A method for preparing polyacrylonitrile fiber and pulp for sealing and friction materials

Polyacrylonitrile fibers were prepared by aqueous precipitation polymerization and dry spinning process under acidic conditions, and polyacrylonitrile pulp was prepared by refining operations, which solved the thermal decomposition temperature and grasping of polyacrylonitrile fibers and pulp in the prior art. The problem of insufficient force has achieved efficient application of sealing and friction materials.

CN116043349BActive Publication Date: 2024-11-08烟台泰和兴材料科技股份有限公司
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202211669577.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-24
Publication Date
2024-11-08
Estimated Expiration
2042-12-24

AI Technical Summary

Technical Problem

The prior art is difficult to prepare polyacrylonitrile fibers and pulp suitable for sealing and friction materials, and their thermal decomposition temperature and adhesion force cannot meet the application requirements.

Method used

Aqueous phase precipitation polymerization is carried out under acidic conditions, polyacrylonitrile fibers are prepared by dry spinning process, and polyacrylonitrile fibers are prepared by refining operation. pulp, controls the number average molecular weight and fiber structure of the polymer to increase the thermal decomposition temperature and specific surface area.

Benefits of technology

The prepared polyacrylonitrile fibers and pulp have high thermal decomposition temperature and large specific surface area, which meet the application requirements of sealing and friction materials, and improve the adhesion and toughening effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116043349B_ABST
    Figure CN116043349B_ABST
Patent Text Reader

Abstract

This invention relates to the field of polyacrylonitrile pulp preparation technology, specifically to a method for preparing polyacrylonitrile fibers and pulp for sealing and friction materials. Acrylonitrile, a second monomer, a third monomer, an initiator, and a chain transfer agent are heated under acidic conditions and polymerized via aqueous precipitation to prepare a polyacrylonitrile copolymer. The polyacrylonitrile copolymer is dissolved in an organic solvent to obtain a spinning solution, which is then used to prepare polyacrylonitrile fibers using a dry spinning process. The polyacrylonitrile fibers are chopped to obtain chopped polyacrylonitrile fibers. After mixing and dispersing the chopped polyacrylonitrile fibers with water, fibrillation and further cutting of the surface of the chopped polyacrylonitrile fibers are achieved through a pulping operation. After dehydration, drying, opening, and packaging processes, polyacrylonitrile pulp is obtained. The prepared polyacrylonitrile fibers have unique internal void defects, which is beneficial for fibrillation. The pulp product has a high thermal decomposition temperature and specific surface area, making it more suitable for applications in sealing and friction materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polyacrylonitrile fiber and a pulp preparation method for sealing and friction materials, belonging to the technical field of polyacrylonitrile pulp preparation. Background Art

[0002] Polyacrylonitrile fiber is a fiber spun from the copolymer of polyacrylonitrile (PAN) or more than 85% acrylonitrile (AN) and other second and third monomers. At present, the methods for synthesizing polyacrylonitrile copolymers mainly include solution polymerization, aqueous precipitation polymerization, aqueous suspension polymerization and emulsion polymerization. Each preparation method has its own unique advantages. Different preparation methods will produce polypropylene fibers with different properties, which will directly affect downstream applications.

[0003] Polyacrylonitrile pulp is a differentiated product obtained by fibrillating polyacrylonitrile fibers. It is used as a toughening and reinforcing material in friction and sealing materials. The excellent specific surface area of ​​polyacrylonitrile pulp can optimize the processing performance of materials during material processing. At the same time, its low hardness and fluffy structure are conducive to reducing the noise of friction materials. It can show excellent dispersibility and dry and wet processing performance in rubber matrix, and can effectively replace expensive para-aramid pulp and environmentally unfriendly asbestos fibers in some fields. Polyacrylonitrile pulp suitable for sealing and friction material processing needs to meet the corresponding thermal decomposition temperature and grip after application. At present, there are almost no relevant technical reports on polyacrylonitrile pulp suitable for sealing and friction materials, which is a technical gap in this field. Commonly used sealing and friction materials include sealing plates and brake pads.

[0004] Patent application WO / 2006 / 012040A1 discloses that polyacrylonitrile fiber and para-aramid pulp are mixed in different proportions and subjected to mechanical strong shearing fibrillation (refining) treatment to prepare polyacrylonitrile / aramid mixed pulp, the longest length of which does not exceed 5 mm and the weighted average length of which does not exceed 1.3 mm. Such products are rarely used in the market and are not suitable for use in sealing and friction materials.

