By using components such as positive monovalent silver, ammonia, C1-C3 alcohols, polyethylenimine and SiO2 colloidal particles in the fabric antibacterial finishing solution, combined with the use of cross-linking agents, the problem of inconsistent color of silver ion fabrics in the existing technology is solved. Stability problem, significantly improving the color stability and antibacterial effect of the fabric.
Patent Information
- Application Number
- CN202310060597.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-17
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-01-17
AI Technical Summary
The existing silver ion fabric antibacterial finishing solution causes unstable fabric color and serious discoloration problems.
Use a fabric antibacterial finishing working fluid containing positive monovalent silver, ammonia, C1-C3 alcohol, polyethyleneimine, SiO2 colloidal particles and cross-linking agent. The color stability of the fabric can be improved by adjusting the proportion of components. Alcohol and polyethyleneimine are used. The mutual promotion between amines reduces the degree of discoloration of antibacterial fabrics.
It significantly improves the color stability of antibacterial fabrics, reduces the degree of discoloration, and achieves long-term color maintenance of fabrics after antibacterial finishing.
Smart Images

Figure BDA0004061170940000061 
Figure BDA0004061170940000071 
Figure BDA0004061170940000091
Abstract
Description
Technical Field
[0001] The invention relates to a silver ion fabric antibacterial finishing working liquid and a method for producing antibacterial fabric. Background Art
[0002] As people pay more attention to healthy living, mattress fabrics with antibacterial properties have begun to receive widespread attention. Silver ions have antibacterial ability and are often used in the prior art to modify fabrics for antibacterial properties. For example, CN115302874A discloses a blended antibacterial fabric containing silver ion-modified fibers that utilizes the antibacterial properties of silver ions, CN217744176U discloses a deodorizing antibacterial towel using silver-containing fabrics, and CN115287896A invents a method for preparing an antibacterial biomass-based fabric using the antibacterial properties of silver ions. However, silver ion-containing fabrics generally have the problem of poor color stability. Summary of the invention
[0003] One of the technical problems to be solved by the present invention is the problem that the existing silver ion antibacterial finishing working liquid for fabrics causes unstable fabric color when used for antibacterial finishing of fabrics, and a new antibacterial finishing working liquid for fabrics is provided. The working liquid is used for fabric finishing and has the characteristic of good fabric color stability.
[0004] To solve one of the above technical problems, the technical solution of the present invention is as follows:
[0005] Antimicrobial finishing solution for fabrics, comprising, by weight:
[0006] (a) Ag, 1 part;
[0007] (b) ammonia, 3 to 10 parts;
[0008] (c) C1-C3 alcohol, 0-80 parts;
[0009] (d) polyethyleneimine, 0 to 80 parts;
[0010] (e) SiO2 colloid particles, 0 to 80 parts;
[0011] (f) a cross-linking agent, 0 to 200 parts, more preferably 50 to 200 parts;
[0012] (g) water, so that the total number of parts of the antibacterial finishing working solution for fabrics is 10,000 to 50,000 parts.
[0013] By way of non-limiting example, ammonia is 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts, and so on.
[0014] In the above technical solution, the alcohol is preferably greater than 0 parts and less than 80 parts, more preferably 20 to 80 parts.
[0015] C1-C3 alcohols reduce the severity of color change of antibacterial fabrics after antibacterial finishing and improve the color stability of antibacterial fabrics.
[0016] As non-limiting examples, the C1-C3 alcohol is 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, etc. For comparison only, 10 parts, 30 parts or 40 parts are generally used in the embodiments and comparative examples.
[0017] In the above technical solution, the alcohol includes at least one selected from the group consisting of methanol, ethanol, ethylene glycol, n-propanol, isopropanol and glycerol.
[0018] In particular, the alcohol includes ethanol and glycerol at the same time. We found that ethanol as a monohydric alcohol and glycerol as a trihydric alcohol have a mutually promoting effect in reducing the color change degree of the antibacterial fabric or improving the color stability of the antibacterial fabric. However, this promoting effect has not been found between different monohydric alcohols, between monohydric alcohols and dihydric alcohols, and between different dihydric alcohols according to the relevant work we have carried out. At this time, the weight ratio of glycerol to ethanol is not particularly limited, for example but not limited to 0.1 to 10. As a non-limiting example of a more condensed body, the weight ratio of glycerol to ethanol is 0.2, 0.4, 0.8, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, etc.
[0019] In the above technical solution, the polyethyleneimine is preferably greater than 0 parts and less than 80 parts, and more preferably 10 to 40 parts.
[0020] As a non-limiting example, polyethyleneimine is 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, etc. For comparison only, the embodiments and comparative examples generally use 24 parts or 58 parts.
[0021] In the above technical scheme, the weight average molecular weight of polyethyleneimine (measured by light scattering method) is preferably 500-10,000, for example but not limited to 600, 800, 1,000, 1,500, 2,000, 2,500, 3,000, 3,500, 4,000, 4,500, 5,000, 8,000, etc., more preferably 500-5,000. In comparison, the molecular weight is too large, and the effect of improving the color stability of the antibacterial fabric becomes insignificant.
[0022] In the above technical solution, in the polyethyleneimine molecule, the ratio of primary amino group: secondary amino group: tertiary amino group is preferably 1:a:b, wherein a is 0.8-1.2 and b is 0.4-0.8.
[0023] As non-limiting examples, for example but not limited to, a is 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, etc.
[0024] As non-limiting examples, for example but not limited to, b is 0.45, 0.50, 0.55, 0.6, 0.65, 0.7, 0.75, etc.
[0025] Polyethyleneimine can be obtained from commercial channels. For example, the specifications of polyethyleneimine from BASF are:
[0026] LUPASOL FG (weight average molecular weight: 800, a: 0.82, b: 0.53),
[0027] LUPASOL G 20wfr (weight average molecular weight is 1300, a is 0.91, b is 0.64,),
[0028] LUPASOL PR8515 (weight average molecular weight is 2000, a is 0.92, b is 0.70),
[0029] LUPASOL FC (weight average molecular weight: 800, a: 0.86, b: 0.42, containing 50% water),
[0030] LUPASOL G 20 (weight average molecular weight 1300, a 0.91, b 0.64, contains 50% water),
[0031] LUPASOL G 35 (weight average molecular weight 2000, a 0.94, b 0.67, contains 50% water),
[0032] LUPASOL G 100 (weight average molecular weight: 5000, a: 1.05, b: 0.76, containing 50% water).
[0033] In the above technical solution, the SiO2 colloid particles are preferably greater than 0 parts and more than 80 parts, and more preferably 10 to 50 parts.
[0034] As a non-limiting example, the SiO2 colloid particles are 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, etc. For comparison only, 34 parts or 58 parts are generally used in the embodiments and comparative examples.
[0035] The use of SiO2 colloid particles reduces the color change degree of the antibacterial fabric and improves the color stability of the antibacterial fabric.
