Regeneration method of spent catalyst
Through the combination of programmed temperature oxidation test and staged roasting, the problem of incomplete or excessive roasting in the high-temperature roasting regeneration method was solved. The activity recovery of the catalyst was significantly improved through organic compound supplementation, and more efficient catalyst regeneration was achieved.
Patent Information
- Application Number
- CN202111291462.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-10-29
AI Technical Summary
The high-temperature roasting regeneration method has the problem of incomplete roasting or excessive roasting, which makes it difficult to effectively restore the activity of the catalyst. In particular, it is difficult to control the regeneration effect of deactivated catalysts with special pore structures.
Use a programmed temperature oxidation test to determine the peak number and peak temperature of the components to be removed, perform segmented roasting, and add organic alcohol compounds and/or carboxylic acid compounds to the catalyst after regeneration to promote the recovery of the catalyst activity.
Through staged roasting and organic compound supplementation, the activity recovery degree of the catalyst is improved, excessive or insufficient roasting is avoided, the catalyst activity after regeneration is significantly improved, and a better regeneration effect is ensured.
Smart Images

Figure CN116060079B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalyst regeneration, and in particular to a method for regenerating a catalyst to be regenerated. Background Art
[0002] Catalysts generally become deactivated during use. Regenerating deactivated catalysts can not only extend the service life of the catalyst, but also save production costs. Therefore, deactivated catalyst regeneration technology has attracted more and more attention.
[0003] There are many types of catalysts, and the deactivation and regeneration methods of different catalysts are not the same. For deactivated catalysts containing carbon deposits, high-temperature roasting is generally used for regeneration. This regeneration method has the advantage of universality, but the efficiency of this regeneration method still has certain shortcomings. For deactivated catalysts with special pore structures, if high-temperature regeneration is directly performed, it is easy to cause problems such as incomplete roasting or over-roasting, and it is difficult to control the regeneration effect of the catalyst, and the optimal regeneration effect cannot be achieved.
[0004] Therefore, there is an urgent need to provide a catalyst regeneration method that can improve the regeneration effect. Summary of the invention
[0005] The purpose of the present invention is to solve the problem of incomplete or excessive roasting in a high-temperature roasting regeneration method and to provide a method for regenerating a spent catalyst.
[0006] In order to achieve the above object, the present invention provides a method for regenerating a spent catalyst, wherein the pore size of the original catalyst of the spent catalyst is in the range of 8-20 nm and presents a single-peak pore distribution; the components to be removed in the spent catalyst include at least one of carbon deposits, sulfides, and nitrogen-containing organic matter;
[0007] The regeneration method comprises: firstly performing a programmed temperature oxidation test on the catalyst to be regenerated to determine the peak quantity and peak temperature of the component to be removed, and then performing segmented roasting on the catalyst to be regenerated according to the peak quantity and peak temperature.
[0008] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:
[0009] 1) A catalyst regeneration method provided by the present invention comprises performing segmented roasting on the catalyst to be regenerated according to the peak quantity and peak temperature of the components to be removed in the test results of the programmed temperature oxidation method, thereby promoting the decomposition of the components in the catalyst to be regenerated, preventing over- or under-roasting, and improving the activity recovery degree of the regenerated catalyst;
[0010] 2) The present invention provides a catalyst regeneration method, preferably by adding an organic alcohol compound and / or a carboxylic acid compound to the regenerated catalyst, so as to further restore the activity of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 This is a graph showing the test results of the programmed temperature oxidation method of the catalyst to be produced in Example 1. DETAILED DESCRIPTION
[0012] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0013] In the present invention, the 2-6nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 6nm, the 2-4nm pores refer to pores with a pore diameter greater than or equal to 2nm and less than 4nm, the 4-6nm pores refer to pores with a pore diameter greater than or equal to 4nm and less than 6nm, and the 8-20nm pores refer to pores with a pore diameter greater than or equal to 8nm and less than 20nm.
[0014] The first aspect of the present invention provides a method for regenerating a spent catalyst, wherein the spent catalyst has an original catalyst pore size in the range of 8-20 nm and presents a unimodal pore distribution; the components to be removed in the spent catalyst include at least one of carbon deposits, sulfides, and nitrogen-containing organic matter;
[0015] The regeneration method comprises: firstly performing a programmed temperature oxidation test on the catalyst to be regenerated to determine the peak quantity and peak temperature of the component to be removed, and then performing segmented roasting on the catalyst to be regenerated according to the peak quantity and peak temperature.
[0016] In the present invention, when a programmed temperature oxidation test is performed on a catalyst to be regenerated, if the difference in peak temperatures between two adjacent peaks is within 10° C., they can be regarded as one peak, and the peak temperature is the average value of the peak temperatures of the two peaks.
[0017] In the procatalyst:
[0018] Among them, the present invention does not specifically limit the specific schematic diagram of the catalyst to be regenerated, and it can be various catalysts to be regenerated in the conventional sense in the field, and its schematic diagram corresponds to the original catalyst (also referred to as a fresh catalyst). In a preferred embodiment of the present invention, all non-fresh catalysts (i.e., catalysts after reaction) that can be regenerated by calcination can be regenerated using the regeneration method of the present invention. Among them, the present invention does not specifically limit the reaction in which the original catalyst participates, and preferably the hydrodesulfurization reaction. The original catalyst pore size presents a unimodal pore distribution in the range of 8-20nm, which means that the original catalyst has a highest pore concentration peak at 8-20nm.
[0019] In a preferred embodiment of the present invention, the procatalyst comprises alumina and Group VIII metal elements, Group VIB metal elements and phosphorus elements supported on the alumina.
[0020] In a preferred embodiment of the present invention, the Group VIII metal element includes but is not limited to at least one of Fe, Co and Ni, preferably Co and / or Ni.