[0005] Chinese patent CN100395387C discloses a polyacrylonitrile pulp prepared by a precipitation method, wherein polyacrylonitrile powder with a polymerization degree of 30,000-100,000 is completely dissolved in a polar solvent, injected into a coagulation liquid to exert a strong shear force on it, and polyacrylonitrile pulp is directly precipitated. Generally, the fiber strength of pulp prepared by the precipitation method cannot provide excellent toughening and strengthening effects, and is not suitable for use in sealing and friction materials.

[0006] Chinese patent application CN104831397A discloses that polyacrylonitrile tow fibers are prepared by electrospinning technology, and polyacrylonitrile pulp fibers are obtained by cutting, dispersing, and grinding. The grinding equipment uses a specially customized screw refiner to fibrillate polyacrylonitrile fibers with a length of 3 mm. The electrospinning technology in this patent is not conducive to continuous industrial production, and the short cut length affects production efficiency.

[0007] Chinese patents CN101058896B and CN101280470B both use a method for preparing polyacrylonitrile pulp by wet spinning of two-component co-polymerization followed by fibrillation. The polymer is prepared by solution polymerization, and the spinning process adopts wet spinning. This method is the current mainstream polyacrylonitrile fiber preparation process, but there are problems of low polymer molecular weight and uneven distribution. The fiber surface produced by wet spinning is smooth, which is not conducive to the fibrillation and specific surface area improvement of polyacrylonitrile fiber during the refining process. When used in sealing and friction materials, the gripping force cannot meet the use requirements. Summary of the invention

[0008] In view of the deficiencies in the prior art, the present invention provides a method for preparing polyacrylonitrile fiber and pulp for use in sealing and friction materials. The prepared polyacrylonitrile fiber has unique hollow defects inside, which is conducive to fibrillation. The pulp product has a higher thermal decomposition temperature and specific surface area, and is more suitable for use in sealing and friction materials.

[0009] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing polyacrylonitrile fiber for sealing and friction materials, the preparation method comprising: heating acrylonitrile, a second monomer, a third monomer, an initiator and a chain transfer agent under acidic conditions, preparing a polyacrylonitrile copolymer by aqueous precipitation polymerization, dissolving the polyacrylonitrile copolymer in an organic solvent to obtain a spinning solution, and preparing the polyacrylonitrile fiber by a dry spinning process; the number average molecular weight of the polyacrylonitrile copolymer is distributed in the range of 5.0×10 5 -7.0×10 5 The thermal decomposition temperature of the polyacrylonitrile fiber is in the range of 295-325°C.

[0010] On the basis of the above technical solution, the present invention can also be improved as follows:

[0011] Furthermore, the second monomer is any one of acrylic acid, vinyl acetate, sodium propylene sulfonate and methyl acrylate, and the third monomer is any one of sodium methacrylate and itaconic acid.

[0012] Preferably, the second monomer is methyl acrylate, and the third monomer is itaconic acid.

[0013] Furthermore, the initiator is any one of organic peroxides, inorganic peroxides and azo compounds.

[0014] Furthermore, the initiator is any one of azobisisobutyl cyanide, benzoyl peroxide, benzoic acid peroxide and sodium carbonate peroxide.

[0015] Preferably, the initiator is azobisisobutyl cyanide.

[0016] Furthermore, the chain transfer agent is any one of isopropanol and mercaptan.

[0017] Furthermore, the organic solvent is any one of dimethylformamide, dimethylacetamide and dimethyl sulfoxide.

[0018] Preferably, the organic solvent is dimethyl sulfoxide.

[0019] Furthermore, in terms of weight, the acrylonitrile is 80-98 parts, the second monomer is 1-15 parts, the third monomer is 0.5-5 parts, the initiator is 0.05-0.5 parts, and the chain transfer agent is 0.1-2 parts.

[0020] Furthermore, the heating temperature is 50-70° C., and the pH of the acidic condition is 2.0-3.0.

[0021] Preferably, the heating temperature is 55-70° C., and the pH of the acidic condition is 2.6.

[0022] Furthermore, the dry spinning process consists of spinning, preheating, drawing, washing, drying and heat setting.

