fluorescent antibacterial polymer material is obtained by fully reacting a linear maleic anhydride copolymer with an alkali metal hydroxide aqueous solution, and then adding the maleic anhydride linear copolymer and an alkali metal hydroxide aqueous solution in the form of droplets and / or liquid lines to a stirred zinc salt aqueous solution for full reaction. The raw materials involved in the fluorescent antibacterial polymer material of the present invention and the items used in the process are low in price, the preparation method is simple and the environmental pollution is low, and the fluorescent antibacterial polymer material has excellent fluorescence performance, high safety, and lasting antibacterial effect, and is suitable for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and more particularly to a nano-level fluorescent antibacterial polymer material and a preparation method and application thereof. Background Art

[0002] Bacterial infection involves many fields such as medical care, food safety, and marine vessels, posing a serious threat to human health and has become one of the world's largest public health issues. In the past few decades, people have continuously developed bactericidal materials that can inhibit bacterial growth, which are mainly divided into organic, inorganic and natural antibacterial agents.

[0003] Natural antimicrobial agents refer to compounds with antimicrobial activity extracted from plants or animals. Common natural antimicrobial agents are mainly chitosan, chitin and antimicrobial peptides. Natural antimicrobial agents are safe and non-toxic, but extraction and processing are relatively difficult. Inorganic antimicrobial agents are mainly metal and metal oxide nanoparticles and carbon nanoparticles. Metals have been effective antimicrobial agents since ancient times. It has been found that metals such as nickel, zinc, cadmium, silver and copper have antimicrobial properties, but inorganic antimicrobial agents have poor compatibility with plastics and generally require modification or carriers to assist in dispersion. Organic antimicrobial agents mainly include cationic polymers, conjugated molecules with reactive oxygen species (ROS) production capabilities and photothermal conversion properties. Common cationic antimicrobial active groups include quaternary ammonium salts, quaternary phosphonium salts, guanidine salts, etc. The antibacterial mechanism of antimicrobial agents is mainly to destroy cell membranes, block cell membrane ion channels, inactivate proteins, etc., so that bacteria cannot metabolize normally and die.

[0004] When antimicrobial agents are applied to plastics, there are often problems with dispersion effect and minimum addition amount. The smaller the antimicrobial particles, the larger their specific surface area and the greater their antimicrobial activity. Therefore, the development of nano-scale antimicrobial agents has greater practical value. As a new type of antimicrobial material, nano-antimicrobial agents have a very broad application prospect in the antimicrobial field. Their preparation methods will surely make greater progress with the development of science and technology. The development and application of more advanced, intelligent, efficient and low-consumption preparation methods will also have a significant impact on human production and life.

[0005] The Chinese patent (publication number: CN111748214A) uses activated carbon as a carrier, nano silver oxide, zinc oxide and zinc pyrithione as antibacterial materials to prepare an environmentally friendly antibacterial agent, which is then mixed with ABS resin to obtain an antibacterial masterbatch. The Chinese patent (publication number: CN109908175B) uses nano copper to load tigecycline by electrostatic adsorption, and then encapsulates it with polydopamine to prepare an organic / inorganic combined antibacterial composition. The composition is composed of nano-scale secondary particles and has good anti-multidrug resistant bacteria effect. Zhang Ziwen et al. (Study on the preparation of a new antibacterial agent by functionalizing hollow nano-silica with polyhexamethyleneguanidine hydrochloride, Materials Engineering 2020, 48(03), 40-46) grafted polyhexamethyleneguanidine hydrochloride to hollow nano-silica, improving the dispersibility of silica while giving it an antibacterial effect. A Chinese patent (publication number: CN109836622B) proposes an organic-inorganic hybrid nano antibacterial material, which has a core-shell structure, wherein the core is an inorganic antibacterial material with a particle size of 50-150nm, and the shell is an organic antibacterial material with a thickness of 1-50nm. This antibacterial material has good dispersibility and interface properties, and is more conducive to the uniform dispersion of the material in the polymer material.

[0006] The maleic anhydride copolymer prepared by "self-stabilizing precipitation polymerization" is a polymer microsphere with uniform particle size. Based on this technology, the application of maleic anhydride copolymer derivatives is currently being studied and developed. Among them, the patents (publication numbers: CN111793155A, CN111793167A, CN111793272A, CN111793340A) modify maleic anhydride copolymers to prepare derivatives with antibacterial properties, but the particle sizes of these derivatives are all in the micron level and above. If the maleic anhydride copolymer can be modified to prepare nano-scale particles with fluorescent and antibacterial properties, its application field will undoubtedly be further expanded. Therefore, the development of nano-scale fluorescent antibacterial polymers and their preparation methods and applications have important market value and research significance. Summary of the invention

[0007] In order to solve the above problems existing in the prior art, the present invention proposes a nano-scale fluorescent antibacterial polymer material. Specifically, it relates to a fluorescent antibacterial polymer material and its preparation method and application. The polymer material of the present invention has both fluorescent and antibacterial functions, and the particle size is less than 1 micron. The preparation process of the present invention is simple and it is easier to promote industrialization.