[0021] In a preferred embodiment of the present invention, the VIB Group metal element includes but is not limited to at least one of Cr, Mo and W, preferably Mo and / or W.
[0022] In a preferred embodiment of the present invention, the specific surface area of the procatalyst is 185-210 m 2 / g.
[0023] In a preferred embodiment of the present invention, the total pore volume of the procatalyst is 0.4-0.6 cm 3 / g, more preferably 0.4-0.5cm 3 / g.
[0024] In a preferred embodiment of the present invention, the average pore size of the procatalyst is 6-18 nm, preferably 8-12 nm.
[0025] In a preferred embodiment of the present invention, the volume of pores with pore diameter distribution in the range of 8-20 nm in the original catalyst accounts for 50-80%, preferably 60-75% of the total pore volume of the catalyst.
[0026] In a preferred embodiment of the present invention, the volume of pores with a pore size distribution between 2-4 nm in the procatalyst does not exceed 4%, preferably does not exceed 1%, of the total pore volume of the procatalyst.
[0027] In the present invention, the specific surface area, pore distribution, pore volume and average pore diameter of the original catalyst are measured after calcination at 400°C for 3 hours. The specific surface area, pore distribution, pore diameter and pore volume of the original catalyst are measured by low temperature nitrogen adsorption method (BET).
[0028] In a preferred embodiment of the present invention, the water absorption rate of the alumina raw material used to prepare the original catalyst is greater than 0.9 mL / g, preferably 0.9-1.1 mL / g; the specific surface area is greater than 260 m 2 / g, preferably 270-280m 2 / g; the average pore size is greater than 8nm, preferably 10-12nm; the pore distribution is unimodal; the pore volume of pores with a pore size distribution between 2-6nm does not exceed 10% of the total pore volume of the alumina raw material, preferably does not exceed 8%, and further preferably does not exceed 5%; the pore volume of pores with a pore size distribution between 2-4nm does not exceed 4% of the total pore volume of alumina, preferably does not exceed 1%.
[0029] In a preferred embodiment of the present invention, the original catalyst composition is (Xi ai )·(Yi bi )·(Zi ci )·Sup represents, wherein Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of carrier P2O5, Sup refers to the carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.18-0.39nm, preferably 0.25-0.38nm; Xi , Yi , Zi are the densities of Group VIB metal oxides, Group VIII metal oxides and P2O5, SA sup The specific surface area of the carrier refers to the specific surface area of the alumina raw material before loading the VIII group metal element, the VIB group metal element and the phosphorus element in the process of preparing the original catalyst. ρMoO3, ρWO3, ρNiO, ρCoO and ρP2O5 are 4.69 g / cm 3 、7.16g / cm 3 、6.67g / cm 3 、6.45g / cm 3 and 2.39 g / cm 3 calculate.
[0030] In a preferred embodiment of the present invention, the molar ratio of Zi / Xi in the procatalyst is 0.1-0.35:1, preferably 0.2-0.35:1.
[0031] In a preferred embodiment of the present invention, the atomic concentration of the VIB group metal element in the original catalyst on the carrier surface is 2-6atom / nm 2 , preferably 3-4.5atom / nm 2 .
[0032] In the present invention, the atomic concentration refers to the average atomic concentration of the metal element of Group VIB on the surface of the carrier, which is obtained by measuring the metal loading and the specific surface area of the carrier and then calculating. For example, it can be obtained by the following calculation formula: atomic concentration = (a / M Xi )×N A / (1×SA sup ), where N A is Avogadro's constant, ai is the mass relative to 1 gram of carrier Xi, M Xi is the molecular weight of Xi, SA sup The advantage of using the atomic concentration within this range is that a moderate number of active centers are formed, which on the one hand meets the needs of the reaction, and on the other hand leaves enough space to achieve the purpose of promoting diffusion and reducing carbon deposition.
[0033] In a preferred embodiment of the present invention, the atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the procatalyst is 0.2-0.4, preferably 0.2-0.35.
[0034] In a preferred embodiment of the present invention, the equivalent diameter of the procatalyst is 0.5-1.8 mm, more preferably 0.8-1.6 mm. The present invention does not specifically limit the shape of the procatalyst, and conventional catalyst shapes in the art are applicable to the present invention. Preferably, the procatalyst is cylindrical, clover, four-leaf clover, butterfly, honeycomb or other irregular shapes, more preferably butterfly.
[0035] In a preferred embodiment of the present invention, the components to be removed include carbon deposits and sulfides. The present invention has no particular limitation on the specific embodiment of the sulfides, which may be sulfur-containing compounds in the conventional sense in the art, such as metal sulfides or sulfur contained in the catalyst itself.
[0036] In a preferred embodiment of the present invention, the carbon content of the spent catalyst is 1-10 wt%, and the sulfur content is 1-10 wt%. The carbon and sulfur contents in the present invention refer to the contents of the elements.
[0037] In the regeneration method:
[0038] In one embodiment of the present invention, in the programmed temperature oxidation test, the carrier gas is selected from oxygen-containing gases, and the oxygen-containing gas is selected from air and / or oxygen, preferably air.
[0039] In one embodiment of the present invention, in the programmed temperature oxidation test, the flow rate of the carrier gas is 30-200 mL / min, preferably 50-150 mL / min.
[0040] In one embodiment of the present invention, in the programmed temperature oxidation test, the temperature is increased from room temperature to 500-800° C. at a heating rate of 1-15° C. / min. The room temperature is not particularly limited in the present invention and may be 10-35° C.
[0041] In one embodiment of the present invention, the peak number corresponds to the number of stages of staged roasting, and the peak temperatures correspond to the roasting temperatures of each stage of roasting from low to high.
