A method for recovering gallium from gallium arsenide waste
By adopting efficient process flow in gallium arsenide waste, including acid solution leaching, extraction, washing, backing and electrochemical refining, combined with complexing agent, the problems of high acid and alkali consumption and low gallium electrostatic current efficiency are solved. , achieving efficient and environmentally friendly gallium recycling, improving economic benefits and resource utilization.
Patent Information
- Application Number
- CN202211681125.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-27
AI Technical Summary
In the prior art, the acid and alkali consumption of gallium arsenide waste is high, and the gallium electrostatic current efficiency is low, resulting in low economic benefits and high environmental pressure. In the process of separating gallium and arsenic, a large amount of acid and alkali are consumed, resulting in pollution and energy. waste.
Adopt an efficient and green process, by mixing gallium arsenide-containing raw materials with acid solution, pH adjustment and extraction, followed by washing and back-extraction using acid and alkali solutions, combined with electrochemical refining, and using complexing agents to improve current efficiency , realize efficient recycling of gallium.
The gallium recovery rate has been achieved to reach more than 96%, reducing the consumption of acid and alkali, improving economic benefits, reducing pollution emissions, and environmentally friendly and efficient processes.
Smart Images

Figure CN116043042B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resource recycling, and in particular to a method for recovering gallium from gallium arsenide waste. Background Art
[0002] Gallium arsenide is widely used as an efficient semiconductor material. It has the characteristics of high electron mobility, high output power, high efficiency and low distortion. It is an important supporting material for information technology. The production process of gallium arsenide is to synthesize gallium arsenide polycrystalline compounds with high-purity arsenic and high-purity gallium first, and then go through a series of steps such as single crystal growth, cutting, grinding, thinning, polishing, corrosion, cleaning, etc. to obtain gallium arsenide single crystals that meet downstream needs. In the entire production process, waste will be generated in each step. Nearly 70% of gallium arsenide is discarded along with waste, with low economic utilization rate and harm to the environment. Efficient gallium arsenide waste recycling process has important economic and environmental significance for improving and optimizing industrial production. The waste generated by gallium arsenide production is mainly gallium arsenide residues and mixed particles with corundum generated in the process of cutting, grinding, polishing, etc., as well as wastewater generated in each process. Patent CN110938742A discloses a method for recovering sodium arsenate and metallic gallium from gallium arsenide waste residue, wherein arsenic and gallium are leached into a solution by alkaline oxidation, metallic gallium is obtained by cyclonic electrowinning, and separated from arsenic. Patent CN106498168A discloses a method for recovering gallium from oil-containing gallium arsenide slurry, wherein gallium arsenide is leached by controlled potential in a sulfuric acid system, P204 is used as an extractant for extraction, gallium and arsenic are separated, gallium is stripped with hydrochloric acid, neutralized and filtered, and then dissolved in liquid alkali for electrodeposition.
[0003] Due to the variety of types and complex composition of gallium arsenide waste, the leaching and neutralization processes in the process consume a large amount of acid and alkali. The extraction process is the most efficient technology for separating arsenic from gallium and is easy to apply industrially. However, its stripping often uses a high-concentration acid as a stripping agent, and the subsequent neutralization precipitation requires a large amount of alkali, which is incomplete. In addition, the gallium hydroxide is colloidal and difficult to filter. In addition, the process of obtaining metallic gallium by electrolysis in a sodium hydroxide system usually has low current efficiency and high energy consumption. Therefore, reducing the consumption of acid and alkali, improving material utilization, further improving economic benefits, and reducing environmental pressure are of great significance to the resource utilization and economic and environmental protection of gallium arsenide waste. Summary of the invention
[0004] In view of the problems existing in the above-mentioned prior art, the present invention provides a gallium recovery method to solve the problems of high acid and alkali consumption and low current efficiency of gallium electrowinning. Through an efficient, green and environmentally friendly process flow, gallium in gallium arsenide waste is recovered and processed, which can effectively improve economic benefits and reduce pollution emissions.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A gallium recovery method comprises the following steps:
[0007] (1) mixing a raw material containing gallium arsenide, an acid solution, and an oxidant, stirring, and leaching to obtain a leaching solution and leaching residue;
[0008] (2) adjusting the pH of the leachate in step (1), extracting the leachate to obtain an organic phase and a raffinate;
[0009] (3) washing the organic phase in step (2) with an acid solution to obtain an acid wash solution and a gallium-containing organic phase;
[0010] (4) stripping the gallium-containing organic phase in step (3) with an alkaline solution to obtain a lean organic phase and a gallium-containing stripping solution;
[0011] (5) electrochemically refining the gallium-containing stripping solution of step (4) to obtain metallic gallium;
[0012] A complexing agent is added to the gallium-containing stripping solution.