[0023] The present invention also discloses a method for preparing polyacrylonitrile pulp for sealing and friction materials. The preparation method comprises the following steps: the polyacrylonitrile fibers prepared by the method for preparing polyacrylonitrile fibers for sealing and friction materials of the present invention are cut into short pieces to obtain polyacrylonitrile chopped fibers; after the polyacrylonitrile chopped fibers are mixed and dispersed with water, the surfaces of the polyacrylonitrile chopped fibers are fibrillated and further cut through a pulping operation; and polyacrylonitrile pulp is obtained through dehydration, drying, opening and packaging steps.

[0024] Furthermore, the polyacrylonitrile fibers are cut into short pieces using a rotary cutter to obtain polyacrylonitrile chopped fibers, and the length of the polyacrylonitrile chopped fibers is adjusted according to demand; preferably, the length of the polyacrylonitrile chopped fibers is 3-10 mm.

[0025] Furthermore, the refining equipment used in the refining operation is a disc refiner or a cone refiner.

[0026] Furthermore, the weight ratio of the polyacrylonitrile chopped fibers to water is (0.5-8):100.

[0027] Furthermore, the polyacrylonitrile pulp has a length of 0.8-1.5 mm, a beating degree of 5-20° SR, and a specific surface area of ​​5-10 g / m 3 , the thermal decomposition temperature is 290-320℃.

[0028] The beneficial effects of the present invention are:

[0029] (1) The spinning solution is prepared by a two-step method. Water phase precipitation polymerization can prepare polyacrylonitrile copolymers with a high degree of polymerization under low temperature conditions. The polyacrylonitrile fibers spun after solvent dissolution have high strength and thermal decomposition temperature, which can meet the requirements of friction materials for the temperature resistance of polyacrylonitrile pulp, so that the obtained polyacrylonitrile pulp can meet the application requirements in sealing and friction materials.

[0030] (2) The surface of the polyacrylonitrile fiber spun by the dry spinning process is rough and cracked like bark, with cavities inside and an irregular peanut-shaped cross-section. This special structure is beneficial to the fibrillation and brooming of the polyacrylonitrile fiber during the pulping process, so that rich hairiness is produced on the surface of the polyacrylonitrile, thereby giving the polyacrylonitrile pulp a larger specific surface area, which is beneficial to improving the grip in downstream friction material applications, and achieving the effect of strengthening and toughening downstream sealing and friction materials, thereby meeting the application requirements of sealing and friction materials.

[0031] (3) In the method for preparing polyacrylonitrile fiber of the present invention, the ratio of raw materials, temperature and pH value are controlled to obtain a number average molecular weight range of 5.0×10 5 -7.0×10 5 Polyacrylonitrile polymer, this molecular weight range can obtain polyacrylonitrile pulp with a higher thermal decomposition temperature, which is more conducive to the application in downstream sealing and friction materials, and the molecular weight range is narrow, which is more conducive to the performance stability of the pulp in the application of sealing and friction materials.

[0032] (4) In the dry spinning process of the present invention, conventional oiling treatment is not performed, which is more conducive to ensuring that polyacrylonitrile pulp with a high specific surface area is obtained, and also avoids the presence of oil agents that affect the processing and application of downstream sealing material products of polyacrylonitrile pulp. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a process flow chart for preparing polyacrylonitrile fiber of the present invention;

[0034] Figure 2 This is a process flow chart for preparing polyacrylonitrile pulp of the present invention;

[0035] Figure 3 This is a microscopic diagram of polyacrylonitrile fiber;

[0036] Figure 4 This is a microscope picture of the polyacrylonitrile pulp of Example 1;

[0037] Figure 5 This is a microscope picture of the polyacrylonitrile pulp of Example 2;

[0038] Figure 6 is a thermal decomposition temperature curve of polyacrylonitrile pulp of Example 2;

[0039] Figure 7 This is a thermal decomposition temperature curve of the polyacrylonitrile pulp of Example 6. DETAILED DESCRIPTION

[0040] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.

[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.

[0042] like Figure 1 As shown, a method for preparing polyacrylonitrile fiber for sealing and friction materials is provided, wherein the preparation method comprises: heating acrylonitrile (first monomer), second monomer, third monomer, initiator and chain transfer agent under acidic conditions, preparing polyacrylonitrile copolymer by aqueous precipitation polymerization, dissolving the polyacrylonitrile copolymer in an organic solvent to obtain spinning solution, and preparing polyacrylonitrile fiber by dry spinning process; the number average molecular weight of the polyacrylonitrile copolymer is distributed in the range of 5.0×10 5 -7.0×10 5 The thermal decomposition temperature of the polyacrylonitrile fiber is in the range of 295-325°C.