[0042] In a preferred embodiment of the present invention, the heating rate of each calcination stage is independently selected from 1-20° C. / min, preferably 2-15° C. / min.
[0043] In a preferred embodiment of the present invention, the calcination time of each calcination stage is independently selected from 1-10 h, preferably 3-6 h.
[0044] In a preferred embodiment of the present invention, in the staged calcination, the heating rate of the first stage calcination is the fastest.
[0045] In a preferred embodiment of the present invention, in the staged roasting, the heating rate of each stage decreases successively; further preferably, between adjacent roasting stages, the heating rate decreases successively by 1-10°C / min, preferably by 2-7°C / min.
[0046] Among them, in the present invention, by controlling the heating rate of each stage of roasting, the regeneration effect can be further improved and the activity recovery degree of the regenerated catalyst can be increased.
[0047] In a preferred embodiment of the present invention, the regeneration method further comprises performing stable roasting after staged roasting, and the stable roasting comprises: raising the final temperature of the staged roasting by 10-50°C, preferably by 15-30°C for roasting.
[0048] Among them, in the present invention, by performing stable calcination, the removal effect of the components to be removed can be better, and the activity recovery degree of the regenerated catalyst can be increased by at least 6%.
[0049] In a preferred embodiment of the present invention, the heating rate of the stable calcination is 1-10°C / min, preferably 1-5°C / min.
[0050] In a preferred embodiment of the present invention, the calcination time of the stable calcination is 1-5h, preferably 2-4h.
[0051] Among them, in the present invention, the calcined product obtained after staged calcination or staged calcination followed by stable calcination is the regenerated catalyst. Compared with the one-step calcination, the calcination method in the present invention can promote the decomposition of carbon deposits, sulfides or nitrogen-containing compounds in the catalyst to be upgraded, make the calcination more uniform and thorough, effectively control the calcination, and promote the recovery of activity.
[0052] In a preferred embodiment of the present invention, the procatalyst further comprises an alcohol compound and / or a carboxylic acid compound. Further preferably, the catalyst further comprises one or more organic alcohol compounds and / or carboxylic acid compounds.
[0053] In a preferred embodiment of the present invention, the molar ratio of the organic alcohol compound and / or carboxylic acid compound to the metal element of Group VIII is 1-6, preferably 2-5.
[0054] In a preferred embodiment of the present invention, the organic alcohol compound is selected from at least one of monohydric alcohol, dihydric alcohol and polyhydric alcohol; preferably, the organic alcohol compound is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane; further preferably, the organic alcohol compound is selected from one of glycerol and propanol.
[0055] In a preferred embodiment of the present invention, the carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid, and is more preferably at least one of formic acid, citric acid and acetic acid.
[0056] In a preferred embodiment of the present invention, the procatalyst comprises one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polypropylene glycol, pentaerythritol, xylitol, sorbitol, trimethylolethane and / or formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid, tartaric acid.
[0057] In a preferred embodiment of the present invention, when the original catalyst also includes one or more organic alcohol compounds and / or carboxylic acid compounds, the regeneration method also includes: contacting the calcination product obtained after the staged calcination and / or stable calcination with an organic alcohol compound and / or a carboxylic acid compound to obtain a regenerated catalyst.
[0058] Among them, in the present invention, when the original catalyst does not contain organic alcohol compounds and / or carboxylic acid compounds, the calcined product obtained after staged calcination or staged calcination followed by stability calcination is the regenerated catalyst. When the original catalyst contains organic alcohol compounds and / or carboxylic acid compounds, it is also preferred to recover the organic alcohol compounds and / or carboxylic acid compounds in the calcined product to obtain a regenerated catalyst with a higher degree of activity recovery.
[0059] In a preferred embodiment of the present invention, the product obtained after calcination is contacted with an aqueous solution of an organic alcohol compound and / or a carboxylic acid compound, preferably by equal volume impregnation contact, and then dried to obtain a regenerated catalyst.
[0060] In a preferred embodiment of the present invention, the organic alcohol compound and / or carboxylic acid compound are of the same type as the organic alcohol compound and / or carboxylic acid compound in the original catalyst.
[0061] In a preferred embodiment of the present invention, the amount of the organic alcohol compound and / or carboxylic acid compound added is 0.5-2 times, preferably 0.75-1.5 times, the amount of the organic alcohol compound and / or carboxylic acid compound in the original catalyst.
[0062] The present invention will be described in detail below through examples.
[0063] The amount of material added during the preparation of the original catalyst is determined according to the specific exemplary description given in the text of the present invention.
[0064] Exemplary description: (1) According to the atomic concentration of the VIB group metal element and the specific surface area of the aluminum oxide, the amount of the VIB group metal precursor per gram of aluminum oxide is determined; (2) According to the atomic ratio of the VIII group metal element to the total amount of the VIII group metal element and the VIB group metal element, the amount of the VIII group metal precursor per gram of aluminum oxide is determined; (3) According to (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The content of the phosphorus-containing compound is calculated based on the value of , and then the amount of the phosphorus-containing compound in each gram of the carrier is determined; (4) the amount of the organic alcohol compound and / or the carboxylic acid compound containing -OH is calculated according to the molar ratio of the organic alcohol compound and / or the carboxylic acid compound containing -OH to the metal element of Group VIII; (5) according to the amount of the above-mentioned Group VIB metal precursor, Group VIII metal precursor, phosphorus-containing compound and organic alcohol compound and / or carboxylic acid compound containing -OH, the alumina is impregnated with the impregnation solution by the pore saturation impregnation method, and then dried. Specifically, a phosphorus-containing compound is first dissolved in water to obtain a phosphorus-containing aqueous solution, and then an organic alcohol compound and / or a carboxylic acid compound, a Group VIB metal precursor and a Group VIII metal precursor are added, and the mixture is stirred under heating until it is completely dissolved, and the temperature is maintained to obtain an impregnation solution; (6) the water absorption rate of alumina is measured, and the liquid absorption rate of alumina is calculated according to the formula of water absorption rate of alumina-0.1; (7) according to the liquid absorption rate of alumina, the volume of the impregnation solution is adjusted to a corresponding volume (alumina liquid absorption rate×carrier mass), and the impregnation solution and a corresponding mass of alumina are evenly mixed and allowed to stand, and then dried to prepare a hydrogenation catalyst.