[0036] The composition more preferably includes both polyethyleneimine and SiO2 colloid particles, and the polyethyleneimine and SiO2 colloid particles have a mutually promoting effect in reducing the color change degree of the antibacterial fabric or improving the color stability of the antibacterial fabric. At this time, the weight ratio of polyethyleneimine to SiO2 colloid particles is not particularly limited, and comparable mutually promoting effects can be achieved, for example but not limited to the weight ratio of polyethyleneimine to SiO2 colloid particles is 0.1 to 10, and more specific non-limiting examples are 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, etc.
[0037] In the above technical scheme, the crosslinking agent is not an essential component, and the comparable technical effects of the present invention can be achieved with or without the addition, so the amount of the crosslinking agent can be 0 parts, but the crosslinking agent can increase the bonding strength between Ag and the fabric during the process of fabric finishing with the antibacterial finishing liquid for fabrics, so the crosslinking agent is preferably greater than 0 parts and less than 200 parts, and more preferably 50 to 200 parts. The crosslinking agent can be a thermal crosslinking type crosslinking agent or a photocrosslinking type crosslinking agent. As the name implies, the thermal crosslinking type crosslinking agent is a crosslinking agent that forms a three-dimensional network structure through a heat treatment process to play a crosslinking role, while the photocrosslinking agent is a crosslinking agent that forms a three-dimensional network structure through a light treatment process to play a crosslinking role. Non-limiting examples of the heat-induced cross-linking cross-linking agent that can be used in the present invention include, but are not limited to, polyacrylic acid cross-linking agents (i.e., cross-linking agents with polyacrylic acid as the skeleton in the molecular structure of the cross-linking agent), polyurethane cross-linking agents (i.e., cross-linking agents with polyurethane as the skeleton in the molecular structure of the cross-linking agent), amide-formaldehyde cross-linking agents (i.e., cross-linking agents with amide-formaldehyde resin as the skeleton in the molecular structure of the cross-linking agent), urea-formaldehyde cross-linking agents (i.e., cross-linking agents with urea-formaldehyde resin as the skeleton in the molecular structure of the cross-linking agent), and polycarboxylic acid cross-linking agents.
[0038] Only for the same period of time, the cross-linking agent in the embodiment and the comparative example generally uses a heat-induced cross-linking type cross-linking agent. Further, also only for the same period of time, the heat-induced cross-linking type cross-linking agent generally used in the embodiment and the comparative example is the JYK FIX-DI cross-linking agent of Shanghai Jieyikang Chemical Technology Co., Ltd. JYK FIX-DI is the above-mentioned polyurethane cross-linking agent (that is, a cross-linking agent with polyurethane as the skeleton in the molecular structure of the cross-linking agent). It is suitable for preparing textile coatings and foam coating slurries; it can improve wet friction fastness when used in coating printing slurries. It can also be used in functional additives to improve the washing resistance of functional finishing. JYKFIX-DI has good compatibility with various functional additives and can be mixed with deionized water in any proportion. The conditions for heat treatment cross-linking can be 130-150°C for 2-5 minutes. As a general rule, the higher the temperature, the shorter the required heat treatment time. Based on this rule, those skilled in the art can reasonably adjust the heat treatment temperature and heat treatment time, and can achieve acceptable technical effects without having to pay creative labor.
[0039] In the above technical solution, as a non-limiting example, the amount of the cross-linking agent is 30 parts, 40 parts, 50 parts, 60 parts, 70 parts, 80 parts, 90 parts, 100 parts, 110 parts, 120 parts, 130 parts, 140 parts, 150 parts, 160 parts, 170 parts, 180 parts, 190 parts, etc. For comparison only, the amount of the cross-linking agent generally used in the embodiments and comparative examples is 100 parts.
[0040] As a non-limiting example, component (g) water makes the total number of parts of the antibacterial finishing working solution for fabrics be 11000 parts, 12000 parts, 13000 parts, 14000 parts, 15000 parts, 16000 parts, 17000 parts, 18000 parts, 19000 parts, 20000 parts, 21000 parts, 22000 parts, 23000 parts, 24000 parts, 25000 parts, 26000 parts, 27000 parts, 28000 parts, 29000 parts, 30000 parts, 31000 parts, 32000 parts, 33000 parts, 34000 parts, 35000 parts, 36000 parts, 37000 parts, 38000 parts, 39000 parts, 40000 parts, 41000 parts, 42000 parts, 43000 parts, 44000 parts, 45000 parts, 46000 parts, 47000 parts, 48000 parts, 49000 parts, 50000 parts, 51000 parts, 52000 parts, 53000 parts, 54000 parts, 55000 parts, 56000 parts, 57000 parts, 58000 parts, 59000 parts, 60000 parts, 61000 parts, 62000 parts, 63000 parts, 64000 parts, 65000 parts, 66000 parts, 67000 parts, 68000 parts, 69000 parts, 71000 000 parts, 000 parts, 000 parts, 01000 parts, 02000 parts, 03000 parts, 04000 parts, 05000 parts, 06000 parts, 07000 parts, 08000 parts, 09000 parts, 10000 parts, 11000 parts, 12000 parts, 13000 parts, 14000 parts, 15000 parts, 16000 parts, 17000 parts, 18000 parts, 19000 parts and the like, more preferably 15000 to 30000 parts. Only for comparison, the embodiments of the present invention and the comparative examples generally adopt 20000 parts.
[0041] The technical key of the present invention is the selection of the components of the antibacterial finishing working liquid. In the case of disclosing the components of the antibacterial finishing working liquid, there is no special restriction on the preparation method of the antibacterial finishing working liquid, and comparable technical effects can be achieved without creative labor. As a non-limiting example only, the preparation method of the antibacterial finishing working liquid includes:
[0042] (1) obtaining a liquid mixture 1 with water as a dispersing solvent and comprising ammonia, optionally C1-C3 alcohol, optionally polyethyleneimine and optionally SiO2 colloid particles;
[0043] (2) obtaining an aqueous solution of a monovalent silver compound;
[0044] (3) adding an aqueous solution of a positive monovalent silver compound to the liquid mixture 1;
[0045] (4) Add a cross-linking agent when necessary.
[0046] As for the water required in the antibacterial finishing working solution, those skilled in the art understand that all the water can be used in step (1) and step (2); or part of the water can be used in step (1) and step (2). Before adding the cross-linking agent in step (4), the mixture 1 obtained in step (3) can be diluted with water first or not. The cross-linking agent can be added by diluting the cross-linking agent with water or directly. However, in order to accurately realize the total number of portions of the antibacterial finishing working solution, the total amount of water used in the aforementioned steps (1) to (4) should be less than the total amount of water required by the formula, and the insufficient water is supplemented in the last step, etc. In this regard, comparable technical effects can be achieved without creative labor.
[0047] In the above technical solution, preferably, ammonia is used as the raw material of the liquid mixture 1 in the form of ammonia water, and / or SiO2 colloid particles are used as the raw material of the liquid mixture 1 in the form of silica sol.