[0013] Preferably, in this gallium recovery method, in step (1), the solid-liquid ratio of the raw material containing gallium arsenide and the acid solution is (4-6) kg:1L; further preferably, the solid-liquid ratio of the raw material containing gallium arsenide and the acid solution is (4.5-5.5) kg:1L; even more preferably, the solid-liquid ratio of the raw material containing gallium arsenide and the acid solution is 5 kg:1L.
[0014] Preferably, in this gallium recovery method, in step (1), the hydrogen ion concentration of the acid solution is 0.8-1.2 mol / L; further preferably, the hydrogen ion concentration of the acid solution is 0.85-1.15 mol / L; further preferably, the hydrogen ion concentration of the acid solution is 0.9-1.1 mol / L; the acid solution can be a hydrochloric acid solution of a gallium arsenide or high-purity gallium pickling process.
[0015] In the present invention, the pickling solution in step (3) can be returned to step (1) as a leaching solution, which can ensure that a gallium leaching rate of more than 97% can be achieved in one leaching under low-acid conditions.
[0016] Preferably, in this gallium recovery method, in step (1), the amount of oxidant added satisfies that the potential of the leaching process is greater than 0 V; further preferably, the amount of oxidant added satisfies that the potential of the leaching process is greater than 0.6 V; by adding the oxidant, the system potential is controlled and no arsine is generated during the process.
[0017] In some specific embodiments of the present invention, the oxidant is hydrogen peroxide, and the hydrogen peroxide is commonly available on the market.
[0018] Preferably, in the gallium recovery method, in step (1), the leaching temperature is 20 to 90°C; more preferably, the leaching temperature is 40 to 90°C; and even more preferably, the leaching temperature is 60 to 85°C.
[0019] Preferably, in the gallium recovery method, in step (1), the leaching time is 2 to 6 hours; more preferably, the leaching time is 2.5 to 5.5 hours; and even more preferably, the leaching time is 3 to 5 hours.
[0020] Preferably, in the gallium recovery method, in step (2), the pH is adjusted to a pH value of 1 to 2.5; further preferably, the pH is adjusted to a pH value of 1.5 to 2.
[0021] Preferably, in the gallium recovery method, in step (2), the extractant includes P204 (di(2-ethylhexyl) phosphate) and a diluent; in some specific embodiments of the present invention, the diluent is sulfonated kerosene; further preferably, the volume ratio of P204 to the diluent is 1:(2-3); further preferably, the volume ratio of P204 to the diluent is 3:7. The present invention uses P204 as an extractant, the gallium extraction rate reaches more than 99%, arsenic has no extraction effect, the gallium content in the raffinate is low, and the separation rate of gallium and arsenic exceeds 99%.
[0022] Preferably, in this gallium recovery method, in step (2), the volume ratio of the extractant to the aqueous phase is 1:(0.5-1.5); further preferably, the volume ratio of the extractant to the aqueous phase is 1:(0.8-1.2); further preferably, the volume ratio of the extractant to the aqueous phase is 1:1.
[0023] Preferably, in this gallium recovery method, in step (3), the pH of the acid solution is 1 to 3; further preferably, the pH of the acid solution is 1 to 2; in some preferred embodiments of the present invention, the acid solution is a hydrochloric acid solution.
[0024] Preferably, in this gallium recovery method, in step (3), the volume ratio of the acid solution to the organic phase is 1: (5-15); further preferably, the volume ratio of the acid solution to the organic phase is 1: (8-12); further preferably, the volume ratio of the acid solution to the organic phase is 1: (9-11); the purpose of washing in step (3) of the present invention is to remove arsenic mechanically entrained in the organic phase.