[0065] The composition of the catalyst is calculated based on the feed amount. The pore distribution, pore size and pore volume of 2-100 nm in the catalyst and the carrier are determined by low temperature nitrogen adsorption method (see "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990). The sulfur mass fraction in the product is analyzed using a sulfur nitrogen analyzer (produced by Thermo Fisher, model TN / TS3000).
[0066] The hydrodesulfurization performance of the original catalyst was measured on a high-pressure small reactor. The upper bed was filled with 6 mL of an industrial catalyst, which was composed of 4.3% by weight of NiO, 27% by weight of MoO3, and 68.7% by weight of alumina. The lower bed was filled with 10 mL of the hydrogenation catalyst suitable for the high temperature section of the present invention. The oxidized catalyst was directly converted into a sulfurized catalyst using a programmed temperature sulfurization method. The sulfurization conditions were: the sulfurization pressure was 6.4 MPa, the sulfurized oil was kerosene containing 2% by weight of CS2, and the volume space velocity was 2 hours. -1, the hydrogen-to-oil volume ratio is 300v / v, first keep the temperature at 230℃ / h for 6h, then heat it up to 360℃ for sulfidation for 8h, and the heating rate of each stage is 10℃ / h. After sulfidation, switch the reaction raw materials for hydrodesulfurization activity test, the reaction raw materials are distillate oil with a sulfur content of 10890ppm. The test conditions are: pressure of 6.4MPa, volume space velocity of 1.875h -1 , the hydrogen-oil volume ratio is 300 v / v, and the reaction temperature is 370°C.
[0067] The activity of the catalyst is defined as the hydrodesulfurization reaction rate constant (k HDS ), the reaction order is calculated according to 1.2, and the calculation formula is: k HDS =1 / (n-1)×(s p (1-n) -s f (1-n) )×LHSV, where n is the reaction rate constant, S p is the sulfur content in the product, S f is the sulfur content in the raw materials.
[0068] The catalyst activity recovery degree is defined as: the ratio of the hydrodesulfurization reaction rate constant of the regenerated catalyst to the hydrodesulfurization reaction rate constant of the fresh catalyst×100%.
[0069] The programmed temperature oxidation method was carried out on a thermogravimetric mass spectrometer (NETZSCH STA 409PC / PG) instrument. The specific operating conditions were: air was used as the carrier gas, the flow rate of the carrier gas was 50 mL / min, the sample was heated from room temperature to 600°C at a heating rate of 10°C / min for a programmed temperature oxidation test, and a mass spectrometer was used to monitor the gas outlet of the instrument to obtain a curve of the sample decomposition product changing with temperature.
[0070] Example 1
[0071] (1) Preparation of catalyst (also known as protocatalyst)
[0072] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of 280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-20nm accounts for 66.8% of the total pore volume.
[0073] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0074] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0075] The atomic concentration of Mo in the catalyst is 4.5atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.2, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup It is 0.346nm, and the molar ratio of glycerol to Ni is 2.
[0076] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 192m 2 / g, pore volume 0.45cm 3 / g, the average pore diameter is 9.4nm, the pore volume with a pore diameter distribution of 8-20nm accounts for 63.0% of the total pore volume of the catalyst, and the pore diameter of the catalyst presents a single-peak pore distribution in the range of 8-20nm.
[0077] (2) Catalyst testing
[0078] The prepared catalyst was subjected to a hydrodesulfurization performance test, and the reaction was stopped after 30 days of operation, and the catalyst after the reaction was unloaded to obtain a spent catalyst. The components to be removed from the spent catalyst included carbon deposits and sulfides, and the carbon and sulfur contents in the spent catalyst were 5.9wt% and 7.2wt%, respectively.
[0079] (3) Regeneration of spent catalyst
[0080] The spent catalyst was subjected to a programmed temperature oxidation test, and it was determined that the number of peaks of the components to be removed of the spent catalyst was 2, the peak temperature of the first peak was 335°C, and the peak temperature of the second peak was 425°C.
[0081] The catalyst to be produced is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, the temperature is increased from room temperature to 335°C at a heating rate of 5°C / min, the temperature is kept constant for 5 hours, the temperature is then increased to 425°C at a heating rate of 2°C / min, the temperature is kept constant for 5 hours, and finally the temperature is increased to 450°C at a heating rate of 1°C / min and the temperature is kept constant for 4 hours to obtain a calcined product;
[0082] The calcined product was mixed evenly with a glycerol aqueous solution by an equal volume impregnation method, and dried at 130° C. for 3 h to obtain a regenerated catalyst, wherein the amount of glycerol used was 1.5 times the glycerol content in the original catalyst.
[0083] After the regenerated catalyst was retested for hydrodesulfurization performance, the activity recovery degree was 97%.
[0084] Example 2
[0085] (1) Preparation of catalyst
[0086] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of 280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-20nm accounts for 66.8% of the total pore volume.
[0087] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and allowed to stand for 2 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0088] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0089] The atomic concentration of Mo in the catalyst is 3atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.3, P2O5 / MoO3 molar ratio is 0.3, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.26 nm, and the molar ratio of glycerol to Ni is 5.