[0048] In order to improve the storage stability of silica sol, there are two major types of commercially available silica sols, namely alkaline silica sol (that is, silica sol with a small amount of alkaline substance added as a stabilizer, common ones are sodium-stabilized silica sol, potassium-stabilized silica sol, and ammonia-stabilized silica sol) and acidic silica sol. Both types of silica sol can be used and can achieve comparable technical effects. However, since acidic silica sol is acidic, it will consume ammonia in the composition. From the perspective of saving material consumption, alkaline silica sol is preferred.
[0049] In the above technical solution, the alkaline silica sol is preferably selected from sodium-stabilized silica sol, potassium-stabilized silica sol or ammonia-stabilized silica sol.
[0050] For comparison only, the silica sol used in the examples is Levasil CS400-222 silica sol produced by Nouryon, in which the silica sol has a silicon dioxide content of 40% by weight, a pH of 9.8, and is a sodium-stabilized silica sol with a Na2O content of 0.42w%.
[0051] The second technical problem to be solved by the present invention is to provide a method for manufacturing the above antibacterial fabric, and the technical solution is:
[0052] A method for manufacturing an antibacterial fabric, comprising:
[0053] (i) contacting a raw fabric with the antibacterial finishing working solution for fabric described in any one of the above technical solutions to obtain a liquid-containing fabric a;
[0054] (ii) drying to obtain fabric b;
[0055] (iii) baking to obtain antibacterial fabric.
[0056] In the above technical solution, the contacting method in step (i) is not particularly limited, and can be contacting by dipping, contacting by spraying, or contacting by rolling.
[0057] In the above technical scheme, for example only, the contact method in step (i) is immersion contact, and there is no special restriction on the contact time. As long as the contact between the fabric deodorant finishing working liquid and the fabric reaches or basically reaches equilibrium, extending the contact time has no special effect on the technical effect. However, too long a contact time will increase the time cost of production, while too short a contact time will affect the loading amount of the photocatalyst. Based on the above contact time principle, technicians in this field can comprehensively consider the above factors and reasonably select the immersion time, and can achieve comparable technical effects without having to pay creative labor.
[0058] For example, but not limited to, the dipping time is not less than 1 minute, and further non-limiting examples of the dipping time may be 2 minutes, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 15 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, etc. For comparison only, the dipping time in the embodiments and comparative examples is 5 minutes.
[0059] In the above technical solution, preferably, the material of the raw fabric in step (i) is cotton, acrylic, polyester, polypropylene or spandex, and the raw fabric is in the form of textiles, knitwear or non-woven fabrics. For comparison only, the raw fabrics in the embodiments of the present invention and the comparative examples are mattress fabrics provided by Xilinmen Furniture Co., Ltd., which are knitted double-sided circular knitting machine sandwich jacquard fabrics. The fabric is a composite fabric with a front side, a sandwich and a back side, which are combined into one by joints. The specific specifications are as follows:
[0060]
[0061]
[0062] In the above technical scheme, the liquid-carrying rate of the liquid-carrying fabric a in step (i) is not particularly limited. Those skilled in the art can reasonably control the liquid-carrying rate according to the silver content in the antibacterial finishing working liquid of the fabric, the ability of the fabric to absorb the finishing working liquid, the amount of silver contained in the desired antibacterial fabric, and whether to squeeze after impregnation and the degree of squeezing. The present invention specification adopts the commonly used meaning of liquid-carrying rate in the art, that is, the ratio of the raw fabric to the antibacterial finishing working liquid of the fabric, which is measured by weight and relative to the raw fabric. By way of example only, the liquid impregnation rate in the liquid impregnated fabric a can be 50-100% by weight and relative to the raw fabric, and more specific non-limiting examples of liquid impregnation rates are 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, etc. Compared with the same period last year, the liquid impregnation rate of the liquid impregnated fabric a in both the embodiment and the comparative example was 80%.
[0063] In the above technical solution, the drying temperature and time of step (ii) are not particularly limited, as long as part or all of the water in the liquid-carrying fabric a can be removed, comparable technical effects can be achieved. However, those skilled in the art know that the lower the drying temperature, the more thorough the water needs to be removed, and the longer the required drying time tends to be. Those skilled in the art can reasonably select the drying time and temperature based on this principle without having to make creative efforts.
[0064] In the above technical solution, for example but not limited to, the drying temperature of step (ii) is 80-110°C, and more specific non-limiting examples of the drying temperature of step (ii) are 85°C, 90°C, 95°C, 100°C, 105°C, etc. For comparison only, the drying temperature of step (ii) in the embodiment and the comparative example is 100°C.
[0065] In the above technical solution, for example but not limited to, the drying time of step (ii) is more than 3 minutes, for example but not limited to 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, etc. For comparison only, the drying time of step (ii) in the embodiment and the comparative example is 5 minutes.
[0066] In the above technical solution, the purpose of baking in step (iii) is to further remove the residual water introduced by the antibacterial finishing working solution in the fabric, and at the same time to cross-link the cross-linking agent added to the finishing working solution so that the silver is more firmly fixed in the fabric. To achieve this purpose, those skilled in the art can reasonably select the baking temperature and baking time.
[0067] In the above technical solution, for example but not limited to the baking temperature of step (iii) is 130-180°C. As a more specific non-limiting example, the baking temperature of step (iii) is 132°C, 134°C, 136°C, 138°C, 140°C, 142°C, 144°C, 146°C, 147°C, 148°C, 150°C, 152°C, 154°C, 156°C, 158°C, 160°C, 165°C, 170°C, 175°C, etc. For comparison only, the baking temperature of step (iii) in the embodiment and the comparative example is 150°C.
[0068] In the above technical scheme, for example but not limited to the time of baking in step (iii) is more than 1 min. As a more specific non-limiting example, the time of baking in step (iii) is 1.5 min, 2 min, 2.5 min, 3 min, 3.5 min, 4 min, 4.5 min, 5 min, 5.5 min, 6 min, 6.5 min, 7 min, 7.5 min, 8 min, 8.5 min, 9 min, 9.5 min, etc. Only for comparison, the time of baking in step (iii) in the embodiment and the comparative example is 3 min.
[0069] The present invention adopts "GB / T 20944.3-2008 Evaluation of Antibacterial Performance of Textiles Part 3: Oscillation Method" to evaluate the antibacterial performance of the antibacterial finishing working solution for fabrics.
[0070] in:
[0071] The test bacteria species used are those specified in Section 8.1 of the standard: Staphylococcus aureus (ATCC 6538); and Escherichia coli (8099).
[0072] Preparation of fabric samples: According to the provisions of Section 10.2 of the method, cut the antibacterial fabric and the control sample (i.e., raw fabric) into pieces of 5 mm × 5 mm, weigh 0.75 g as a sample, and wrap it with a small piece of paper. Then, according to the provisions of Section 10.3 of the method, put the small paper package containing the sample into an autoclave at 121°C and 103 kPa for 15 minutes for use.
[0073] The higher the inhibition rate measured by this method, the better the antibacterial effect on the corresponding test bacteria.