[0008] One of the purposes of the present invention is to provide a nano-scale fluorescent antibacterial polymer material, which may include a zinc salt derivative of a maleic anhydride copolymer; wherein zinc ions are bound to the carboxylic acid groups of the maleic anhydride copolymer; wherein the weight fraction of the zinc element may be 10% to 70% (for example, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70% or any value between the above values ​​or a numerical range between any two of the above values), preferably 20% to 60%.

[0009] The average particle size of the nanoscale fluorescent antibacterial polymer material can be 10 to 800 nm (for example, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 80, 100, 200, 300, 400, 500, 600, 700, 800 nm or any value between the above values ​​or a numerical range between any two of the above values), preferably 100 to 800 nm, and more preferably 100 to 500 nm.

[0010] Preferably, the excitation wavelength of the nano-scale fluorescent antibacterial polymer material may be 325-550 nm, and the strongest fluorescence emission range is 350-600 nm.

[0011] The maleic anhydride copolymer can be various maleic anhydride alternating copolymers available in the prior art, including at least one of maleic anhydride linear alternating copolymers and maleic anhydride cross-linked alternating copolymers; preferably, it is a maleic anhydride linear alternating copolymer obtained by structural unit A provided by maleic anhydride and structural unit B provided by monomer M; the monomer M is selected from monomers containing isolated carbon-carbon double bonds, preferably at least one of vinyl acetate, styrene, α-methylstyrene, C4, C5, C8, and C9 mixed olefins; preferably at least one of vinyl acetate, styrene, α-methylstyrene, C4, and C5 mixed olefins; wherein the C4 and C5 mixed olefins are selected from C4 and / or C5 fractions of oil refining or ethylene industry, preferably C4 and / or C5 fractions obtained from ethylene cracking in the petrochemical industry.

[0012] Generally speaking, the maleic anhydride copolymer can be prepared by the existing methods in the prior art, for example, according to the method proposed in the literature: A new family of thermoplastic photoluminescence polymers. Polym. Chem., 2016, 7, 6250-6256, and patent CN107722177A.

[0013] The structural characteristics of the fluorescent antibacterial polymer material are as follows: the maleic anhydride in the maleic anhydride copolymer and the zinc ion produce a grafting and complexing reaction, and one zinc ion can be connected to one or more maleic anhydride copolymer molecular chains. The zinc ion in the maleic anhydride copolymer zinc salt derivative is connected to multiple carboxylic acid groups obtained by ring opening of maleic anhydride in the maleic anhydride copolymer, and the multiple connected carboxylic acid groups are the same molecular chain and / or two molecular chains.

[0014] The second object of the present invention is to provide a method for preparing the nano-scale fluorescent antibacterial polymer material, which may include the following steps:

[0015] The maleic anhydride copolymer is fully reacted with an alkali metal hydroxide solution, and then the solution is added in the form of droplets and / or liquid lines to a stirred zinc salt aqueous solution for full reaction; preferably, the stirring is shear stirring. The speed of the shear stirring can be 4000 to 60000 rpm, preferably 5000 to 50000 rpm.

[0016] The preparation of the nano-scale fluorescent antibacterial polymer material of the present invention comprises the steps of directly mixing maleic anhydride linear copolymer solid with an alkali metal hydroxide aqueous solution for full reaction, and then adding a zinc salt aqueous solution with shear stirring in the form of droplets and / or liquid lines for full reaction to obtain the fluorescent antibacterial polymer material.

[0017] Specifically, the preparation method of the nanoscale fluorescent antibacterial polymer material may include the following steps:

[0018] a. Take an alkali metal hydroxide and add it to water to dissolve it to obtain an alkali metal hydroxide aqueous solution;

[0019] b. adding the maleic anhydride copolymer to the aqueous solution of alkali metal hydroxide prepared in step a, and mixing well to react;

[0020] c. adding zinc salt into water to dissolve it to obtain a zinc salt aqueous solution; adding a certain amount of aqueous defoamer into the zinc salt aqueous solution, and then adding the solution of step b into the zinc salt aqueous solution with the aqueous defoamer in the form of droplets and / or liquid lines, accompanied by stirring with shear force, and separating the suspended matter after sufficient mixing and reaction to obtain the fluorescent antibacterial polymer material.

[0021] in,

[0022] In the step a,

[0023] The alkali metal hydroxide may be selected from at least one of lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide and cesium hydroxide, preferably at least one of lithium hydroxide, sodium hydroxide and potassium hydroxide;

[0024] Preferably, the weight ratio of the alkali metal hydroxide to water may range from (0.1 to 100):100, preferably from (0.5 to 50):100.