[0025] Preferably, in the gallium recovery method, in step (4), the alkaline solution is a sodium hydroxide solution; sodium hydroxide is used as a stripping agent, and the stripping rate reaches 100%, thereby simplifying the process flow and improving production efficiency.
[0026] Preferably, in this gallium recovery method, in step (4), the concentration of the alkaline solution is 80-180 g / L; further preferably, the concentration of the alkaline solution is 90-160 g / L; further preferably, the concentration of the alkaline solution is 100-150 g / L.
[0027] Preferably, in this gallium recovery method, in step (4), the volume ratio of the alkaline solution to the gallium-containing organic phase is 1:(1-3); further preferably, the volume ratio of the alkaline solution to the gallium-containing organic phase is 1:(1.5-2.5).
[0028] Preferably, in this gallium recovery method, the amount of the complexing agent added is 0.25-0.4 g / L; further preferably, the amount of the complexing agent added is 0.25-0.35 g / L; and further preferably, the amount of the complexing agent added is 0.25-0.3 g / L. When the amount of the complexing agent added exceeds this range, the current efficiency does not increase with the increase in the amount of the complexing agent added. The complexing agent can be added to the alkaline solution in step (4), and the complexing agent enters the gallium-containing stripping solution through stripping; the complexing agent can also be added to the gallium-containing stripping solution during electrochemical refining. The electrolyte solution used in the electrochemical refining process is the stripping solution. Since it involves recycling, adding it to the stripping solution will not affect the stripping rate. Its function is only to improve the current efficiency of the electrochemical refining process. The amount of the complexing agent added is the concentration in the stripping solution or the electrolyte solution.
[0029] Preferably, in the gallium recovery method, the complexing agent includes disodium ethylenediaminetetraacetate; the present invention adopts this specific complexing agent to achieve an improvement in current efficiency.
[0030] Preferably, in the gallium recovery method, in step (5), the current density of the electrochemical refining is 100 to 200 A / m 2 Further preferably, the current density of electrochemical refining is 120 to 180 A / m 2 Further preferably, the current density of electrochemical refining is 140 to 160 A / m 2 .
[0031] Preferably, in the gallium recovery method, in step (5), the electrochemical refining is carried out in an electrochemical refining device; the electrochemical refining device comprises:
[0032] A cathode, disposed at one end of the electrochemical refining device;
[0033] an anode, disposed at the other end of the electrochemical refining device;
[0034] The partition is arranged between the cathode and the anode to divide the electrochemical refining device into two spaces, namely the electrolysis chamber and the electrolysis chamber. A channel is arranged at the bottom of the partition to keep the electrolysis chamber and the electrolysis chamber connected.
[0035] The electrochemical refining device of the present invention is composed of an electrolytic chamber and an electrolytic chamber. The partition between the two functions to block the electrolyte. There is a channel at the bottom thereof, which is filled with flowing liquid gallium. The conductive property of gallium is utilized to realize current conduction between the electrolytic chamber and the electrolytic chamber. The gallium-containing stripping solution obtained in step (4) is placed in the electrolytic chamber of the electrochemical refining device. By performing electrolytic + electrolysis simultaneously, metallic gallium is obtained in the electrolytic chamber. The electrolytic solution after electrochemical treatment can be returned to step (4) for use as a stripping solution.
[0036] Further preferably, in the electrochemical refining device, the cathode electrode used is liquid metal gallium.
[0037] More preferably, in the electrochemical refining device, the electrode used as the anode is a platinum electrode.
[0038] The beneficial effects of the present invention are:
[0039] The pickling solution, electrolytic solution and organic extractant produced by the method of the present invention can be returned to the process for recycling, the consumption of acid and alkali reagents is small, and the recovery rate of gallium can reach more than 96%, which is economical, efficient, energy-saving and environmentally friendly.
[0040] The present invention adds a small amount of complexing agent and utilizes the property that the complexing agent can be adsorbed on the cathode under the action of an electric field to form a thin layer of complexing agent on the cathode surface. The complex formed by gallium and the complexing agent is more stable, and the gallium in the solution system is captured at the cathode, thereby increasing the gallium concentration in the cathode area. The current efficiency of the gallium electrochemical refining process can be increased to 78%, and the electrolytic solution after electrolysis can be returned to the stripping process for use. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 Schematic diagram of the process flow for recovering gallium from gallium arsenide waste in an embodiment.