[0074] The effect of antibacterial finishing liquid on the color stability of antibacterial fabrics was measured by color change value (ΔE* ab ) for evaluation, ΔE* ab The larger the value, the worse the color stability of the antibacterial fabric. On the contrary, ΔE* ab The smaller the value, the better the color stability of the antibacterial fabric. The operation process is:
[0075] 1. Preparation of test samples and control samples
[0076] The fabric samples to be aged were aged for 24 hours in a Q-Sun XE-2 series Xe-2-HE xenon lamp test chamber produced by Q Lab, USA. The test surface was the front side of the fabric. The aging conditions were:
[0077] Relative humidity, 40%;
[0078] Irradiance, 42W / m 2 / nm;
[0079] Blackboard temperature, 47°C;
[0080] Box air temperature, 39°C;
[0081] The filter is Window-IR type;
[0082] Irradiance sensor model, TUV;
[0083] Black panel temperature sensor, black standard type (structure is black painted stainless steel and insulating plastic back panel).
[0084] The raw fabric treated by the above aging method is the control sample, and the antibacterial fabric obtained by the above aging method is the sample to be tested.
[0085] 2. Fabric color property measurement
[0086] The fabric color was measured using an X-Rite spectrophotometer (model: Ci7800) with a pulsed xenon arc light source, diffuse illumination and an 8° observation angle (d / 8), with a measurement area of 25 mm (1 inch). After the instrument was calibrated in black and white, the measurements were performed on a control sample backed by a standard white tile and on a sample to be tested backed by a standard white tile, with the front side of the fabric as the test surface, to obtain the measured values of L, a and b, which describe the coordinate space of light / dark, red / green and blue / yellow.
[0087] 3. ΔE* ab Calculation
[0088] ΔE* ab The calculation is based on the measured values of L, a and b, and the calculation formula is as follows:
[0089]
[0090] The subscript 0 indicates the control sample measurement, and i indicates the single experimental sample measurement. Each fabric sample was measured at three locations on the front side, and the ΔE* ab The average values of L, a, and b were used in the calculation.
[0091] The present invention is described in detail below through specific implementation modes. DETAILED DESCRIPTION
[0092] [Comparative Example]
[0093] 1. Fabric antibacterial finishing working fluid
[0094] 1.1. Fabric antibacterial finishing working solution formula, by weight:
[0095] Positive monovalent Ag, 1 part; ammonia, 5 parts; cross-linking agent, 100 parts; water, so that the total number of parts of the fabric antibacterial finishing working solution is 20,000 parts.
[0096] 1.2. Preparation of antibacterial finishing working solution for fabrics
[0097] 1.2.1. Silver-containing liquid composition
[0098] Silver-containing antibacterial liquid composition formula, by weight:
[0099] Positive monovalent Ag, 1 part; ammonia, 5 parts; water, so that the total number of parts of the silver-containing antibacterial liquid composition is 1000 parts.
[0100] Add 5 parts of ammonia water with a weight concentration of 28% to 420 parts of water, and stir evenly to obtain a liquid mixture 1;
[0101] Dissolve AgNO3 equivalent to 1 part of Ag in 200 parts of water to obtain an aqueous solution of a positive monovalent silver compound;
[0102] Under stirring, an aqueous solution of a positive monovalent silver compound is added to the liquid mixture 1, and water is added to make the total number of parts of the silver-containing antibacterial liquid composition 1000 parts to obtain a mixture 2.
[0103] 1.2.2. Preparation of antibacterial finishing liquid for fabrics using a silver-containing liquid composition
[0104] 10 parts of the cross-linking agent were added to 100 parts of the mixture 2, and water was added so that the total number of parts of the antibacterial finishing working solution for fabrics was 2000 parts.
[0105] 2. Manufacture of antibacterial fabrics
[0106] According to the weight ratio of fabric antibacterial finishing liquid to raw fabric being 15, the raw fabric was immersed in the fabric antibacterial finishing working liquid for 5 minutes, and then the excess fabric antibacterial finishing working liquid was squeezed out to make the liquid carrying rate of the fabric 80%, dried at 100°C for 5 minutes, and then baked at 150°C for 3 minutes to obtain the antibacterial fabric.
[0107] 3. Performance testing
[0108] After testing, the antibacterial fabric has an antibacterial rate of 72% against Staphylococcus aureus and 75% against Escherichia coli; the ΔE* ab It is 10.5.
[0109] [Example 1]
[0110] 1. Fabric antibacterial finishing working fluid
[0111] 1.1. Fabric antibacterial finishing working solution formula, by weight:
[0112] Positive monovalent Ag, 1 part; ammonia, 5 parts; ethanol, 40 parts; cross-linking agent, 100 parts; water, so that the total number of parts of the fabric antibacterial finishing working solution is 20,000 parts.
[0113] 1.2. Preparation of fabric antibacterial finishing working solution
[0114] 1.2.1. Silver-containing liquid composition
[0115] Silver-containing antibacterial liquid composition formula, by weight:
[0116] Positive monovalent Ag, 1 part; ammonia, 5 parts; ethanol, 40 parts; water, so that the total number of parts of the silver-containing antibacterial liquid composition is 1000 parts.
[0117] Add 5 parts of ammonia water with a weight concentration of 28% and 40 parts of ethanol to 420 parts of water, and stir evenly to obtain a liquid mixture 1;
[0118] Dissolve AgNO3 equivalent to 1 part of Ag in 200 parts of water to obtain an aqueous solution of a positive monovalent silver compound;
[0119] Under stirring, an aqueous solution of a positive monovalent silver compound is added to the liquid mixture 1, and water is added to make the total number of parts of the silver-containing antibacterial liquid composition 1000 parts to obtain a mixture 2.
[0120] 1.2.2. Preparation of antibacterial finishing liquid for fabrics using a silver-containing liquid composition
[0121] 10 parts of the cross-linking agent were added to 100 parts of the mixture 2, and water was added so that the total number of parts of the antibacterial finishing working solution for fabrics was 2000 parts.
[0122] 2. Manufacture of antibacterial fabrics
[0123] According to the weight ratio of fabric antibacterial finishing liquid to raw fabric being 15, the raw fabric was immersed in the fabric antibacterial finishing working liquid for 5 minutes, and then the excess fabric antibacterial finishing working liquid was squeezed out to make the liquid carrying rate of the fabric 80%, dried at 100°C for 5 minutes, and then baked at 150°C for 3 minutes to obtain the antibacterial fabric.
[0124] 3. Performance testing
[0125] After testing, the antibacterial fabric has an antibacterial rate of 85% against Staphylococcus aureus and 90% against Escherichia coli; the ΔE* ab is 4.5.
[0126] [Example 2]
[0127] 1. Fabric antibacterial finishing working fluid
[0128] 1.1. Fabric antibacterial finishing working solution formula, by weight:
[0129] Positive monovalent Ag, 1 part; ammonia, 5 parts; propylene glycol, 40 parts; cross-linking agent, 100 parts; water, so that the total number of parts of the fabric antibacterial finishing working solution is 20,000 parts.