[0025] In the step b,

[0026] The maleic anhydride copolymer may be a maleic anhydride alternating copolymer, and may include at least one of a maleic anhydride linear alternating copolymer and a maleic anhydride cross-linked alternating copolymer; preferably, it is a maleic anhydride linear alternating copolymer obtained by the structural unit A provided by maleic anhydride and the structural unit B provided by the monomer M; the monomer M may be selected from monomers containing isolated carbon-carbon double bonds, preferably at least one of vinyl acetate, styrene, α-methylstyrene, C4, C5, C8, and C9 mixed olefins; preferably, at least one of vinyl acetate, styrene, α-methylstyrene, C4, and C5 mixed olefins; wherein the C4 and C5 mixed olefins are selected from the C4 and / or C5 fractions of the oil refining or ethylene industry, preferably the C4 and / or C5 fractions obtained from ethylene cracking in the petrochemical industry.

[0027] The weight ratio of the maleic anhydride copolymer to the alkali metal hydroxide may be in the range of (0.1-20):1, preferably (0.1-10):1; the reaction is an acid-base neutralization reaction between the carboxylic acid groups of the maleic anhydride copolymer and the alkali metal hydroxide.

[0028] In the step c,

[0029] The zinc salt can be selected from various zinc salts in the prior art, preferably at least one of water-soluble zinc salts, more preferably at least one of zinc acetate, zinc lactate, zinc chloride, zinc bromide, zinc nitrate, zinc sulfate, and zinc gluconate;

[0030] There is no requirement for the concentration of the zinc salt aqueous solution, as long as the content of the zinc salt in water is within the solubility range of the zinc salt;

[0031] The weight ratio of the zinc salt (solid) to the maleic anhydride copolymer may be in the range of (0.1-20):1 (for example, 0.1, 0.2, 0.3, 0.5, 0.8, 1.0, 1.5, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10, 15, 20 or any value in between the above values ​​or a numerical range between any two of the above values), preferably (0.1-10):1.

[0032] In the step c,

[0033] The aqueous defoamer can be selected from various aqueous defoamers in the prior art, preferably at least one selected from polyether defoamers, alcohol defoamers (especially high-carbon alcohol defoamers), mineral oil defoamers, and silicone defoamers;

[0034] The weight ratio of the aqueous defoamer (solid content) to the maleic anhydride copolymer may be in the range of (0.01% to 1%): 1 (for example, 0.01, 0.02, 0.05, 0.1, 0.2, 0.3, 0.5, 0.8, 1.0% or any value between the above values ​​or a numerical range between any two of the above values).

[0035] Preferably,

[0036] The diameter of the droplet and / or liquid line is 0.005 mm to 5 mm, preferably 0.01 mm to 5 mm, more preferably 0.01 mm to 2 mm, and even more preferably 0.06 mm to 1.55 mm. In practice, multiple droplets / liquid lines can be added together. When the droplets / liquid lines of this diameter come into contact with the zinc salt solution, they can be broken and reacted into nanoparticles under the action of shearing and stirring. If they are too large, the resulting product particles may exceed nanometers; if they are too small, the preparation efficiency will be reduced.

[0037] In the preparation of the nano-scale fluorescent antibacterial polymer material of the present invention, after the maleic anhydride linear copolymer solid is added to the alkali metal hydroxide solution, the maleic anhydride ring will undergo acid-base neutralization reaction and open the ring, and then the maleic anhydride linear copolymer will dissolve in water to form a solution. When the above solution is added to the zinc salt aqueous solution in the form of droplets and / or liquid lines, the system is accompanied by shear stirring, so that the droplets and / or liquid lines will enter the zinc salt aqueous solution and break into smaller droplets. At the same time, the alkali metal ions on the alkali metal salt derivatives of the maleic anhydride linear copolymer will be replaced by zinc ions. The zinc ions are high-valent salts and are easy to react with the alkali metal carboxylates on one or more polymer molecular chains in the form of complexation, coordination, etc., so that the maleic anhydride linear copolymer derivatives undergo cross-linking reaction to form nano precipitation, and then precipitate from water to obtain a nano-antibacterial polymer material. The nano-antibacterial polymer material obtained by the present invention has secondary fluorescent groups (such as C=O, CO, etc.) on the molecular chain, and under the cross-linking action of the zinc salt, the aggregation of these groups is enhanced, so that the product has special fluorescent properties. In addition, the surface of the alkali metal salt derivative of maleic anhydride linear copolymer has hydrophilic and lipophilic groups, which are similar to surfactants. When subjected to high-speed shear stirring, the solution is prone to foaming. Therefore, a certain amount of defoaming agent can be added to the zinc salt aqueous solution system to eliminate the effect of foam on droplet and / or liquid line dispersion and ion replacement cross-linking reaction, and finally obtain a small-particle fluorescent antibacterial polymer material.

[0038] The third object of the present invention is to provide a fluorescent antibacterial polymer material prepared by the preparation method described in the second object of the present invention.