[0042] Figure 2 Schematic diagram of the electrochemical refining device used in the examples.
[0043] Attached Figure 2 mark:
[0044] 100 - first circulation pump, 200 - anode, 300 - partition, 400 - cathode, 500 - second circulation pump, 600 - liquid gallium, 700 - electrolysis chamber, 800 - electrolysis chamber. DETAILED DESCRIPTION
[0045] The present invention is further described in detail below through specific examples. It should be noted that the following examples do not limit the scope of protection claimed by the present invention.
[0046] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0047] As attached Figure 2 As shown, the electrochemical refining device of the present invention includes an anode 200 , a separator 300 , and a cathode 400 .
[0048] The anode 200 is arranged at one end of the electrochemical refining device; the cathode 400 is arranged at the other end of the electrochemical refining device; the partition 300 is arranged between the anode 200 and the cathode 400, dividing the electrochemical refining device into two spaces, namely the electrolysis chamber 700 and the electrolysis chamber 800, and a channel is provided at the bottom of the partition 300 to keep the electrolysis chamber 700 and the electrolysis chamber 800 connected.
[0049] The electrochemical refining device of the present invention further includes a first circulation pump 100, which is used for circulating the electrolyte in the electrolysis chamber 700; the electrochemical refining device of the present invention further includes a second circulation pump 500, which is used for circulating the electrolyte in the electrolysis chamber 800; the gallium-containing stripping solution is placed in the electrolysis chamber 700 of the electrochemical treatment device, the first circulation pump 100 and the second circulation pump 500 are turned on, the power is turned on, and the liquid gallium is recovered at the bottom of the electrolysis chamber 800.
[0050] The electrochemical refining device of the present invention utilizes the conductive property of liquid gallium and induces the cathode and anode formed by an external electric field to form an anion-cation concentration difference in the solution, so as to realize that part of the liquid gallium 600 in the electrolysis chamber 800 is used as the anode to electrolyze gallium, and part of the liquid gallium 600 in the electrolysis chamber 800 is used as the anode to electrolyze gallium. The cathode 400 in the electrolysis chamber is liquid metal gallium. A conductive plate, such as a platinum electrode plate, is inserted into the liquid metal gallium and connected to electricity. After one electrochemical refining, the electrolysis and electrolysis processes are completed synchronously, which can solve the problem of incomplete separation of the electrolytic solution and metal gallium, and can effectively avoid the contamination of metal gallium by a small amount of organic phase remaining in the electrolytic solution.
[0051] Example 1
[0052] like Figure 1 As shown, this embodiment provides a method for recovering gallium from gallium arsenide waste, comprising the following steps:
[0053] Step S1: controlled potential low-acid leaching: gallium arsenide waste is mixed with gallium-containing waste acid washing liquid (hydrogen ion concentration is 0.9 mol / L) at a solid-liquid ratio of 5kg:1L, slurried at room temperature, and an oxidant (hydrogen peroxide) is added to adjust the system potential. The slurry process is greater than 0V. The room temperature is maintained at 25°C, and the leaching is stirred. During the leaching process, the potential is greater than 0.6V. The reaction is performed for 5h, and the leachate and leaching residue are obtained by filtering;
[0054] Step S2: Extracting gallium with P204: The pH of the leaching solution obtained in step S1 is adjusted to 1.5-2, and two-stage extraction is adopted. According to the ratio of organic phase to aqueous phase of 1:1, 30% P204+70% sulfonated kerosene and the leaching solution after pH adjustment are added to the extraction equipment, and after shaking for 5 minutes, the mixture is allowed to stand for clarification, and the gallium-containing organic phase and the raffinate are separated;
[0055] Step S3: washing the organic phase: washing the gallium-containing organic phase obtained in step S2 with a dilute hydrochloric acid solution having a pH of 1.5 and a ratio of organic phase to aqueous phase of 10:1, shaking and mixing, standing to clarify, and separating to obtain a washing liquid and a gallium-containing organic phase, and the washing liquid is returned to step S1 for use as an acid leaching solution;
[0056] Step S4: Gallium stripping: The gallium-containing organic phase obtained in step S3 is placed in a stripping device, and 100 g / L sodium hydroxide solution is added thereto at a ratio of 2:1 between the organic phase and the aqueous phase to perform stripping operation, and the mixture is shaken to mix, allowed to stand for clarification, and separated to obtain a lean organic phase and a gallium-containing stripping solution.