[0090] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption. The specific surface area of the catalyst is 210m 2 / g, pore volume 0.5cm 3 / g, the average pore diameter is 9.5nm, the pore volume with a pore diameter distribution of 8-20nm accounts for 65.8% of the total pore volume of the catalyst, and the pore diameter of the catalyst presents a single-peak pore distribution in the range of 8-20nm.
[0091] (2) Catalyst testing
[0092] The prepared catalyst was subjected to a hydrodesulfurization performance test, and the reaction was stopped after 30 days of operation, and the catalyst after the reaction was unloaded to obtain a spent catalyst. The components to be removed in the spent catalyst included carbon deposits and sulfides, and the carbon and sulfur contents in the spent catalyst were 5.5wt% and 6.5wt%, respectively.
[0093] (3) Regeneration of spent catalyst
[0094] The catalyst to be regenerated was subjected to a programmed temperature oxidation test, and it was determined that the number of peaks of the components to be removed of the catalyst to be regenerated was 2, the peak temperature of the first peak was 320°C, and the peak temperature of the second peak was 435°C.
[0095] The catalyst to be produced is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, the temperature is increased from room temperature to 320°C at a heating rate of 8°C / h, the temperature is kept constant for 5h, the temperature is then increased to 435°C at a heating rate of 3°C / min, the temperature is kept constant for 5h, and finally the temperature is increased to 465°C at a heating rate of 2°C / min and the temperature is kept constant for 4h to obtain a calcined product;
[0096] The calcined product was mixed evenly with a glycerol aqueous solution by an equal volume impregnation method, and dried at 130° C. for 3 h to obtain a regenerated catalyst, wherein the amount of glycerol used was 0.8 times the glycerol content in the original catalyst.
[0097] After the regenerated catalyst was retested for hydrodesulfurization performance, the activity recovery degree was 94%.
[0098] Example 3
[0099] (1) Preparation of catalyst
[0100] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of 280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-20nm accounts for 66.8% of the total pore volume.
[0101] A certain amount of MoO3, basic nickel carbonate, and glycerol were added to an aqueous solution containing phosphoric acid, heated and stirred at 95°C for 2 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution and the carrier were mixed evenly and then allowed to stand for 4 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0102] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0103] The atomic concentration of Mo in the catalyst is 3.5atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.28, P2O5 / MoO3 molar ratio is 0.25, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The nanostructured carbon fiber is 0.29 nm, and the molar ratio of glycerol to Ni is 3.
[0104] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 204m 2 / g, pore volume 0.48cm 3 / g, the average pore diameter is 9.4nm, the pore volume with a pore diameter distribution of 8-20nm accounts for 66.2% of the total pore volume of the catalyst, and the pore diameter of the catalyst presents a single-peak pore distribution in the range of 8-20nm.
[0105] (2) Catalyst testing
[0106] The prepared catalyst was subjected to a hydrodesulfurization performance test, and the reaction was stopped after 30 days of operation, and the catalyst after the reaction was unloaded to obtain a spent catalyst. The components to be removed in the spent catalyst included carbon deposits and sulfides, and the carbon and sulfur contents in the spent catalyst were 5.9wt% and 6.8wt%, respectively.
[0107] (3) Regeneration of spent catalyst
[0108] The spent catalyst was subjected to a programmed temperature oxidation test, and it was determined that the number of peaks of the components to be removed of the spent catalyst was 2, the peak temperature of the first peak was 325°C, and the peak temperature of the second peak was 445°C.
[0109] The catalyst to be produced is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, the temperature is increased from room temperature to 325°C at a heating rate of 10°C / h, the temperature is kept constant for 5h, the temperature is then increased to 445°C at a heating rate of 3°C / min, the temperature is kept constant for 5h, and finally the temperature is increased to 475°C at a heating rate of 2°C / min and the temperature is kept constant for 4h to obtain a calcined product;
[0110] The calcined product was mixed evenly with a glycerol aqueous solution by an equal volume impregnation method, and dried at 130° C. for 3 h to obtain a regenerated catalyst, wherein the amount of glycerol used was 1.2 times the glycerol content in the original catalyst.
[0111] After the regenerated catalyst was retested for hydrodesulfurization performance, the activity recovery degree was 96%.
[0112] Example 4
[0113] (1) Preparation of catalyst
[0114] The γ-alumina carrier was selected with a water absorption rate of 0.98 mL / g and a specific surface area of 280 m 2 / g, the average pore size is 10.7nm, the pore volume with a pore size of 2-6nm accounts for 8% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 4% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-20nm accounts for 66.8% of the total pore volume.
[0115] A certain amount of ammonium metatungstate, basic nickel carbonate and citric acid were added to the aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 2 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0116] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0117] The atomic concentration of W in the catalyst is 4atom / nm 2 , Ni / (Ni+W) atomic ratio is 0.3, P2O5 / WO3 molar ratio is 0.35, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.38 nm, and the molar ratio of citric acid to Ni is 2.
[0118] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 170m 2 / g, pore volume 0.4cm 3 / g, the average pore diameter is 9.4nm, the pore volume with a pore diameter distribution of 8-20nm accounts for 65.8% of the total pore volume of the catalyst, and the pore diameter of the catalyst presents a single-peak pore distribution in the range of 8-20nm.
[0119] (2) Catalyst testing
[0120] The prepared catalyst was subjected to a hydrodesulfurization performance test, and the reaction was stopped after 30 days of operation, and the catalyst after the reaction was unloaded to obtain a spent catalyst. The components to be removed in the spent catalyst included carbon deposits and sulfides, and the carbon and sulfur contents in the spent catalyst were 5.2wt% and 7.0wt%, respectively.