[0039] The fluorescent antibacterial polymer material is a zinc salt derivative of a maleic anhydride copolymer, wherein zinc ions are combined with the carboxylic acid groups of the maleic anhydride copolymer, wherein the weight fraction of the zinc element is 10% to 70%, preferably 20% to 60%;

[0040] The average particle size of the fluorescent antibacterial polymer material may be 10 to 800 nm, preferably 100 to 800 nm, and more preferably 100 to 500 nm;

[0041] Preferably, the excitation wavelength of the fluorescent antibacterial polymer material is 325-550 nm, and the strongest fluorescence emission range is 350-600 nm.

[0042] A fourth object of the present invention is to provide applications of the nano-scale fluorescent antibacterial polymer material, specifically applications in the fields of thermoplastic polymer materials, thermosetting polymer materials, rubber, coatings, inks or anti-counterfeiting.

[0043] The inventors of the present application have found in their research that the modification treatment of maleic anhydride linear copolymers according to the present invention can produce nano-scale fluorescent antibacterial polymers. The main advantages of the present invention are:

[0044] ① The maleic anhydride copolymer is a by-product of industrial polyolefin synthesis, the raw materials are easily available, and the industrial production process is mature;

[0045] ② The preparation process of the fluorescent antibacterial polymer material is simple and easy, with low environmental pollution, small particle size, easy to disperse in a variety of matrices, low addition amount, high safety, long-lasting antibacterial effect, can meet the use requirements under different conditions, and is suitable for industrial application;

[0046] ③The fluorescent antibacterial polymer material has special fluorescent properties and can be quickly distinguished from other products through fluorescence testing. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is a scanning electron microscope (SEM) photograph of the fluorescent antibacterial polymer material of Example 1;

[0048] Figure 2 This is the three-dimensional fluorescence spectrum of the fluorescent antibacterial polymer material of Example 1;

[0049] Figure 3 This is the element energy spectrum of the fluorescent antibacterial polymer material in Example 1, where the ordinate is the intensity and the abscissa is the energy value of the element. The corresponding element can be found in the manual according to the energy value;

[0050] Figure 4 This is the SEM photo of Comparative Example 1;

[0051] Figure 5This is the SEM photo of Comparative Example 2;

[0052] Figure 6 This is the SEM photo of Comparative Example 3;

[0053] Figure 7 SEM photo of Comparative Example 4

[0054] Figure 8 This is the SEM photo of Example 2;

[0055] Fig. 9 is the three-dimensional fluorescence spectrum of Example 2;

[0056] Fig.10 This is the SEM photo of Example 3;

[0057] Fig.11 This is the three-dimensional fluorescence spectrum of Example 3. DETAILED DESCRIPTION

[0058] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0059] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0060] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0061] 1. The raw materials in the embodiments and comparative examples include:

[0062] Maleic anhydride, vinyl acetate, styrene, isoamyl acetate, azobisisobutyronitrile, lithium hydroxide, sodium hydroxide, potassium hydroxide, zinc nitrate, zinc chloride, and zinc lactate were all purchased from Inokite and were of analytical grade; mixed carbon 4 was from Zhenhai Refining and Chemical.

[0063] Water-based defoamer 1: Dow, USA, DF104; (polyether defoamer, ingredients propylene oxide ethylene oxide block polyether)

[0064] Water-based defoamer 2: German SILCONA, AF833; (mineral oil defoamer)

[0065] Water-based defoamer 3: Fujian Xisite Technology, XST-4930; (alcohol defoamer)

[0066] Alumina template: Shanghai Juna Technology, TNT-1, pore size 60-80nm;

[0067] The maleic anhydride-vinyl acetate linear alternating copolymer (MVL) used in the example was prepared by referring to the preparation method described in the open document Anew family of thermoplastic photoluminescence polymers. The main preparation conditions and parameters were as follows: the molar ratio of the reaction monomers maleic anhydride and vinyl acetate was 1:1, the medium was isoamyl acetate, the initiator was azobisisobutyronitrile, and the reaction was carried out at 70° C. for 6 hours.

[0068] The maleic anhydride-C4 linear alternating copolymer (MC4L) used in the embodiment refers to the preparation method described in Example 1 of the Chinese patent with publication number CN107722177A, and the main preparation conditions and parameters are: the reaction monomers are maleic anhydride (20kg) and mixed C4A (14kg), the medium is isoamyl acetate (100L), the initiator is azobisisobutyronitrile (2.4kg), and the reaction is carried out at 70°C for 6 hours. The composition (weight percentage) of the mixed C4A is: 1,2-butadiene, 8.92%; 1,3-butadiene, 14.14%; 1-butene, 8.38%; trans-2-butene, 5.84%; cis-2-butene, 31.7%; vinyl acetylene, 10.99%; isobutane, 1.3%; isobutylene, 12.78%; n-butane, 2.58%, and others, 3.37%.