[0057] In this embodiment, the leaching rate of gallium contained in the gallium arsenide waste is 42.04%, and the leaching rate of arsenic is 37.77%. The leaching solution undergoes an extraction process, wherein the extraction rate of gallium is 99.90%, and there is no extraction effect on arsenic. The separation rate of gallium and arsenic exceeds 99%. Using 100 g / L sodium hydroxide solution as a stripping agent, the stripping rate of gallium is 92.15%.
[0058] Example 2
[0059] like Figure 1 As shown, this embodiment provides a method for recovering gallium from gallium arsenide waste, comprising the following steps:
[0060] Step S1: controlled potential low-acid leaching: gallium arsenide waste is mixed with gallium-containing waste acid washing liquid (hydrogen ion concentration is 0.9 mol / L) at a solid-liquid ratio of 5:1, slurried at room temperature, and an oxidant (hydrogen peroxide) is added to adjust the system potential. The slurry process is greater than 0V. The temperature is maintained at 80°C, and leaching is stirred. During the leaching process, the potential is greater than 0.6V. The reaction is performed for 4 hours, and the leachate and leaching residue are obtained by filtration;
[0061] Step S2: Extracting gallium with P204: The pH of the leaching solution obtained in step S1 is adjusted to 1.5-2, and 30% P204 + 70% sulfonated kerosene and the leaching solution after pH adjustment are added to the extraction equipment according to the ratio of organic phase to aqueous phase of 1:1. After shaking for 5 minutes, the mixture is allowed to stand for clarification, and the gallium-containing organic phase and the raffinate are separated;
[0062] Step S3: washing the organic phase: washing the gallium-containing organic phase obtained in step S2 with a dilute hydrochloric acid solution having a pH of 1.5 and a ratio of organic phase to aqueous phase of 10:1, shaking and mixing, standing to clarify, and separating to obtain a washing liquid and a gallium-containing organic phase, and the washing liquid is returned to step S1 for use as an acid leaching solution;
[0063] Step S4: Gallium stripping: the gallium-containing organic phase obtained in step S3 is placed in a stripping device, and 150 g / L sodium hydroxide solution is added thereto in a ratio of 2:1 between the organic phase and the aqueous phase to perform stripping operation, and the mixture is shaken and mixed, allowed to stand for clarification, and separated to obtain a lean organic phase and a gallium-containing stripping solution;
[0064] Step S5: Electrochemical refining of gallium: In an environment with a temperature of 35°C, the gallium-containing stripping solution obtained in step S4 is placed in the electrochemical refining chamber of the electrochemical refining device, and electrolysis and electrolysis are carried out simultaneously at a current density of 150A / m 2 In the electrolysis chamber, metallic gallium is obtained, and the electrolytic solution after electrochemical treatment is returned to step S4 for use as a stripping solution.
[0065] In this embodiment, the leaching rate of gallium contained in gallium arsenide waste is 97.21%, and the leaching rate of arsenic is 97.28%. The leaching solution is subjected to an extraction process, wherein the extraction rate of gallium is 99.33%, and there is no extraction effect on arsenic. The separation rate of gallium and arsenic exceeds 99%. Using 150g / L sodium hydroxide solution as a stripping agent, the stripping rate of gallium is 100%. Without adding a complexing agent, in the electrochemical refining process, the current efficiency of gallium precipitation at the cathode is 41%. The theoretical output is calculated by the electrochemical equivalent of the metal. By measuring the actual mass of the cathode precipitate, the actual output ÷ theoretical output = current efficiency, and the gallium content in the electrolytic solution can be reduced to below 1g / L.