[0043] The second monomer is any one of acrylic acid, vinyl acetate, sodium propylene sulfonate and methyl acrylate, and the third monomer is any one of sodium methacrylate and itaconic acid.

[0044] The initiator is any one of organic peroxide, inorganic peroxide and azo compound.

[0045] The initiator is any one of azobisisobutyl cyanide, benzoyl peroxide, benzoic acid peroxide and sodium carbonate peroxide.

[0046] The chain transfer agent is any one of isopropanol and mercaptan.

[0047] The organic solvent is any one of dimethylformamide, dimethylacetamide and dimethyl sulfoxide.

[0048] In terms of weight, the acrylonitrile is 80-98 parts, the second monomer is 1-15 parts, the third monomer is 0.5-5 parts, the initiator is 0.05-0.5 parts, and the chain transfer agent is 0.1-2 parts.

[0049] The heating temperature is 50-70° C., and the pH of the acidic condition is 2.0-3.0. In the embodiment of the present invention, the pH of the polymerization system is adjusted by adding hydrochloric acid with a mass concentration of 10%.

[0050] The dry spinning process is composed of spinning, preheating, drawing, washing, drying and heat setting. Since polyacrylonitrile pulp is mainly used in the field of friction and sealing materials, no oiling treatment is performed during the spinning process to avoid adverse effects on downstream products of the pulp.

[0051] like Figure 2 As shown, a method for preparing polyacrylonitrile pulp for sealing and friction materials is provided, wherein the preparation method comprises: cutting the polyacrylonitrile fibers into short pieces to obtain polyacrylonitrile chopped fibers, mixing and dispersing the polyacrylonitrile chopped fibers with water, performing a pulping operation to achieve fibrillation of the surface of the polyacrylonitrile chopped fibers and further cutting, and performing dehydration, drying, opening and packaging processes to obtain polyacrylonitrile pulp. The microstructure of the polyacrylonitrile fibers is as follows: Figure 3 shown.

[0052] The polyacrylonitrile fibers are cut into short pieces using a rotary cutter to obtain polyacrylonitrile chopped fibers. The length of the polyacrylonitrile chopped fibers is adjusted according to demand; the length of the polyacrylonitrile chopped fibers is 3-10 mm.

[0053] The refining equipment used in the refining operation is a disc refiner or a cone refiner.

[0054] The weight ratio of the polyacrylonitrile chopped fibers to water is (0.5-8):100.

[0055] The polyacrylonitrile pulp has a length of 0.8-1.5 mm, a beating degree of 5-20°SR, and a specific surface area of ​​5-10 g / m 3 , the thermal decomposition temperature is 290-320℃.

[0056] Example 1

[0057] Acrylonitrile, methyl acrylate, itaconic acid, azobisisobutyl cyanide and mercaptan were sequentially injected into a polymerization kettle in a weight ratio of 95:2.8:1:0.2:1, and an aqueous phase precipitation polymerization reaction was carried out at pH = 2.6 and a polymerization temperature of 65°C. After termination reaction, removal of monomers and dehydration treatment, a polymer filter cake was obtained. The number average molecular weight of the polymer cake was 6.5×10 5 DMSO and polymer filter cake were dissolved in a weight ratio of 100:22, and polyacrylonitrile fibers were spun by dry spinning after degassing. The polyacrylonitrile fiber filaments were cut into 6±0.5mm short fibers by a cutting machine. The thermal decomposition temperature of the polyacrylonitrile fiber was 315℃ after testing.

[0058] The polyacrylonitrile chopped fibers and water are dispersed in a pulping tank at a weight ratio of 3:100. The fibers are fibrillated and refined using a disc refiner. After dehydration, drying, opening and packaging, polyacrylonitrile pulp products are obtained. Microscope images of polyacrylonitrile pulp are shown below. Figure 4 As shown, from Figure 4 It can be seen that the surface of the polyacrylonitrile pulp prepared in this embodiment contains more hairiness, which is beneficial to increasing the specific surface area of ​​the polyacrylonitrile pulp.

[0059] The product specifications of polyacrylonitrile pulp are as follows: fiber length is 1.126 mm, beating degree is 12°SR, specific surface area is 6.59 g / m 3 , the thermal decomposition temperature is 312℃.