[0069] The maleic anhydride-styrene linear alternating copolymer (MSL) used in the example was prepared by referring to the preparation method described in the open document A new family of thermoplastic photoluminescence polymers. The main preparation conditions and parameters were as follows: the molar ratio of maleic anhydride and styrene as the reaction monomers was 1:1, the medium was isoamyl acetate, the initiator was azobisisobutyronitrile, and the reaction was carried out at 70° C. for 6 hours.

[0070] Other raw materials are commercially available.

[0071] 2. The experimental data of the embodiments and comparative examples were measured using the following method:

[0072] (1) Scanning electron microscopy (SEM): The sample was glued to a conductive adhesive, gold-sprayed, and then observed using a Hitachi S-4800 scanning electron microscope.

[0073] (2) Fluorescence spectral data: The samples were analyzed and tested using a JY FL3 fluorescence spectrometer from Horiba, Japan, using a 450 W xenon lamp as the light source, an excitation wavelength range of 250 to 650 nm, and an emission spectrum range of 300 to 1000 nm.

[0074] (3) Antibacterial test standards: GB / T 21510-2008 "Test methods for antibacterial properties of nano-inorganic materials", GB / T31402-2015 "Test methods for antibacterial properties of plastic surfaces"; test bacteria: Escherichia coli (ATCC25922), Staphylococcus aureus (ATCC 6538).

[0075] The antibacterial test steps are tested in accordance with GB / T 21510-2008 standard. The specific steps are as follows: weigh 1.0g of the sample to be tested and add 5.0mL of the pre-made bacterial suspension. Take 1.0mL of the inoculation solution and pour it into the agar medium, then culture it in a constant temperature incubator at 37℃ for 48 hours, and finally count the live bacteria on the sample to calculate the antibacterial rate. The blank control group does not add the sample to be tested, and other operations are the same as above.

[0076] Test of antibacterial durability: first soak the sample in 50℃ distilled water for 16 hours, and then test it according to GB / T 21510-2008 standard.

[0077] The antibacterial test steps for plastic surface are tested in accordance with GB / T 31402-2015 standard. The specific steps are as follows: The sample to be tested is made into a 50×50mm specimen, and the bacterial suspension is diluted with 1 / 500 nutrient broth for standby use. Take 0.4mL of inoculation liquid and drop it on the surface of the specimen, and cover it with a 40×40mm film, then cover it with a culture dish cover and culture it for 24 hours at a temperature of 35°C and a humidity of 90%. Finally, the viable bacteria on the specimen are counted to calculate the antibacterial rate. The blank control group is replaced by a specimen without adding fluorescent antibacterial polymer materials, and other operations are the same as above.

[0078] Embodiment 1:

[0079] 5g of sodium hydroxide was dissolved in 100g of water; 5g of MVL was weighed and put into the sodium hydroxide aqueous solution to form a uniform solution; the prepared zinc nitrate solution (50g of zinc nitrate was dissolved in 50g of water) was added with 0.05g of aqueous defoamer 1 and mixed evenly; the zinc nitrate solution was stirred in a high shear emulsifier (FLUKO, FA25, Germany) (shear stirring speed 20000 rpm), and the sodium hydroxide solution of MVL was injected in the form of a liquid line with a needle with a pore size of 0.06mm. After reacting for 3 minutes, the suspended matter was centrifuged and dried to obtain a fluorescent antibacterial polymer material, and its SEM photograph is shown as follows: Figure 1 As shown in FIG. 1 , it can be seen that the obtained product is composed of particles with a particle size of about 100 nm; the three-dimensional fluorescence spectrum is shown in FIG. Figure 2As shown in Figure 1, when the excitation is at 350-530 nm, the emission range is 425-600 nm. Figure 3 As shown (the gold element sprayed on the sample surface at 2.15 eV), the product contains zinc element, the weight fraction of which is 60%, and no sodium element exists, indicating that the sodium element is completely replaced by zinc. The fluorescent antibacterial polymer material was subjected to antibacterial testing.

[0080] Antibacterial results: before boiling, the antibacterial rate against Escherichia coli was >99.9%, and the antibacterial rate against Staphylococcus aureus was >99.9%; after boiling, the antibacterial rate against Escherichia coli was >99.9%, and the antibacterial rate against Staphylococcus aureus was >99.9%.

[0081] Comparative Example 1:

[0082] 5g of sodium hydroxide was dissolved in 100g of water; 5g of MVL was weighed and put into the sodium hydroxide aqueous solution to form a uniform solution; the prepared zinc nitrate solution (50g of zinc nitrate was dissolved in 50g of water) was added with 0.05g of aqueous defoamer 1 and mixed evenly; the zinc nitrate solution was stirred by magnetic stirring, and the sodium hydroxide solution of MVL was injected in the form of a liquid line with a needle with a pore size of 0.06mm. After reacting for 3 minutes, the suspended matter was separated by centrifugation and dried to obtain a fluorescent antibacterial polymer material, and its SEM photograph is shown as follows: Figure 4 As shown. Figure 4 and Figure 1 It can be seen from the comparison that under the action of ordinary magnetic stirring, the obtained fluorescent antibacterial polymer material agglomerated into blocks of tens of microns, which illustrates the indispensability of shear stirring.