[0130] 1.2. Preparation of antibacterial finishing working solution for fabrics
[0131] 1.2.1. Silver-containing liquid composition
[0132] Silver-containing antibacterial liquid composition formula, by weight:
[0133] Positive monovalent Ag, 1 part; ammonia, 5 parts; glycerol, 40 parts; water, so that the total number of parts of the silver-containing antibacterial liquid composition is 1000 parts.
[0134] To 420 parts of water, add 5 parts of ammonia water with a weight concentration of 28% and 40 parts of propylene glycol, and stir evenly to obtain a liquid mixture 1;
[0135] Dissolve AgNO3 equivalent to 1 part of Ag in 200 parts of water to obtain an aqueous solution of a positive monovalent silver compound;
[0136] Under stirring, an aqueous solution of a positive monovalent silver compound is added to the liquid mixture 1, and water is added to make the total number of parts of the silver-containing antibacterial liquid composition 1000 parts to obtain a mixture 2.
[0137] 1.2.2. Preparation of antibacterial finishing liquid for fabrics using a silver-containing liquid composition
[0138] 10 parts of the cross-linking agent were added to 100 parts of the mixture 2, and water was added so that the total number of parts of the antibacterial finishing working solution for fabrics was 2000 parts.
[0139] 2. Manufacture of antibacterial fabrics
[0140] According to the weight ratio of fabric antibacterial finishing liquid to raw fabric being 15, the raw fabric was immersed in the fabric antibacterial finishing working liquid for 5 minutes, and then the excess fabric antibacterial finishing working liquid was squeezed out to make the liquid carrying rate of the fabric 80%, dried at 100°C for 5 minutes, and then baked at 150°C for 3 minutes to obtain the antibacterial fabric.
[0141] 3. Performance testing
[0142] After testing, the antibacterial fabric has an antibacterial rate of 88% against Staphylococcus aureus and 93% against Escherichia coli; the ΔE* of the antibacterial fabric is ab is 4.2.
[0143] [Example 3]
[0144] 1. Fabric antibacterial finishing working fluid
[0145] 1.1. Fabric antibacterial finishing working solution formula, by weight:
[0146] Positive monovalent Ag, 1 part; ammonia, 5 parts; ethanol, 30 parts; propylene glycol, 10 parts; cross-linking agent, 100 parts; water, so that the total number of parts of the fabric antibacterial finishing working solution is 20,000 parts.
[0147] 1.2. Preparation of fabric antibacterial finishing working solution
[0148] 1.2.1. Silver-containing liquid composition
[0149] Silver-containing antibacterial liquid composition formula, by weight:
[0150] Positive monovalent Ag, 1 part; ammonia, 5 parts; ethanol, 30 parts; glycerol, 10 parts; water, so that the total number of parts of the silver-containing antibacterial liquid composition is 1000 parts.
[0151] To 420 parts of water, add 5 parts of ammonia water with a weight concentration of 28%, 30 parts of ethanol, and 10 parts of propylene glycol, and stir evenly to obtain a liquid mixture 1;
[0152] Dissolve AgNO3 equivalent to 1 part of Ag in 200 parts of water to obtain an aqueous solution of a positive monovalent silver compound;
[0153] Under stirring, an aqueous solution of a positive monovalent silver compound is added to the liquid mixture 1, and water is added to make the total number of parts of the silver-containing antibacterial liquid composition 1000 parts to obtain a mixture 2.
[0154] 1.2.2. Preparation of antibacterial finishing liquid for fabrics using a silver-containing liquid composition
[0155] 10 parts of the cross-linking agent were added to 100 parts of the mixture 2, and water was added so that the total number of parts of the antibacterial finishing working solution for fabrics was 2000 parts.
[0156] 2. Manufacture of antibacterial fabrics
[0157] According to the weight ratio of fabric antibacterial finishing liquid to raw fabric being 15, the raw fabric was immersed in the fabric antibacterial finishing working liquid for 5 minutes, and then the excess fabric antibacterial finishing working liquid was squeezed out to make the liquid carrying rate of the fabric 80%, dried at 100°C for 5 minutes, and then baked at 150°C for 3 minutes to obtain the antibacterial fabric.
[0158] 3. Performance testing
[0159] After testing, the antibacterial fabric has an antibacterial rate of 90% against Staphylococcus aureus and 95% against Escherichia coli; the ΔE* of the antibacterial fabric is ab is 3.4.
[0160] [Example 4]
[0161] 1. Fabric antibacterial finishing working fluid
[0162] 1.1. Fabric antibacterial finishing working solution formula, by weight:
[0163] Positive monovalent Ag, 1 part; ammonia, 5 parts; polyethyleneimine, 58 parts; cross-linking agent, 100 parts; water, so that the total number of parts of the fabric antibacterial finishing working solution is 20,000 parts.
[0164] 1.2. Preparation of antibacterial finishing working solution for fabrics
[0165] 1.2.1. Silver-containing liquid composition
[0166] Silver-containing antibacterial liquid composition formula, by weight:
[0167] Positive monovalent Ag, 1 part; ammonia, 5 parts; polyethyleneimine, 58 parts; water, so that the total number of parts of the silver-containing antibacterial liquid composition is 1000 parts.
[0168] To 420 parts of water, add 5 parts of ammonia water with a weight concentration of 28% and 58 parts of polyethyleneimine, and stir evenly to obtain a liquid mixture 1;
[0169] Dissolve AgNO3 equivalent to 1 part of Ag in 200 parts of water to obtain an aqueous solution of a positive monovalent silver compound;
[0170] Under stirring, an aqueous solution of a positive monovalent silver compound is added to the liquid mixture 1, and water is added to make the total number of parts of the silver-containing antibacterial liquid composition 1000 parts to obtain a mixture 2.
[0171] 1.2.2. Preparation of antibacterial finishing liquid for fabrics using a silver-containing liquid composition
[0172] 10 parts of the cross-linking agent were added to 100 parts of the mixture 2, and water was added so that the total number of parts of the antibacterial finishing working solution for fabrics was 2000 parts.
[0173] 2. Manufacture of antibacterial fabrics
[0174] According to the weight ratio of fabric antibacterial finishing liquid to raw fabric being 15, the raw fabric was immersed in the fabric antibacterial finishing working liquid for 5 minutes, and then the excess fabric antibacterial finishing working liquid was squeezed out to make the liquid carrying rate of the fabric 80%, dried at 100°C for 5 minutes, and then baked at 150°C for 3 minutes to obtain the antibacterial fabric.
[0175] 3. Performance testing
[0176] After testing, the antibacterial fabric has an antibacterial rate of 95% against Staphylococcus aureus and 98% against Escherichia coli; the ΔE* ab is 3.5.
[0177] [Example 5]
[0178] 1. Fabric antibacterial finishing working fluid
[0179] 1.1. Fabric antibacterial finishing working solution formula, by weight:
[0180] Positive monovalent Ag, 1 part; ammonia, 5 parts; SiO2 colloid particles, 58 parts; crosslinking agent, 100 parts; water, so that the total number of parts of the fabric antibacterial finishing working solution is 20,000 parts.