[0121] (3) Regeneration of spent catalyst
[0122] The catalyst to be regenerated was subjected to a programmed temperature oxidation method test, and it was determined that the number of peaks of the components to be removed of the catalyst to be regenerated was 2, the peak temperature of the first peak was 295°C, and the peak temperature of the second peak was 460°C.
[0123] The catalyst to be produced is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, the temperature is increased from room temperature to 295°C at a heating rate of 10°C / h, the temperature is kept constant for 5h, the temperature is then increased to 460°C at a heating rate of 3°C / min, the temperature is kept constant for 5h, and finally the temperature is increased to 470°C at a heating rate of 2°C / min and the temperature is kept constant for 4h to obtain a calcined product;
[0124] The calcined product was mixed evenly with a citric acid aqueous solution by an equal volume impregnation method, and dried at 130° C. for 3 hours to obtain a regenerated catalyst, wherein the amount of citric acid used was 1.5 times the citric acid content in the original catalyst.
[0125] After the regenerated catalyst was retested for hydrodesulfurization performance, the activity recovery degree was 97%.
[0126] Example 5
[0127] (1) Preparation of catalyst
[0128] The γ-alumina carrier was selected, with a water absorption rate of 1.04 mL / g and a specific surface area of 270 m 2 / g, the average pore size is 11.7nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, the pore size distribution is mainly concentrated in 8-20nm, and the pore volume with a pore size of 8-2nm accounts for 73.5% of the total pore volume.
[0129] A certain amount of MoO3, basic nickel carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 85°C for 4 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0130] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0131] The atomic concentration of Mo in the catalyst is 4.2atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.25, P2O5 / MoO3 molar ratio is 0.32, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.37 nm, and the molar ratio of citric acid to Ni is 2.
[0132] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 189m 2 / g, pore volume 0.48cm 3 / g, the average pore diameter is 10.2nm, the pore volume with a pore diameter distribution of 8-20nm accounts for 69.5% of the total pore volume of the catalyst, and the pore diameter of the catalyst presents a single-peak pore distribution in the range of 8-20nm.
[0133] (2) Catalyst testing
[0134] The prepared catalyst was subjected to a hydrodesulfurization performance test, and the reaction was stopped after 30 days of operation, and the catalyst after the reaction was unloaded to obtain a spent catalyst. The components to be removed in the spent catalyst included carbon deposits and sulfides, and the carbon and sulfur contents in the spent catalyst were 6.3wt% and 6.8wt%, respectively.
[0135] (3) Regeneration of spent catalyst
[0136] The catalyst to be regenerated was subjected to a programmed temperature oxidation method test, and it was determined that the number of peaks of the components to be removed of the catalyst to be regenerated was 2, the peak temperature of the first peak was 300°C, and the peak temperature of the second peak was 410°C.
[0137] The catalyst to be produced is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, with the temperature being increased from room temperature to 300°C at a heating rate of 6°C / h, and kept at the constant temperature for 5h, and then increased to 410°C at a heating rate of 3°C / min, and kept at the constant temperature for 5h, and finally increased to 430°C at a heating rate of 1°C / min, and kept at the constant temperature for 4h, to obtain a calcined product;
[0138] The calcined product was mixed evenly with a citric acid aqueous solution by an equal volume impregnation method, and dried at 130° C. for 3 h to obtain a regenerated catalyst, wherein the amount of citric acid used was 1 times the citric acid content in the original catalyst.
[0139] After the regenerated catalyst was retested for hydrodesulfurization performance, the activity recovery degree was 94%.
[0140] Example 6
[0141] (1) Preparation of catalyst
[0142] The γ-alumina carrier was selected, with a water absorption rate of 1.04 mL / g and a specific surface area of 270 m 2 / g, the average pore size is 11.7nm, the pore volume with a pore size of 2-6nm accounts for 5% of the total pore volume, the pore volume with a pore size of 2-4nm accounts for 1% of the total pore volume, and the pore size distribution is mainly concentrated in 8-20nm, accounting for 73.5%.
[0143] A certain amount of MoO3, basic nickel carbonate and citric acid were added to an aqueous solution containing phosphoric acid, heated and stirred at 90°C for 3 hours until completely dissolved, to obtain an impregnation solution containing active metals. The impregnation solution was mixed evenly with the carrier and then allowed to stand for 3 hours, and dried at 120°C for 5 hours to prepare a catalyst with a particle size of 1.6 mm and a butterfly shape.
[0144] The amounts of the alumina and the components are such that the prepared catalyst satisfies:
[0145] The atomic concentration of Mo in the catalyst is 4.5atom / nm 2 , Ni / (Ni+Mo) atomic ratio is 0.2, P2O5 / MoO3 molar ratio is 0.25, (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup is 0.36 nm, and the molar ratio of citric acid to Ni is 2.
[0146] After the catalyst was calcined at 400℃ for 3h, its pore size distribution was analyzed by low temperature nitrogen adsorption method. The specific surface area of the catalyst is 190m 2 / g, pore volume 0.47cm 3 / g, the average pore diameter is 9.9nm, the pore volume with a pore diameter distribution of 8-20nm accounts for 72.6% of the total pore volume of the catalyst, and the pore diameter of the catalyst presents a single-peak pore distribution in the range of 8-20nm.
[0147] (2) Catalyst testing
[0148] The prepared catalyst was subjected to a hydrodesulfurization performance test, and the reaction was stopped after 30 days of operation, and the catalyst after the reaction was unloaded to obtain a spent catalyst. The components to be removed in the spent catalyst included carbon deposits and sulfides, and the carbon and sulfur contents in the spent catalyst were 5.8wt% and 6.9wt%, respectively.