[0066] Example 3
[0067] like Figure 1 As shown, this embodiment provides a method for recovering gallium from gallium arsenide waste, comprising the following steps:
[0068] Step S1: controlled potential low-acid leaching: gallium arsenide waste is mixed with gallium-containing waste acid washing liquid (hydrogen ion concentration is 0.9 mol / L) at a solid-liquid ratio of 5:1, slurried at room temperature, and an oxidant (hydrogen peroxide) is added to adjust the system potential. The slurry process is greater than 0V. The temperature is maintained at 80°C and leached with stirring. During the leaching process, the potential is greater than 0.6V. The reaction is performed for 3 hours, and the leachate and leaching residue are obtained by filtration;
[0069] Step S2: Extracting gallium with P204: The pH of the leaching solution obtained in step S1 is adjusted to 1.5-2, and 30% P204 + 70% sulfonated kerosene and the leaching solution after pH adjustment are added to the extraction equipment according to the ratio of organic phase to aqueous phase of 1:1. After shaking for 5 minutes, the mixture is allowed to stand for clarification, and the gallium-containing organic phase and the raffinate are separated;
[0070] Step S3: washing the organic phase: washing the gallium-containing organic phase obtained in step S2 with a dilute hydrochloric acid solution having a pH of 1.5 and a ratio of organic phase to aqueous phase of 10:1, shaking and mixing, standing to clarify, and separating to obtain a washing liquid and a gallium-containing organic phase, and the washing liquid is returned to step S1 for use as an acid leaching solution;
[0071] Step S4: Gallium stripping: the gallium-containing organic phase obtained in step S3 is placed in a stripping device, and 150 g / L sodium hydroxide solution is added thereto at a ratio of 2:1 between the organic phase and the aqueous phase, and a complexing agent is added at a ratio of 0.200 g / L, and stripping operation is performed, the mixture is shaken and mixed, and allowed to stand for clarification, and the lean organic phase and gallium-containing stripping solution are separated;
[0072] Step S5: Electrochemical refining of gallium: In an environment with a temperature of 35°C, the gallium-containing stripping solution obtained in step S4 is placed in the electrochemical refining chamber of the electrochemical refining device, and electrolysis and electrolysis are carried out simultaneously at a current density of 150A / m 2 In the electrolysis chamber, metallic gallium is obtained, and the electrolytic solution after electrochemical treatment is returned to step S4 for use as a stripping solution.
[0073] In this embodiment, the leaching rate of gallium contained in the gallium arsenide waste is 95.57%, and the leaching rate of arsenic is 96.46%. After the leaching solution is subjected to the extraction process, the extraction rate of gallium is 99.72%, and there is no extraction effect on arsenic. The separation rate of gallium and arsenic exceeds 99%. Using 150g / L sodium hydroxide solution as the stripping agent, the stripping rate of gallium is 100%. The amount of complexing agent added is 0.200g / L. In the electrochemical refining process, the current efficiency of gallium precipitation at the cathode is 40%. When the amount of complexing agent is insufficient, the effect of improving the current efficiency is not obvious; the gallium content in the electrolytic solution can be reduced to below 1g / L.
[0074] Example 4
[0075] like Figure 1 As shown, this embodiment provides a method for recovering gallium from gallium arsenide waste, comprising the following steps:
[0076] Step S1: controlled potential low-acid leaching: gallium arsenide waste is mixed with gallium-containing waste acid washing liquid (hydrogen ion concentration is 0.9 mol / L) at a solid-liquid ratio of 5:1, slurried at room temperature, and an oxidant (hydrogen peroxide) is added to adjust the system potential. The slurry process is greater than 0V. The temperature is maintained at 80°C and leached with stirring. During the leaching process, the potential is greater than 0.6V. The reaction is performed for 5 hours, and the leachate and leaching residue are obtained by filtration;
[0077] Step S2: Extracting gallium with P204: The pH of the leaching solution obtained in step S1 is adjusted to 1.5-2, and 30% P204 + 70% sulfonated kerosene and the leaching solution after pH adjustment are added to the extraction equipment according to the ratio of organic phase to aqueous phase of 1:1. After shaking for 5 minutes, the mixture is allowed to stand for clarification, and the gallium-containing organic phase and the raffinate are separated;
[0078] Step S3: washing the organic phase: washing the gallium-containing organic phase obtained in step S2 with a dilute hydrochloric acid solution having a pH of 1.5 and a ratio of organic phase to aqueous phase of 10:1, shaking and mixing, standing to clarify, and separating to obtain a washing liquid and a gallium-containing organic phase, and the washing liquid is returned to step S1 for use as an acid leaching solution;
[0079] Step S4: Gallium stripping: the gallium-containing organic phase obtained in step S3 is placed in a stripping device, and 150 g / L sodium hydroxide solution is added thereto at a ratio of 2:1 between the organic phase and the aqueous phase, and a complexing agent is added at a ratio of 0.250 g / L, and stripping operation is performed, the mixture is shaken and mixed, and allowed to stand for clarification, and the lean organic phase and gallium-containing stripping solution are separated;
[0080] Step S5: Electrochemical refining of gallium: In an environment with a temperature of 35°C, the gallium-containing stripping solution obtained in step S4 is placed in the electrochemical refining chamber of the electrochemical refining device, and electrolysis and electrolysis are carried out simultaneously at a current density of 150A / m 2 In the electrolysis chamber, metallic gallium is obtained, and the electrolytic solution after electrochemical treatment is returned to step S4 for use as a stripping solution.