[0060] Example 2

[0061] Acrylonitrile, methyl acrylate, itaconic acid, azobisisobutyl cyanide and mercaptan were sequentially injected into a polymerization kettle in a weight ratio of 90:6.3:2:0.2:1.5, and an aqueous phase precipitation polymerization reaction was carried out at pH = 2.6 and a polymerization temperature of 65°C. After termination reaction, removal of monomers and dehydration treatment, a polymer filter cake was obtained. The number average molecular weight of the polymer cake was 5.4×10 5 Dimethyl sulfoxide and polymer filter cake were dissolved in a weight ratio of 100:20, and polyacrylonitrile fibers were spun by dry spinning after degassing. The polyacrylonitrile fiber filaments were cut into 6±0.5mm short fibers by a cutting machine. After testing, the thermal decomposition temperature of the polyacrylonitrile fiber was 296℃.

[0062] The polyacrylonitrile chopped fibers and water are dispersed in a pulping tank at a weight ratio of 3:100. The fibers are fibrillated and refined using a disc refiner. After dehydration, drying, opening and packaging, polyacrylonitrile pulp products are obtained. Microscope images of polyacrylonitrile pulp are shown below. Figure 5 As shown, from Figure 5It can be seen that the surface of the polyacrylonitrile pulp prepared in this embodiment contains more hairiness, which is beneficial to increasing the specific surface area of ​​the polyacrylonitrile pulp.

[0063] The product indicators of polyacrylonitrile pulp are as follows: fiber length is 1.163mm, beating degree is 11.5°SR, specific surface area is 7.06g / m 3 The thermal decomposition temperature is 292.3℃, and the thermal decomposition temperature of polyacrylonitrile pulp is Figure 6 shown.

[0064] Example 3

[0065] Acrylonitrile, methyl acrylate, itaconic acid, azobisisobutyl cyanide and mercaptan were sequentially injected into a polymerization kettle in a weight ratio of 96:2:0.7:0.05:1.25, and an aqueous phase precipitation polymerization reaction was carried out at pH = 2.6 and a polymerization temperature of 67 ° C. After termination reaction, de-monomer removal and dehydration treatment, a polymer filter cake was obtained. The number average molecular weight of the polymer cake was 6.78×10 5 DMSO and polymer filter cake were dissolved in a weight ratio of 100:22, and polyacrylonitrile fibers were spun by dry spinning after degassing. The polyacrylonitrile fiber filaments were cut into 6±0.5mm short fibers by a cutting machine. The thermal decomposition temperature of the polyacrylonitrile fiber was 316℃ after testing.

[0066] The polyacrylonitrile short-cut fibers and water are dispersed in a pulping tank at a weight ratio of 3:100, and the fibers are fibrillated and refined using a disc pulping machine. After dehydration, drying, opening and packaging, polyacrylonitrile pulp products are obtained. The polyacrylonitrile pulp product indicators are as follows: fiber length is 1.098mm, beating degree is 14.5°SR, specific surface area is 7.56g / m 3 , the thermal decomposition temperature is 312.5℃.

[0067] Example 4

[0068] Acrylonitrile, methyl acrylate, itaconic acid, azobisisobutyl cyanide and isopropanol were sequentially injected into a polymerization kettle in a weight ratio of 96:2.2:1:0.5:0.75, and an aqueous phase precipitation polymerization reaction was carried out at pH = 2.6 and a polymerization temperature of 65 ° C. After termination reaction, de-monomer removal and dehydration treatment, a polymer filter cake was obtained. After testing, the number average molecular weight of the polymer cake was 6.5×10 5 Dimethyl sulfoxide and polymer filter cake were dissolved in a weight ratio of 100:22, and polyacrylonitrile fibers were spun by dry spinning after degassing. The polyacrylonitrile fiber filaments were cut into 6±0.5mm short fibers by a cutting machine. After testing, the thermal decomposition temperature of the polyacrylonitrile fiber was 315°C.

[0069] The polyacrylonitrile short-cut fibers and water are dispersed in a pulping tank at a weight ratio of 3:100, and the fibers are fibrillated and refined using a disc pulping machine. After dehydration, drying, opening and packaging, polyacrylonitrile pulp products are obtained. The polyacrylonitrile pulp product indicators are as follows: fiber length is 1.289 mm, beating degree is 10.5°SR, specific surface area is 5.68 g / m 3 , the thermal decomposition temperature is 311℃.