[0149] (3) Regeneration of spent catalyst
[0150] The catalyst to be regenerated was subjected to a programmed temperature oxidation test, and it was determined that the number of peaks of the components to be removed of the catalyst to be regenerated was 2, the peak temperature of the first peak was 310°C, and the peak temperature of the second peak was 415°C.
[0151] The catalyst to be produced is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, the temperature is increased from room temperature to 310°C at a heating rate of 6°C / h, the temperature is kept constant for 5h, the temperature is then increased to 415°C at a heating rate of 3°C / min, the temperature is kept constant for 5h, and finally the temperature is increased to 435°C at a heating rate of 1°C / min and the temperature is kept constant for 4h to obtain a calcined product;
[0152] The calcined product and the citric acid aqueous solution were mixed evenly by an equal volume impregnation method, and dried at 130° C. for 3 hours to obtain a regenerated catalyst, wherein the amount of citric acid used was 1 times the citric acid content in the original catalyst.
[0153] After the regenerated catalyst was retested for hydrodesulfurization performance, the activity recovery degree was 94%.
[0154] Example 7
[0155] The method is the same as Example 1, except that the last high-temperature calcination is not performed. Specifically, in step (3) of regenerating the catalyst to be regenerated, the catalyst to be regenerated is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere. The temperature is increased from room temperature to 335°C at a heating rate of 5°C / h, and the temperature is maintained for 5 hours. The temperature is then increased to 425°C at a heating rate of 2°C / h, and the temperature is maintained for 5 hours to obtain a regenerated catalyst.
[0156] After the regenerated catalyst was retested for hydrodesulfurization performance, the activity recovery degree was 91%.
[0157] Example 8
[0158] The method is the same as Example 1, except that, in step (3) of regenerating the catalyst to be regenerated, the catalyst to be regenerated is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, the temperature is increased from room temperature to 335°C at a heating rate of 5°C / h, the temperature is maintained at this temperature for 5 hours, the temperature is then increased to 425°C at a heating rate of 5°C / h, the temperature is maintained at this temperature for 5 hours, and finally the temperature is increased to 450°C at a heating rate of 5°C / h and the temperature is maintained at this temperature for 4 hours to obtain a calcined product.
[0159] After the regenerated catalyst was retested for hydrodesulfurization performance, the activity recovery degree was 92.8%.
[0160] Example 9
[0161] The method is the same as Example 1, except that, in step (3) of regenerating the catalyst to be regenerated, the catalyst to be regenerated is placed in a muffle furnace and subjected to programmed temperature calcination in an air atmosphere, the temperature is increased from room temperature to 335°C at a heating rate of 3°C / h, the temperature is maintained constant for 5 hours, the temperature is then increased to 425°C at a heating rate of 5°C / h, the temperature is maintained constant for 5 hours, and finally the temperature is increased to 450°C at a heating rate of 10°C / h and the temperature is maintained constant for 4 hours to obtain a calcined product.
[0162] After the regenerated catalyst was retested for hydrodesulfurization performance, the activity recovery degree was 89.5%.
[0163] Comparative Example 1
[0164] The method is the same as Example 1, except that, in step (3) of regenerating the spent catalyst, the spent catalyst is directly placed in a muffle furnace, and the temperature is increased from room temperature to 450°C at a heating rate of 5°C / h in an air atmosphere, and the temperature is maintained at this temperature for 14 hours to obtain a calcined product.
[0165] After the regenerated catalyst was retested for hydrodesulfurization performance, the activity recovery degree was 85.3%.
[0166] It can be seen from the examples and comparative examples that the present invention has good inventive effects, the catalyst regeneration method and the prepared regenerated catalyst have high activity and stability, and have good industrial application prospects.
[0167] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for regenerating a spent catalyst, characterized in that: The pore size of the original catalyst of the spent catalyst is in the range of 8-20 nm and presents a single peak pore distribution; the components to be removed in the spent catalyst include at least one of carbon deposits, sulfides, and nitrogen-containing organic matter; The regeneration method comprises: firstly performing a programmed temperature oxidation test on the catalyst to be regenerated to determine the peak quantity and peak temperature of the component to be removed, and then performing segmented roasting on the catalyst to be regenerated according to the peak quantity and peak temperature; In the programmed temperature oxidation test, the temperature is increased from room temperature to 500-800°C at a heating rate of 1-15°C / min; The peak number corresponds to the number of stages of staged roasting, and the peak temperature corresponds to the roasting temperature of each stage of roasting from low to high; The heating rate of each stage of calcination is independently selected from 1-20°C / min; The procatalyst comprises alumina and a Group VIII metal element, a Group VIB metal element and a phosphorus element supported on the alumina; The specific surface area of the original catalyst is 185-210m 2 / g; The total pore volume of the original catalyst is 0.4-0.6 cm 3 / g; The average pore size of the procatalyst is 6-18 nm; The volume of pores with a pore size distribution of 8-20 nm in the original catalyst accounts for 50-80% of the total pore volume of the original catalyst; The volume of pores with a pore size distribution between 2-4 nm in the procatalyst does not exceed 4% of the total pore volume of the procatalyst.
2. The regeneration method according to claim 1, wherein: The total pore volume of the original catalyst is 0.4-0.5 cm 3 / g.
3. The regeneration method according to claim 1, wherein: The average pore size of the procatalyst is 8-12 nm.
4. The regeneration method according to claim 1, wherein: The volume of pores with pore diameter distribution in the range of 8-20 nm in the original catalyst accounts for 60-75% of the total pore volume of the original catalyst.
5. The regeneration method according to claim 1, wherein: The volume of pores with a pore size distribution between 2-4 nm in the procatalyst does not exceed 1% of the total pore volume of the procatalyst.