[0181] 1.2. Preparation of fabric antibacterial finishing working solution
[0182] 1.2.1. Silver-containing liquid composition
[0183] Silver-containing antibacterial liquid composition formula, by weight:
[0184] Positive monovalent Ag, 1 part; ammonia, 5 parts; SiO2 colloid, 58 parts; water, so that the total number of parts of the silver-containing antibacterial liquid composition is 1000 parts.
[0185] Add 5 parts of ammonia water with a weight concentration of 28% to 420 parts of water, stir evenly, add 58 parts of silica sol with a weight content of 40% of silicon oxide, stir evenly, and obtain liquid mixture 1;
[0186] Dissolve AgNO3 equivalent to 1 part of Ag in 200 parts of water to obtain an aqueous solution of a positive monovalent silver compound;
[0187] Under stirring, an aqueous solution of a positive monovalent silver compound is added to the liquid mixture 1, and water is added to make the total number of parts of the silver-containing antibacterial liquid composition 1000 parts to obtain a mixture 2.
[0188] 1.2.2. Preparation of antibacterial finishing liquid for fabrics using a silver-containing liquid composition
[0189] 10 parts of the cross-linking agent were added to 100 parts of the mixture 2, and water was added so that the total number of parts of the antibacterial finishing working solution for fabrics was 2000 parts.
[0190] 2. Manufacture of antibacterial fabrics
[0191] According to the weight ratio of fabric antibacterial finishing liquid to raw fabric being 15, the raw fabric was immersed in the fabric antibacterial finishing working liquid for 5 minutes, and then the excess fabric antibacterial finishing working liquid was squeezed out to make the liquid carrying rate of the fabric 80%, dried at 100°C for 5 minutes, and then baked at 150°C for 3 minutes to obtain the antibacterial fabric.
[0192] 3. Performance testing
[0193] After testing, the antibacterial fabric has an antibacterial rate of 89% against Staphylococcus aureus and 92% against Escherichia coli; the ΔE* ab is 3.8.
[0194] [Example 6]
[0195] 1. Fabric antibacterial finishing working fluid
[0196] 1.1. Fabric antibacterial finishing working solution formula, by weight:
[0197] Positive monovalent Ag, 1 part; ammonia, 5 parts; polyethyleneimine, 24 parts; SiO2 colloid particles, 34 parts; crosslinking agent, 100 parts; water, so that the total number of parts of the fabric antibacterial finishing working solution is 20,000 parts.
[0198] 1.2. Preparation of antibacterial finishing working solution for fabrics
[0199] 1.2.1. Silver-containing liquid composition
[0200] Silver-containing antibacterial liquid composition formula, by weight:
[0201] Positive monovalent Ag, 1 part; ammonia, 5 parts; polyethyleneimine, 24 parts; SiO2 colloid, 34 parts; water, so that the total number of parts of the silver-containing antibacterial liquid composition is 1000 parts.
[0202] Add 5 parts of ammonia water with a weight concentration of 28% and 24 parts of polyethyleneimine to 420 parts of water, stir evenly, add 34 parts of silica sol with a weight content of 40% of silicon oxide, stir evenly, and obtain a liquid mixture 1;
[0203] Dissolve AgNO3 equivalent to 1 part of Ag in 200 parts of water to obtain an aqueous solution of a positive monovalent silver compound;
[0204] Under stirring, an aqueous solution of a positive monovalent silver compound is added to the liquid mixture 1, and water is added to make the total number of parts of the silver-containing antibacterial liquid composition 1000 parts to obtain a mixture 2.
[0205] 1.2.2. Preparation of antibacterial finishing liquid for fabrics using a silver-containing liquid composition
[0206] 10 parts of the cross-linking agent were added to 100 parts of the mixture 2, and water was added so that the total number of parts of the antibacterial finishing working solution for fabrics was 2000 parts.
[0207] 2. Manufacture of antibacterial fabrics
[0208] According to the weight ratio of fabric antibacterial finishing liquid to raw fabric being 15, the raw fabric was immersed in the fabric antibacterial finishing working liquid for 5 minutes, and then the excess fabric antibacterial finishing working liquid was squeezed out to make the liquid carrying rate of the fabric 80%, dried at 100°C for 5 minutes, and then baked at 150°C for 3 minutes to obtain the antibacterial fabric.
[0209] 3. Performance testing
[0210] After testing, the antibacterial fabric has an antibacterial rate of 99% against Staphylococcus aureus and 99% against Escherichia coli; the ΔE* of the antibacterial fabric is ab is 2.5.
[0211] [Example 7]
[0212] 1. Fabric antibacterial finishing working fluid
[0213] 1.1. Fabric antibacterial finishing working solution formula, by weight:
[0214] Positive monovalent Ag, 1 part; ammonia, 5 parts; ethanol, 40 parts; polyethyleneimine, 24 parts; SiO2 colloid particles, 34 parts; crosslinking agent, 100 parts; water, so that the total number of parts of the fabric antibacterial finishing working solution is 20,000 parts.
[0215] 1.2. Preparation of fabric antibacterial finishing working solution
[0216] 1.2.1. Silver-containing liquid composition
[0217] Silver-containing antibacterial liquid composition formula, by weight:
[0218] Positive monovalent Ag, 1 part; ammonia, 5 parts; ethanol, 40 parts; polyethyleneimine, 24 parts; SiO2 colloid particles, 34 parts; water, so that the total number of parts of the silver-containing antibacterial liquid composition is 1000 parts.
[0219] To 420 parts of water, add 5 parts of ammonia water with a weight concentration of 28%, 40 parts of ethanol, and 24 parts of polyethyleneimine, stir evenly, add 34 parts of silica sol with a weight content of 40% of silicon oxide, stir evenly, and obtain a liquid mixture 1;
[0220] Dissolve AgNO3 equivalent to 1 part of Ag in 200 parts of water to obtain an aqueous solution of a positive monovalent silver compound;
[0221] Under stirring, an aqueous solution of a positive monovalent silver compound is added to the liquid mixture 1, and water is added to make the total number of parts of the silver-containing antibacterial liquid composition 1000 parts to obtain a mixture 2.
[0222] 1.2.2. Preparation of antibacterial finishing liquid for fabrics using a silver-containing liquid composition
[0223] 10 parts of the cross-linking agent were added to 100 parts of the mixture 2, and water was added so that the total number of parts of the antibacterial finishing working solution for fabrics was 2000 parts.
[0224] 2. Manufacture of antibacterial fabrics
[0225] According to the weight ratio of fabric antibacterial finishing liquid to raw fabric being 15, the raw fabric was immersed in the fabric antibacterial finishing working liquid for 5 minutes, and then the excess fabric antibacterial finishing working liquid was squeezed out to make the liquid carrying rate of the fabric 80%, dried at 100°C for 5 minutes, and then baked at 150°C for 3 minutes to obtain the antibacterial fabric.