[0070] Example 5

[0071] Acrylonitrile, methyl acrylate, itaconic acid, azobisisobutyl cyanide and mercaptan were sequentially injected into a polymerization kettle in a weight ratio of 96:2.7:1:0.15:0.15, and an aqueous phase precipitation polymerization reaction was carried out at pH = 2.6 and a polymerization temperature of 65°C. After termination reaction, de-monomer removal and dehydration treatment, a polymer filter cake was obtained. The number average molecular weight of the polymer cake was 6.5×10 5 DMSO and polymer filter cake were dissolved in a weight ratio of 100:22, and polyacrylonitrile fibers were spun by dry spinning after degassing. The polyacrylonitrile fiber filaments were cut into 6±0.5mm short fibers by a cutting machine. The thermal decomposition temperature of the polyacrylonitrile fiber was 315℃ after testing.

[0072] The polyacrylonitrile short-cut fibers and water are dispersed in a pulping tank at a weight ratio of 4:100, and the fibers are fibrillated and refined using a disc pulping machine. After dehydration, drying, opening and packaging, polyacrylonitrile pulp products are obtained. The polyacrylonitrile pulp product indicators are as follows: fiber length is 1.126mm, beating degree is 12°SR, specific surface area is 6.59g / m 3 , the thermal decomposition temperature is 312℃.

[0073] Example 6

[0074] Acrylonitrile, methyl acrylate, itaconic acid, azobisisobutyl cyanide and isopropanol were sequentially injected into a polymerization kettle in a weight ratio of 85:10.5:3:0.3:1.2, and an aqueous phase precipitation polymerization reaction was carried out at pH = 2.0 and a polymerization temperature of 62°C. After termination reaction, removal of monomers and dehydration treatment, a polymer filter cake was obtained. The number average molecular weight of the polymer cake was 5.25×10 5 DMSO and polymer filter cake were dissolved in a weight ratio of 100:22, and polyacrylonitrile fibers were spun by dry spinning after degassing. The polyacrylonitrile fiber filaments were cut into 6±0.5mm short fibers by a cutting machine. The thermal decomposition temperature of the polyacrylonitrile fiber was 302℃ after testing.

[0075] The polyacrylonitrile short-cut fibers and water are dispersed in a pulping tank at a weight ratio of 2:100, and the fibers are fibrillated and refined using a disc pulping machine. After dehydration, drying, opening and packaging, polyacrylonitrile pulp products are obtained. The polyacrylonitrile pulp product indicators are as follows: fiber length is 0.896 mm, beating degree is 15°SR, specific surface area is 9.59 g / m 3 The thermal decomposition temperature is 295.1℃, and the thermal decomposition temperature of polyacrylonitrile pulp is Figure 7 shown.

[0076] Example 7

[0077] Acrylonitrile, acrylic acid, sodium methacrylate, benzoyl peroxide and mercaptan were sequentially injected into a polymerization kettle at a weight ratio of 98:1:0.5:0.1:0.4, and an aqueous phase precipitation polymerization reaction was carried out at a pH of 3.0 and a polymerization temperature of 70°C. After termination reaction, removal of monomers and dehydration treatment, a polymer filter cake was obtained. The number average molecular weight of the polymer cake was 6.2×10 5 Dimethylformamide and polymer filter cake were dissolved in a weight ratio of 100:20, and polyacrylonitrile fibers were spun by dry spinning after degassing. The polyacrylonitrile fiber filaments were cut into 4±0.5mm short fibers by a cutting machine. After testing, the thermal decomposition temperature of the polyacrylonitrile fiber was 307℃.

[0078] The polyacrylonitrile short-cut fibers and water are dispersed in a pulping tank at a weight ratio of 8:100, and the fibers are fibrillated and refined using a disc refiner. The polyacrylonitrile pulp product is obtained through dehydration, drying, opening and packaging processes.

[0079] The product specifications of polyacrylonitrile pulp are as follows: fiber length is 0.985 mm, beating degree is 14°SR, specific surface area is 5.63 g / m 3 , the thermal decomposition temperature is 301℃.