[0081] In this embodiment, the leaching rate of gallium contained in the gallium arsenide waste is 97.00%, and the leaching rate of arsenic is 96.68%. After the leaching solution is subjected to the extraction process, the extraction rate of gallium is 99.61%, and there is no extraction effect on arsenic. The separation rate of gallium and arsenic exceeds 99%. Using 150g / L sodium hydroxide solution as a stripping agent, the stripping rate of gallium is 100%. The amount of complexing agent added is 0.250g / L. In the electrochemical refining process, the current efficiency of gallium precipitation at the cathode is 78%, and the gallium content in the electrolytic solution can be reduced to below 1g / L.
[0082] The present invention recycles gallium-containing waste pickling liquid, leaches arsenic and gallium under low-acid conditions, then separates arsenic from gallium through extraction, and finally obtains metallic gallium through electrochemical refining. The method has high resource utilization, low acid and alkali consumption, is safe and environmentally friendly, does not generate toxic gases, and has a high gallium recovery rate.
[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A gallium recovery method, characterized in that: The following steps are involved: (1) mixing a raw material containing gallium arsenide, an acid solution, and an oxidant, stirring, and leaching to obtain a leaching solution and leaching residue; (2) adjusting the pH of the leachate in step (1), extracting the leachate to obtain an organic phase and a raffinate; (3) washing the organic phase in step (2) with an acid solution to obtain an acid wash solution and a gallium-containing organic phase; (4) stripping the gallium-containing organic phase in step (3) with an alkaline solution to obtain a lean organic phase and a gallium-containing stripping solution; (5) electrochemically refining the gallium-containing stripping solution of step (4) to obtain metallic gallium; A complexing agent is added to the gallium-containing stripping solution; the complexing agent is disodium ethylenediaminetetraacetate; the amount of the complexing agent added is 0.25-0.4 g / L; In the step (1), the amount of the oxidant added is such that the potential of the leaching process is greater than 0V; In the step (1), the hydrogen ion concentration of the acid solution is 0.9 to 1.1 mol / L; the acid solution is a hydrochloric acid solution of a gallium arsenide or high-purity gallium pickling process; In the step (1), the raw material containing gallium arsenide is first mixed with an acid solution to form a slurry, and then an oxidant is added; In the step (2), the extractant is P204-sulfonated kerosene; The pickling solution in step (3) is returned to step (1) as a leaching solution.
2. The gallium recovery method according to claim 1, characterized in that: In step (1), the leaching temperature is 20 to 90°C.
3. The gallium recovery method according to claim 1, characterized in that: In step (1), the leaching time is 2 to 6 hours.
4. The gallium recovery method according to claim 1, characterized in that: In step (4), the concentration of the alkaline solution is 80 to 180 g / L.
5. The gallium recovery method according to claim 1, characterized in that: In step (5), the current density of the electrochemical refining is 100 to 200 A / m 2 .
6. The gallium recovery method according to claim 1, characterized in that: In step (5), the electrochemical refining is carried out in an electrochemical refining device; the electrochemical refining device comprises: A cathode, disposed at one end of the electrochemical refining device; an anode, disposed at the other end of the electrochemical refining device; The partition is arranged between the cathode and the anode to divide the electrochemical refining device into two spaces, namely the electrolysis chamber and the electrolysis chamber. A channel is arranged at the bottom of the partition to keep the electrolysis chamber and the electrolysis chamber connected.