[0083] Comparative Example 2:

[0084] 5g of sodium hydroxide was dissolved in 100g of water; 5g of MVL was weighed and put into the sodium hydroxide aqueous solution to form a uniform solution; the prepared zinc nitrate solution (50g of zinc nitrate was dissolved in 50g of water); the zinc nitrate solution was stirred in a high shear emulsifier (FLUKO, FA25, Germany), and the sodium hydroxide solution of MVL was injected in the form of a liquid line with a needle with a pore size of 0.06mm. After reacting for 3 minutes, the suspended matter was separated by centrifugation and dried to obtain a fluorescent antibacterial polymer material, and its SEM photo is shown as follows Figure 5 As shown. Figure 1 and Figure 5 By comparison, it can be seen that when no defoaming agent is added to the system, although the obtained fluorescent antibacterial polymer material is composed of particles with a particle size of about 150nm, the adhesion and agglomeration phenomenon between the particles is very obvious. This is because during the preparation process, the system produces foam under the action of high-speed shear stirring, which is not conducive to the rapid contact reaction between MVL sodium hydroxide solution and zinc nitrate.

[0085] Comparative Example 3:

[0086] Take 5g of sodium hydroxide and dissolve it in 100g of water; weigh 5g of MVL and put it into the sodium hydroxide aqueous solution to form a uniform solution; prepare a zinc nitrate solution (50g of zinc nitrate is dissolved in 50g of water); under the stirring of the zinc nitrate solution in a high shear emulsifier (FLUKO, FA25, Germany), pour the sodium hydroxide solution of MVL directly into the zinc nitrate solution, react for 3 minutes, centrifuge and separate the suspended matter, and dry to obtain a fluorescent antibacterial polymer material, whose SEM photo is shown as follows Figure 6 As shown. Figure 1 and Figure 6 By comparison, when the MVL sodium hydroxide aqueous solution is not added in the form of droplets / lines, the resulting fluorescent antibacterial polymer material has a particle size of about 2 to 10 μm, and the adhesion and agglomeration phenomenon between the particles is very obvious. This is because during the preparation process, after the MVL sodium hydroxide solution is added to the zinc nitrate, the solution is not broken up, and it contacts and reacts with the zinc nitrate over a large area, resulting in a larger product particle size.

[0087] Comparative Example 4:

[0088] Take 5g of sodium hydroxide and dissolve it in 100g of water; weigh 5g of MVL and put it into the sodium hydroxide aqueous solution to form a uniform solution; prepare a zinc nitrate solution (50g of zinc nitrate is dissolved in 50g of water); pass the sodium hydroxide solution of MVL through an alumina template and mix it with the zinc nitrate solution, react for 3 minutes, centrifuge and separate the suspended matter, and dry it to obtain a fluorescent antibacterial polymer material, whose SEM photo is shown as follows Figure 7 As shown. Figure 1 and Figure 7 By comparison, it can be seen that the fluorescent antibacterial polymer material obtained by the template method has a particle size of about 1 to 10 μm, and the bonding and agglomeration phenomenon between the particles is very obvious. This is because during the preparation process, after the MVL sodium hydroxide solution is added to zinc nitrate through the alumina template, due to the lack of shear stirring, some nanodroplets will polymerize again, and some nanodroplets will bond during the reaction with zinc nitrate, resulting in a larger particle size of the obtained product.

[0089] Embodiment 2:

[0090] Take 0.5g potassium hydroxide and dissolve it in 100g water; weigh 5g MC4L and put it into the potassium hydroxide aqueous solution to form a uniform solution; prepare zinc chloride solution (5g zinc chloride dissolved in 50g water), and add 0.005g aqueous defoamer 2 to mix evenly; the zinc chloride solution is stirred in a high shear emulsifier (FLUKO, FA25, Germany) (shear stirring speed 50000 rpm), and the potassium hydroxide solution of MC4L is injected in the form of a liquid line with a needle with a pore size of 0.84mm. After reacting for 3 minutes, the suspended matter is centrifuged and dried to obtain a fluorescent antibacterial polymer material, and the weight fraction of zinc element in the product is 45%. Its SEM photo is as follows Figure 8As shown in FIG. 1 , it can be seen that the obtained product is composed of particles with a particle size of about 100 nm; the three-dimensional fluorescence spectrum is shown in FIG. Fig. 9 As shown, when the excitation is at 325-500 nm, the emission range is 350-575 nm. The fluorescent antibacterial polymer material is subjected to antibacterial test.

[0091] Antibacterial results: before boiling, the antibacterial rate against Escherichia coli was >99.9%, and the antibacterial rate against Staphylococcus aureus was >99.9%; after boiling, the antibacterial rate against Escherichia coli was >99.9%, and the antibacterial rate against Staphylococcus aureus was >99.9%.