[0080] Example 8

[0081] Acrylonitrile, vinyl acetate, sodium methacrylate, azobisisobutyl cyanide and isopropanol were sequentially injected into a polymerization kettle at a weight ratio of 80:15:5:0.5:2, and an aqueous phase precipitation polymerization reaction was carried out at pH = 2.3 and a polymerization temperature of 55°C. After termination reaction, removal of monomers and dehydration treatment, a polymer filter cake was obtained. The number average molecular weight of the polymer cake was 5.1×10 5 Dimethylacetamide and polymer filter cake were dissolved in a weight ratio of 100:20, and polyacrylonitrile fibers were spun by dry spinning after degassing. The polyacrylonitrile fiber filaments were cut into 5±0.5mm short fibers by a cutting machine. After testing, the thermal decomposition temperature of the polyacrylonitrile fiber was 292℃.

[0082] The polyacrylonitrile short-cut fibers and water are dispersed in a pulping tank at a weight ratio of 0.5:100, and the fibers are fibrillated and refined using a disc refiner. The polyacrylonitrile pulp product is obtained through dehydration, drying, opening and packaging processes.

[0083] The product indicators of polyacrylonitrile pulp are as follows: fiber length is 1.203mm, beating degree is 5.32°SR, specific surface area is 6.52g / m 3 , the thermal decomposition temperature is 290℃.

[0084] Comparative Example 1

[0085] The polyacrylonitrile pulp was prepared in the same manner as in Example 1, except that during the preparation of the polyacrylonitrile polymer, the pH in the polymerization reactor was adjusted to 4.0 by using hydrochloric acid.

[0086] The polymer filter cake prepared in this comparative example was tested and its number average molecular weight was 4.0×10 5 The thermal decomposition temperature of polyacrylonitrile fiber is 275℃.

[0087] The final polyacrylonitrile pulp product indicators are as follows: fiber length is 1.121 mm, beating degree is 9°SR, specific surface area is 5.23 g / m 3 , the thermal decomposition temperature is 272℃.

[0088] Comparative Example 2

[0089] The polyacrylonitrile pulp was prepared in the same manner as in Example 1, except that during the preparation of the polyacrylonitrile polymer, the pH in the polymerization reactor was adjusted to 1.5 by using hydrochloric acid.

[0090] The polymer filter cake prepared in this comparative example was tested and its number average molecular weight was 4.7×10 5 , and the molecular weight distribution becomes wider, and the production stability is poor. The thermal decomposition temperature of polyacrylonitrile fiber is 281℃.

[0091] The final polyacrylonitrile pulp product indicators are as follows: fiber length is 1.123 mm, beating degree is 9.5°SR, specific surface area is 5.34 g / m 3 , the thermal decomposition temperature is 276℃.

[0092] It can be seen from the experimental data of Example 1 and Comparative Examples 1 and 2 that when the pH in the polymerization kettle is too low or too high, the molecular weight of the obtained polymer is low, and the thermal decomposition temperature of the spun polyacrylonitrile pulp is low, which cannot meet the application requirements of sealing and friction materials. The polyacrylonitrile pulp prepared within the pH range described in the present invention has a higher thermal decomposition temperature, which is more conducive to the application of polypropylene pulp in sealing and friction materials.

[0093] Comparative Example 3

[0094] The polyacrylonitrile pulp was prepared in the same manner as in Example 1, except that the polyacrylonitrile fiber was spun by a wet spinning process.

[0095] The final polyacrylonitrile pulp product specifications are as follows: fiber length is 1.125 mm, beating degree is 11° SR, specific surface area is 3.87 g / m 3 , the thermal decomposition temperature is 305℃.

[0096] It can be seen from the experimental data of Example 1 and Comparative Example 3 that when the wet spinning process is used for polyacrylonitrile fiber, the specific surface area of ​​the prepared polyacrylonitrile pulp is significantly reduced. When used in friction materials, the gripping force cannot meet customer requirements. However, the dry spinning process described in the present invention is used to prepare the polyacrylonitrile pulp, which has a higher specific surface area and exhibits a higher gripping force when used. Because the surface of the polyacrylonitrile fiber obtained by the dry spinning process is cracked and rough bark-like, there are holes inside, and the cross-section is irregular peanut-shaped, this special structure is conducive to the fibrillation and brooming of the polyacrylonitrile fiber during the pulping process, so that the polyacrylonitrile surface produces abundant hairiness, so that the polyacrylonitrile pulp has a larger specific surface area, which is conducive to the improvement of gripping force in downstream applications, while the surface of the polyacrylonitrile fiber prepared by the wet spinning process is smooth and has no hairiness structure, and ultimately polyacrylonitrile pulp with a larger specific surface area cannot be obtained.