6. The regeneration method according to claim 1, wherein: The original catalyst composition is as follows (Xi ai )•(Yi bi )•(Zi ci )•Sup represents, where Xi is a metal oxide of Group VIB, ai is the mass relative to 1 gram of carrier Xi, Yi is a metal oxide of Group VIII, bi is the mass relative to 1 gram of carrier Yi, Zi is P2O5, ci is the mass relative to 1 gram of carrier P2O5, Sup refers to the carrier in the catalyst, and its mass is calculated as 1 gram. The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value of is 0.18-0.39nm; Xi , Yi , Zi are the densities of Group VIB metal oxides, Group VIII metal oxides and P2O5, SA sup is the specific surface area of the carrier.
7. The regeneration method according to claim 6, wherein: The catalyst satisfies: (ai / ρ Xi +bi / ρ Yi +ci / ρ Zi ) / SA sup The value is 0.25-0.38nm.
8. The regeneration method according to claim 6, wherein: The molar ratio of Zi / Xi in the original catalyst is 0.1-0.35:
1.
9. The regeneration method according to claim 8, wherein: The molar ratio of Zi / Xi in the original catalyst is 0.2-0.35:
1.
10. The regeneration method according to claim 6, wherein: The atomic concentration of the VIB group metal element in the original catalyst on the carrier surface is 2-6atom / nm 2 .
11. The regeneration method according to claim 10, wherein: The atomic concentration of the VIB group metal elements in the original catalyst on the carrier surface is 3-4.5atom / nm 2 .
12. The regeneration method according to claim 6, wherein: The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the procatalyst is 0.2-0.
4.
13. The regeneration method according to claim 12, wherein: The atomic ratio of the Group VIII metal element to the total amount of the Group VIII metal element and the Group VIB metal element in the procatalyst is 0.2-0.
35.
14. The regeneration method according to any one of claims 1 to 12, wherein: The heating rate of each calcination stage is independently selected from 2-15°C / min.
15. The regeneration method according to any one of claims 1 to 12, wherein: The calcination time of each calcination stage is independently selected from 1 to 10 hours.
16. The regeneration method according to claim 15, wherein: The roasting time of each roasting stage is independently selected from 3 to 6 hours.
17. The regeneration method according to any one of claims 1 to 12, wherein: In the staged roasting, the heating rate of the first stage is the fastest.
18. The regeneration method according to claim 17, wherein: In the staged roasting, the heating rate of each stage decreases successively.
19. The regeneration method according to claim 18, wherein: Between adjacent roasting sections, the heating rate decreases by 1-10°C / min.
20. The regeneration method according to claim 19, wherein: Between adjacent roasting sections, the heating rate decreases by 2-7°C / min.
21. The regeneration method according to any one of claims 1 to 12, wherein: The regeneration method further comprises performing stable roasting after staged roasting, and the stable roasting comprises: raising the final temperature of the staged roasting by 10-50°C.
22. The regeneration method according to claim 21, wherein: The stable roasting comprises: raising the final temperature of the staged roasting by 15-30° C. for roasting.
23. The regeneration method according to claim 21, wherein: The heating rate of the stable calcination is 1-10°C / min.
24. The regeneration method according to claim 23, wherein: The heating rate of the stable calcination is 1-5°C / min.
25. The regeneration method according to claim 21, wherein: The calcination time of the stable calcination is 1-5h.
26. The regeneration method according to claim 25, wherein: The calcination time of the stable calcination is 2-4h.
27. The regeneration method according to claim 1, wherein: The procatalyst further comprises an alcohol compound and / or a carboxylic acid compound.
28. The regeneration method according to claim 27, wherein: The molar ratio of the organic alcohol compound and / or carboxylic acid compound to the metal element of Group VIII is 1-4.
29. The regeneration method according to claim 28, wherein: The molar ratio of the organic alcohol compound and / or carboxylic acid compound to the metal element of Group VIII is 2-5.
30. The regeneration method according to claim 27, wherein: The organic alcohol compound is selected from one or more of methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, heptanol, ethylene glycol, glycerol, tetramethylene glycol, polyethylene glycol, polyglycerol, pentaerythritol, xylitol, sorbitol and trimethylolethane.
31. The regeneration method according to claim 30, wherein: The organic alcohol compound is selected from one of glycerol and propanol.
32. The regeneration method according to claim 27, wherein: The carboxylic acid compound is selected from one or more of formic acid, acetic acid, propionic acid, citric acid, caprylic acid, adipic acid, malonic acid, succinic acid, maleic acid, valeric acid, caproic acid, capric acid, benzoic acid, phenylacetic acid, phthalic acid, terephthalic acid, valeric acid, caproic acid, capric acid, octadecanoic acid and tartaric acid.
33. The regeneration method according to claim 27, wherein: The carboxylic acid compound is selected from at least one of formic acid, citric acid and acetic acid.
34. The regeneration method according to any one of claims 27 to 33, further comprising: The calcined product obtained after the staged calcination and / or stable calcination is contacted with an organic alcohol compound and / or a carboxylic acid compound to obtain a regenerated catalyst.
35. The regeneration method according to claim 34, wherein: The organic alcohol compound and / or carboxylic acid compound are of the same type as the organic alcohol compound and / or carboxylic acid compound in the original catalyst.
36. The regeneration method according to claim 35, wherein: The amount of the organic alcohol compound and / or carboxylic acid compound added is 0.5-2 times the content of the organic alcohol compound and / or carboxylic acid compound in the original catalyst.
37. The regeneration method according to claim 35, wherein: The amount of the organic alcohol compound and / or carboxylic acid compound added is 0.75-1.5 times the content of the organic alcohol compound and / or carboxylic acid compound in the original catalyst.