[0092] Embodiment 3:

[0093] Take 50g lithium hydroxide and dissolve it in 100g water; weigh 5g MSL and put it into the lithium hydroxide aqueous solution to form a uniform solution; prepare zinc lactate solution (0.5g zinc lactate dissolved in 50g water), add 0.0005g aqueous defoamer 3 and mix evenly; the zinc lactate solution is stirred in a high shear emulsifier (FLUKO, FA25, Germany) (shear stirring speed 5000 rpm), and the MSL lithium hydroxide solution is injected in the form of droplets using a needle with a pore size of 1.55mm. After reacting for 3 minutes, the suspended matter is centrifuged and dried to obtain a fluorescent antibacterial polymer material, and the weight fraction of zinc element in the product is 20.5%. Its SEM photo is as follows Fig.10 As shown in FIG. 1 , it can be seen that the obtained product is composed of particles with a particle size of about 500 nm; the three-dimensional fluorescence spectrum is shown in FIG. Fig.11 As shown, when the excitation is at 325-550 nm, the emission range is 400-600 nm. The fluorescent antibacterial polymer material is subjected to antibacterial test.

[0094] Antibacterial results: before boiling, the antibacterial rate against Escherichia coli was >99.9%, and the antibacterial rate against Staphylococcus aureus was >99.9%; after boiling, the antibacterial rate against Escherichia coli was >99.9%, and the antibacterial rate against Staphylococcus aureus was >99.9%.

[0095] Embodiment 4:

[0096] 100 parts by weight of a polypropylene resin (Sinopec Beijing Yanshan Company, brand K9026, melt index 29.0 g / 10 min, impact copolymer), 0.1 parts by weight of the fluorescent antibacterial polymer material described in Example 1, 0.1 parts by weight of an antioxidant 168 (Ciba-Geigy, Switzerland), and 0.1 parts by weight of an antioxidant 1010 (Ciba-Geigy, Switzerland) were respectively weighed, stirred and mixed, and the mixture was put into a Haake twin-screw extruder, the temperature was set at 180-230° C., and a polypropylene composition was obtained by screw extrusion granulation.

[0097] The obtained antibacterial polypropylene composition was injection molded into a 50×50×1mm sample and subjected to antibacterial testing according to standard GB / T31402-2015. Antibacterial results: before boiling, the antibacterial rate against Escherichia coli was >99.9%, and the antibacterial rate against Staphylococcus aureus was >99.9%; after boiling, the antibacterial rate against Escherichia coli was >99.9%, and the antibacterial rate against Staphylococcus aureus was >99.9%.

[0098] Comparative Example 4:

[0099] 100 parts by weight of polypropylene resin (Sinopec Beijing Yanshan Branch, brand K9026, melt index 29.0 g / 10 min, impact copolymer), 0.1 parts by weight of the fluorescent antibacterial polymer material described in Comparative Example 3, 0.1 parts by weight of antioxidant 168 (Ciba-Geigy, Switzerland), and 0.1 parts by weight of antioxidant 1010 (Ciba-Geigy, Switzerland) were weighed respectively, and after stirring and mixing, the mixture was put into a Haake twin-screw extruder, the temperature was set at 180-230°C, and a polypropylene composition was obtained by screw extrusion and granulation.

[0100] The obtained antibacterial polypropylene composition was injection molded into a 50×50×1mm specimen and subjected to antibacterial testing according to standard GB / T31402-2015. Antibacterial results: before boiling, the antibacterial rate against Escherichia coli was >99.1%, and the antibacterial rate against Staphylococcus aureus was >99.0%; after boiling, the antibacterial rate against Escherichia coli was >99.0%, and the antibacterial rate against Staphylococcus aureus was >99.0%.

Claims

1. A nano-scale fluorescent antibacterial polymer material, wherein the fluorescent antibacterial polymer material comprises a zinc salt derivative of a maleic anhydride copolymer; in, The carboxylic acid group of the maleic anhydride copolymer is bonded with zinc ions; the weight fraction of the zinc element is 10% to 70%; The average particle size of the fluorescent antibacterial polymer material is 10-800nm.

2. The nanoscale fluorescent antibacterial polymer material according to claim 1, Features: The weight fraction of the zinc element is 20% to 60%.

3. The nano-scale fluorescent antibacterial polymer material according to claim 1, Features: The average particle size of the fluorescent antibacterial polymer material is 100-800nm.

4. The nanoscale fluorescent antibacterial polymer material according to claim 3, Features: The average particle size of the fluorescent antibacterial polymer material is 100-500nm.

5. The nanoscale fluorescent antibacterial polymer material according to claim 1, Features: The excitation wavelength of the fluorescent antibacterial polymer material is 325-550nm, and the strongest fluorescence emission range is 350-600nm.

6. The nano-scale fluorescent antibacterial polymer material according to claim 1, Features: The maleic anhydride copolymer is a maleic anhydride alternating copolymer, including at least one of a maleic anhydride linear alternating copolymer and a maleic anhydride cross-linked alternating copolymer.