[0097] Comparative Example 4

[0098] The same method as in Example 1 was adopted to prepare polyacrylonitrile pulp, except that an oiling treatment operation was added during the dry spinning process.

[0099] The final polyacrylonitrile pulp product specifications are as follows: fiber length is 1.124 mm, beating degree is 12°SR, specific surface area is 4.97 g / m 3 , the thermal decomposition temperature is 302℃.

[0100] The polyacrylonitrile pulp obtained in Examples 1 to 8 has a good application effect in sealing plates and brake pads, meeting the performance requirements such as thermal decomposition temperature, strength, grip, sealing and toughness. However, when the polypropylene pulp prepared in Comparative Example 4 is used in a sealing plate, a poor sealing effect occurs because Comparative Example 4 adds an oiling operation during the preparation of the polyacrylonitrile pulp, and the polyacrylonitrile pulp contains an oil agent, and the presence of the oil agent will affect the sealing of the sealing material.

[0101] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0102] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.

Claims

1. A method for preparing polyacrylonitrile fiber for sealing and friction materials, It is characterized in that The preparation method comprises the following steps: acrylonitrile, a second monomer, a third monomer, an initiator and a chain transfer agent are heated under acidic conditions to prepare a polyacrylonitrile copolymer by aqueous precipitation polymerization; the polyacrylonitrile copolymer is dissolved in an organic solvent to obtain a spinning solution; and the polyacrylonitrile fiber is prepared by a dry spinning process; the number average molecular weight of the polyacrylonitrile copolymer is distributed in the range of 5.0×10 5 -7.0×10 5 , the thermal decomposition temperature range of the polyacrylonitrile fiber is 295-325°C; The second monomer is any one of acrylic acid, vinyl acetate, sodium propylene sulfonate and methyl acrylate, and the third monomer is any one of sodium methacrylate and itaconic acid; In terms of weight, the acrylonitrile is 80-98 parts, the second monomer is 1-15 parts, the third monomer is 0.5-5 parts, the initiator is 0.05-0.5 parts, and the chain transfer agent is 0.1-2 parts; The heating temperature is 50-70°C, and the pH of the acidic condition is 2.0-3.0; The dry spinning process consists of spinning, preheating, drawing, washing, drying and heat setting.

2. A method for preparing polyacrylonitrile fiber for sealing and friction materials according to claim 1, It is characterized in that The initiator is any one of organic peroxide, inorganic peroxide and azo compound; the chain transfer agent is any one of isopropanol and mercaptan.

3. The method for preparing polyacrylonitrile fiber for sealing and friction materials according to claim 1, It is characterized in that The organic solvent is any one of dimethylformamide, dimethylacetamide and dimethyl sulfoxide.

4. A method for preparing polyacrylonitrile pulp for sealing and friction materials, It is characterized in that The preparation method comprises: cutting the polyacrylonitrile fibers prepared by the method for preparing polyacrylonitrile fibers for sealing and friction materials according to any one of claims 1 to 3 into short pieces to obtain polyacrylonitrile chopped fibers; after the polyacrylonitrile chopped fibers are mixed and dispersed with water, the surfaces of the polyacrylonitrile chopped fibers are fibrillated and further cut through a pulping process; and after dehydration, drying, opening and packaging steps, polyacrylonitrile pulp is obtained.

5. A method for preparing polyacrylonitrile pulp for sealing and friction materials according to claim 4, It is characterized in that The weight ratio of the polyacrylonitrile chopped fibers to water is (0.5-8):

100.

6. A method for preparing polyacrylonitrile pulp for sealing and friction materials according to claim 4, It is characterized in that The polyacrylonitrile pulp has a length of 0.8-1.5 mm, a beating degree of 5-20°SR, and a specific surface area of ​​5-10 g / m 3 , the thermal decomposition temperature is 290-320℃.

Citation Information

Patent Citations

  • Method for preparing polyacrylonitrile pomace

    CN100395387C

  • Preparation of polyacrylonitrile pulp-shape fibre

    CN101058896B

  • Method for continuously producing polyacryl-nitrile pulp-like fibre

    CN101280470B

  • Preparation method of acrylon pulp

    CN104831397A

  • Acrylic and para-aramid pulp and processes of making same

    WO2006012040A1