[0226] 3. Performance testing
[0227] After testing, the antibacterial fabric has an antibacterial rate of 99% against Staphylococcus aureus and 99% against Escherichia coli; the ΔE* of the antibacterial fabric is ab is 1.6.
[0228] [Example 8]
[0229] 1. Fabric antibacterial finishing working fluid
[0230] 1.1. Fabric antibacterial finishing working solution formula, by weight:
[0231] Positive monovalent Ag, 1 part; ammonia, 5 parts; propylene glycol, 40 parts; polyethylene imine, 24 parts; SiO2 colloid particles, 34 parts; crosslinking agent, 100 parts; water, so that the total number of parts of the fabric antibacterial finishing working solution is 20,000 parts.
[0232] 1.2. Preparation of fabric antibacterial finishing working solution
[0233] 1.2.1. Silver-containing liquid composition
[0234] Silver-containing antibacterial liquid composition formula, by weight:
[0235] Positive monovalent Ag, 1 part; ammonia, 5 parts; propylene glycol, 40 parts; polyethylene imine, 24 parts; SiO2 colloid particles, 34 parts; water, so that the total number of parts of the silver-containing antibacterial liquid composition is 1000 parts.
[0236] To 420 parts of water, add 5 parts of ammonia water with a weight concentration of 28%, 40 parts of propylene glycol, and 24 parts of polyethyleneimine, stir evenly, add 34 parts of silica sol with a weight content of 40% of silicon oxide, stir evenly, and obtain a liquid mixture 1;
[0237] Dissolve AgNO3 equivalent to 1 part of Ag in 200 parts of water to obtain an aqueous solution of a positive monovalent silver compound;
[0238] Under stirring, an aqueous solution of a positive monovalent silver compound is added to the liquid mixture 1, and water is added to make the total number of parts of the silver-containing antibacterial liquid composition 1000 parts to obtain a mixture 2.
[0239] 1.2.2. Preparation of antibacterial finishing liquid for fabrics using a silver-containing liquid composition
[0240] 10 parts of the cross-linking agent were added to 100 parts of the mixture 2, and water was added so that the total number of parts of the antibacterial finishing working solution for fabrics was 2000 parts.
[0241] 2. Manufacture of antibacterial fabrics
[0242] According to the weight ratio of fabric antibacterial finishing liquid to raw fabric being 15, the raw fabric was immersed in the fabric antibacterial finishing working liquid for 5 minutes, and then the excess fabric antibacterial finishing working liquid was squeezed out to make the liquid carrying rate of the fabric 80%, dried at 100°C for 5 minutes, and then baked at 150°C for 3 minutes to obtain the antibacterial fabric.
[0243] 3. Performance testing
[0244] After testing, the antibacterial fabric has an antibacterial rate of 99% against Staphylococcus aureus and 99% against Escherichia coli; the ΔE* of the antibacterial fabric is ab is 1.5.
[0245] [Example 9]
[0246] 1. Fabric antibacterial finishing working fluid
[0247] 1.1. Fabric antibacterial finishing working solution formula, by weight:
[0248] Positive monovalent Ag, 1 part; ammonia, 5 parts; ethanol, 30 parts; propylene glycol, 10 parts; polyethylene imine, 58 parts; cross-linking agent, 100 parts; water, so that the total number of parts of the fabric antibacterial finishing working solution is 20,000 parts.
[0249] 1.2. Preparation of antibacterial finishing working solution for fabrics
[0250] 1.2.1. Silver-containing liquid composition
[0251] Silver-containing antibacterial liquid composition formula, by weight:
[0252] Positive monovalent Ag, 1 part; ammonia, 5 parts; ethanol, 30 parts; glycerol, 10 parts; polyethyleneimine, 58 parts; water, so that the total number of parts of the silver-containing antibacterial liquid composition is 1000 parts.
[0253] To 420 parts of water, add 5 parts of ammonia water with a weight concentration of 28%, 30 parts of ethanol, 10 parts of propylene glycol, and 58 parts of polyethyleneimine, and stir evenly to obtain a liquid mixture 1;
[0254] Dissolve AgNO3 equivalent to 1 part of Ag in 200 parts of water to obtain an aqueous solution of a positive monovalent silver compound;
[0255] Under stirring, an aqueous solution of a positive monovalent silver compound is added to the liquid mixture 1, and water is added to make the total number of parts of the silver-containing antibacterial liquid composition 1000 parts to obtain a mixture 2.
[0256] 1.2.2. Preparation of antibacterial finishing liquid for fabrics using a silver-containing liquid composition
[0257] 10 parts of the cross-linking agent were added to 100 parts of the mixture 2, and water was added so that the total number of parts of the antibacterial finishing working solution for fabrics was 2000 parts.
[0258] 2. Manufacture of antibacterial fabrics
[0259] According to the weight ratio of fabric antibacterial finishing liquid to raw fabric being 15, the raw fabric was immersed in the fabric antibacterial finishing working liquid for 5 minutes, and then the excess fabric antibacterial finishing working liquid was squeezed out to make the liquid carrying rate of the fabric 80%, dried at 100°C for 5 minutes, and then baked at 150°C for 3 minutes to obtain the antibacterial fabric.
[0260] 3. Performance testing
[0261] After testing, the antibacterial fabric has an antibacterial rate of >99% against Staphylococcus aureus and >99% against Escherichia coli; the ΔE* of the antibacterial fabric is ab is 1.0.
[0262] [Example 10]
[0263] 1. Fabric antibacterial finishing working fluid
[0264] 1.1. Fabric antibacterial finishing working solution formula, by weight:
[0265] Positive monovalent Ag, 1 part; ammonia, 5 parts; ethanol, 30 parts; propylene glycol, 10 parts; SiO2 colloid particles, 58 parts; crosslinking agent, 100 parts; water, so that the total number of parts of the fabric antibacterial finishing working solution is 20,000 parts.
[0266] 1.2. Preparation of antibacterial finishing working solution for fabrics
[0267] 1.2.1. Silver-containing liquid composition
[0268] Silver-containing antibacterial liquid composition formula, by weight:
[0269] Positive monovalent Ag, 1 part; ammonia, 5 parts; ethanol, 30 parts; propylene glycol, 10 parts; SiO2 colloid, 58 parts; water, so that the total number of parts of the silver-containing antibacterial liquid composition is 1000 parts.
[0270] To 420 parts of water, add 5 parts of ammonia water with a weight concentration of 28%, 30 parts of ethanol, and 10 parts of propylene glycol, and stir evenly, and add 58 parts of silica sol with a weight content of 40% of silicon oxide, and stir evenly to obtain a liquid mixture 1;
[0271] Dissolve AgNO3 equivalent to 1 part of Ag in 200 parts of water to obtain an aqueous solution of a positive monovalent silver compound;
[0272] Under stirring, an aqueous solution of a positive monovalent silver compound is added to the liquid mixture 1, and water is added to make the total number of parts of the silver-containing antibacterial liquid composition 1000 parts to obtain a mixture 2.