7. The nanoscale fluorescent antibacterial polymer material according to claim 6, Features: The maleic anhydride copolymer is a maleic anhydride linear alternating copolymer obtained by structural unit A provided by maleic anhydride and structural unit B provided by monomer M; the monomer M is selected from monomers containing isolated carbon-carbon double bonds.

8. The nanoscale fluorescent antibacterial polymer material according to claim 7, Features: The monomer M is selected from at least one of vinyl acetate, styrene, α-methylstyrene, and C4, C5, C8, and C9 mixed olefins.

9. The nanoscale fluorescent antibacterial polymer material according to claim 8, Features: The monomer M is selected from at least one of vinyl acetate, styrene, α-methylstyrene, C4 and C5 mixed olefins; wherein the C4 and C5 mixed olefins are selected from the C4 fraction and C5 fraction of the oil refining or ethylene industry.

10. The nanoscale fluorescent antibacterial polymer material according to claim 9, Features: The C4 and C5 mixed olefins are selected from the C4 fraction and C5 fraction of ethylene cracking in the petrochemical industry.

11. A method for preparing the nano-scale fluorescent antibacterial polymer material according to any one of claims 1 to 10, Features The following steps are involved: a. Take an alkali metal hydroxide and add it to water to dissolve it to obtain an alkali metal hydroxide solution; b. adding the maleic anhydride copolymer to the alkali metal hydroxide solution obtained in step a and mixing well to react; c. taking a zinc salt and adding it to water to dissolve it to obtain a zinc salt aqueous solution; adding an aqueous defoamer to the zinc salt aqueous solution, and then adding the solution of step b in the form of droplets and / or liquid lines to the zinc salt aqueous solution with the aqueous defoamer, accompanied by shear stirring, mixing and reacting thoroughly, separating the suspended matter to obtain the fluorescent antibacterial polymer material; The diameter of the droplet and / or liquid line is 0.005 mm to 5 mm; The rotation speed of the shear stirring is 4000-60000 rpm.

12. The method for preparing the nano-scale fluorescent antibacterial polymer material according to claim 11, Features: In the step a, The alkali metal hydroxide is selected from at least one of lithium hydroxide, sodium hydroxide and potassium hydroxide.

13. The method for preparing the nano-scale fluorescent antibacterial polymer material according to claim 12, Features: The weight ratio of the alkali metal hydroxide to water is in the range of (0.1-100):

100.

14. The method for preparing the nano-scale fluorescent antibacterial polymer material according to claim 13, Features: The weight ratio of the alkali metal hydroxide to water is in the range of (0.5-50):

100.

15. The method for preparing the nano-scale fluorescent antibacterial polymer material according to claim 11, Features: In the step b, The weight ratio of the maleic anhydride copolymer to the alkali metal hydroxide is in the range of (0.1-20):

1.

16. The method for preparing the nano-scale fluorescent antibacterial polymer material according to claim 15, Features: The weight ratio of the maleic anhydride copolymer to the alkali metal hydroxide is in the range of (0.1-10):

1.

17. The method for preparing the nano-scale fluorescent antibacterial polymer material according to claim 11, Features: In the step c, The zinc salt is at least one of water-soluble zinc salts; The weight ratio of the zinc salt to the maleic anhydride copolymer is in the range of (0.1-20):

1.

18. The method for preparing the nano-scale fluorescent antibacterial polymer material according to claim 17, Features: The zinc salt is selected from at least one of zinc acetate, zinc lactate, zinc chloride, zinc bromide, zinc nitrate, zinc sulfate and zinc gluconate.

19. The method for preparing the nano-scale fluorescent antibacterial polymer material according to claim 17, Features: The weight ratio of the zinc salt to the maleic anhydride copolymer is in the range of (0.1-10):

1.

20. The method for preparing the nano-scale fluorescent antibacterial polymer material according to claim 11, Features: In the step c, The aqueous defoamer is selected from at least one of polyester defoamers, alcohol defoamers, mineral oil defoamers, and silicone defoamers; and / or, The weight ratio of the aqueous defoamer to the maleic anhydride copolymer is in the range of (0.01% to 1%):

1.

21. The method for preparing the nano-scale fluorescent antibacterial polymer material according to claim 11, Features: In the step c, The diameter of the liquid droplets and / or liquid lines is 0.01 mm to 5 mm.

22. The method for preparing the nano-scale fluorescent antibacterial polymer material according to claim 21, Features: The diameter of the liquid droplets and / or liquid lines is 0.01 mm to 2 mm.

23. The method for preparing the nano-scale fluorescent antibacterial polymer material according to claim 11, Features: In the step c, The rotation speed of the shear stirring is 5000-50000 rpm.

24. Use of the nano-scale fluorescent antibacterial polymer material according to any one of claims 1 to 10 in the fields of thermoplastic polymer materials, thermosetting polymer materials, rubber, coatings, inks, and anti-counterfeiting.