[0273] 1.2.2. Preparation of antibacterial finishing liquid for fabrics using a silver-containing liquid composition
[0274] 10 parts of the cross-linking agent were added to 100 parts of the mixture 2, and water was added so that the total number of parts of the antibacterial finishing working solution for fabrics was 2000 parts.
[0275] 2. Manufacture of antibacterial fabrics
[0276] According to the weight ratio of fabric antibacterial finishing liquid to raw fabric being 15, the raw fabric was immersed in the fabric antibacterial finishing working liquid for 5 minutes, and then the excess fabric antibacterial finishing working liquid was squeezed out to make the liquid carrying rate of the fabric 80%, dried at 100°C for 5 minutes, and then baked at 150°C for 3 minutes to obtain the antibacterial fabric.
[0277] 3. Performance testing
[0278] After testing, the antibacterial fabric has an antibacterial rate of >99% against Staphylococcus aureus and >99% against Escherichia coli; the ΔE* of the antibacterial fabric is ab is 1.2.
[0279] [Example 11]
[0280] 1. Fabric antibacterial finishing working fluid
[0281] 1.1. Fabric antibacterial finishing working solution formula, by weight:
[0282] Positive monovalent Ag, 1 part; ammonia, 5 parts; ethanol, 30 parts; propylene glycol, 10 parts; polyethyleneimine, 24 parts; SiO2 colloid particles, 34 parts; crosslinking agent, 100 parts; water, so that the total number of parts of the fabric antibacterial finishing working solution is 20,000 parts.
[0283] 1.2. Preparation of fabric antibacterial finishing working solution
[0284] 1.2.1. Silver-containing liquid composition
[0285] Silver-containing antibacterial liquid composition formula, by weight:
[0286] Positive monovalent Ag, 1 part; ammonia, 5 parts; ethanol, 30 parts; propylene glycol, 10 parts; polyethyleneimine, 24 parts; SiO2 colloid, 34 parts; water, so that the total number of parts of the silver-containing antibacterial liquid composition is 1000 parts.
[0287] To 420 parts of water, add 5 parts of ammonia water with a weight concentration of 28%, 30 parts of ethanol, 10 parts of propylene glycol, and 24 parts of polyethyleneimine, stir evenly, add 34 parts of silica sol with a weight content of 40% of silicon oxide, stir evenly, and obtain a liquid mixture 1;
[0288] Dissolve AgNO3 equivalent to 1 part of Ag in 200 parts of water to obtain an aqueous solution of a positive monovalent silver compound;
[0289] Under stirring, an aqueous solution of a positive monovalent silver compound is added to the liquid mixture 1, and water is added to make the total number of parts of the silver-containing antibacterial liquid composition 1000 parts to obtain a mixture 2.
[0290] 1.2.2. Preparation of antibacterial finishing liquid for fabrics using a silver-containing liquid composition
[0291] 10 parts of the cross-linking agent were added to 100 parts of the mixture 2, and water was added so that the total number of parts of the antibacterial finishing working solution for fabrics was 2000 parts.
[0292] 2. Manufacture of antibacterial fabrics
[0293] According to the weight ratio of fabric antibacterial finishing liquid to raw fabric being 15, the raw fabric was immersed in the fabric antibacterial finishing working liquid for 5 minutes, and then the excess fabric antibacterial finishing working liquid was squeezed out to make the liquid carrying rate of the fabric 80%, dried at 100°C for 5 minutes, and then baked at 150°C for 3 minutes to obtain the antibacterial fabric.
[0294] 3. Performance testing
[0295] After testing, the antibacterial fabric has an antibacterial rate of >99% against Staphylococcus aureus and >99% against Escherichia coli; the ΔE* of the antibacterial fabric is ab is 0.6.
[0296] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. Antimicrobial finishing solution for fabrics, comprising, by weight: (a) Ag (positive monovalent), 1 part; (b) ammonia, 3 to 10 parts; (c) C1-C3 alcohol, greater than 0 parts and less than 80 parts; (d) polyethyleneimine, 0-80 parts; (e) SiO2 colloid particles, 0-80 parts; (f) cross-linking agent, 0 to 200 parts; (g) water, so that the total number of parts of the antibacterial finishing working solution for fabrics is 10,000 to 50,000 parts The C1~C3 alcohols include ethanol and glycerol.
2. The fabric antibacterial finishing working solution according to claim 1, characterized in that The number of parts of water is such that the total number of parts of the antibacterial finishing working solution for fabrics is 15,000 to 30,000 parts.
3. The fabric antibacterial finishing working solution according to claim 1, characterized in that The C1-C3 alcohol is 20-80 parts.
4. The fabric antibacterial finishing working solution according to claim 1, characterized in that The amount of polyethyleneimine is greater than 0 parts and less than 80 parts.
5. The fabric antibacterial finishing working solution according to claim 4 is characterized in that The amount of polyethyleneimine is 10 to 40 parts.
6. The fabric antibacterial finishing working solution according to claim 1, characterized in that The weight average molecular weight of polyethyleneimine is 500~10000.
7. The fabric antibacterial finishing working solution according to claim 6, characterized in that The weight average molecular weight of polyethyleneimine is 500~5000.
8. The fabric antibacterial finishing working solution according to claim 1, characterized in that In the polyethyleneimine molecule, the ratio of primary amino group: secondary amino group: tertiary amino group is 1:a:b on a molar basis, wherein a is 0.8-1.2 and b is 0.4-0.
8.
9. The fabric antibacterial finishing working solution according to claim 1, characterized in that The amount of SiO2 colloid particles is greater than 0 parts and less than 80 parts.
10. The antibacterial finishing working liquid for fabrics according to claim 1, characterized in that The amount of SiO2 colloid particles is 10~50 parts.
11. A method for producing an antibacterial fabric, comprising: (i) contacting a raw fabric with the fabric antibacterial finishing working solution according to any one of claims 1 to 10 to obtain a liquid-containing fabric a; (ii) drying to obtain fabric b; (iii) baking to obtain antibacterial fabric.
12. The manufacturing method according to claim 11, characterized in that The material of the raw fabric in step (i) is cotton, acrylic, polyester, polypropylene or spandex, and the raw fabric is in the form of textile.
13. The manufacturing method according to claim 12, characterized in that The raw fabric in step (i) is in the form of knitted fabric or non-woven fabric.
14. The manufacturing method according to claim 12, characterized in that: The liquid-carrying rate of the liquid-carrying fabric a is 50-100% based on weight and relative to the raw fabric.
15. The manufacturing method according to claim 11, characterized in that The drying temperature in step (ii) is 80-110°C.
16. The manufacturing method according to claim 11, characterized in that The drying time in step (ii) is more than 3 minutes.
17. The manufacturing method according to claim 11, characterized in that The baking temperature in step (iii) is 130-180°C.
18. The manufacturing method according to claim 11, characterized in that The baking time in step (iii) is more than 1 minute.
Citation Information
Cited By
Woolen cloth mothproof finishing liquid and finishing process thereof
CN119571613A