Polyurethane road material and preparation method thereof
By combining the modified single-component polyurethane adhesive with stone, the coordinated action of ketoimine and Schiff base is used to accelerate the curing, and the gas adsorption through the porous material is solved, and the expansion rate of polyurethane highway materials in high temperature and low temperature environments is solved. The problem of slow curing speed achieves high strength, low expansion rate and rapid curing, extending the service life of the material.
Patent Information
- Application Number
- CN202111300090.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-11-04
AI Technical Summary
Existing polyurethane road materials are prone to bulging, have high expansion rates and slow curing speed in high temperature environments, making it difficult to meet the requirements of road materials.
The modified one-component polyurethane adhesive is combined with stone to form high-strength adhesive through prepolymerization, and Marshall compaction and curing are carried out in a humid environment, and the coordinated effect of ketoimine and Schiff base is used to accelerate the curing. Combined with porous materials, residual gas is adsorbed to reduce expansion rate.
The high strength, low expansion rate, rapid curing and long life of polyurethane road materials have been achieved, and the disadvantages of polyurethane adhesives in road materials have been solved, and the efficiency of road paving and the service life of materials have been improved.
Smart Images

Figure BDA0003338006920000021 
Figure BDA0003338006920000061 
Figure BDA0003338006920000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road material engineering, and in particular relates to a polyurethane road material and a preparation method thereof. Background Art
[0002] In the field of highway materials, asphalt concrete is currently widely used for highway paving and construction. my country has a hot summer and a cold and drastic temperature drop in winter. Asphalt road pavements are highly sensitive to temperature, prone to rutting at high temperatures and cracking at low temperatures, making it difficult to meet the requirements. Polyurethane has been widely studied as an adhesive to replace asphalt materials in recent years. Compared with asphalt materials, polyurethane is safe and environmentally friendly. As a high molecular polymer, it has high strength after molding and is not affected by temperature. It can reduce the thickness of the structural layer and save aggregates. It can be used in various highway pavement structures such as surface layers and base layers. However, when polyurethane adhesives are used in highway materials, there are still many disadvantages, such as being sensitive to humidity, prone to bubbles causing bulging, and slow curing in the later stage, which limits its application in the field of highway materials.
[0003] Patent CN106317371B modifies asphalt with polyurethane, which not only retains the elastic components of asphalt, but also solves the problem that the polymer system has high functionality and is very easy to stick to glue. However, the research is still based on asphalt, and the pain points of asphalt as a pavement material cannot be avoided; Patent CN111170678A uses a single-component polyurethane adhesive to prepare a castable concrete, which solves the problem of serious early disease and short service life of the steel bridge deck pavement layer, but the performance of the polyurethane adhesive is not clearly described, and it is impossible to meet the process requirements of long initial static time and short later maintenance and molding time.
[0004] Therefore, how to obtain a high-strength polyurethane highway material with a long open time, fast post-curing and low expansion rate and a preparation method thereof is of great significance. Summary of the invention
[0005] The purpose of the present invention is to provide a polyurethane road material and a preparation method thereof, which is made of polyurethane adhesive and stone. The adhesive of the present invention has a long operating time in the early stage, fast curing in the later stage and high bonding strength.
[0006] Another object of the present invention is to provide a method for preparing a polyurethane road material. The process is more suitable for using polyurethane as an adhesive material for road paving, and the final product has high strength, low expansion rate and long service life.
[0007] In order to achieve the above purpose, the present invention adopts the following technical solutions:
[0008] A polyurethane road material, comprising the following components:
[0009] Modified one-component polyurethane adhesive 1-10wt%, preferably 2-9wt%,
[0010] Stone 90-99wt%, preferably 91-98wt%;
[0011] Based on the total mass of the above components.
[0012] The modified one-component polyurethane adhesive comprises the following components:
[0013]
[0014] Based on the total mass of the above components.
[0015] In the present invention, the isocyanate is selected from one or more aromatic diisocyanates and their derivatives with NCO functionality ≥ 2, preferably polymethylene polyphenyl polyisocyanate, including but not limited to PM-200, PM-400, PM-700 of Wanhua Chemical. The grade of the stone selected in the present invention is AC-13.
[0016] The organic porous material in the present invention includes one or more of MOFs or COFs. MOFs are metal organic framework materials, which are a type of crystalline porous and high specific surface area materials with a periodic network structure formed by the self-assembly of inorganic metal centers and bridging organic ligands. COFs are organic covalent materials, which are organic porous crystalline materials formed by light atoms (hydrogen, boron, carbon, nitrogen, etc.) connected by covalent bonds. They are a type of large specific surface area material with a certain number and size of pore structures.
[0017] Furthermore, the MOFs or COFs in the present invention are preferably amino-functionalized MOFs or COFs materials, wherein amino-functionalized MOFs include but are not limited to MIL-125-NH2 and MIL-101-NH2, and amino-functionalized COFs include but are not limited to COF-JLU2 and COF-JLU3.
[0018] The ketimine in the present invention is prepared by the reaction of aliphatic amine and ketones. The aliphatic amine includes but is not limited to one or more of diethylenetriamine, m-phenylenediamine, m-phenylenediamine, triethylenetetramine, 1,3-BAC, preferably diethylenetriamine or triethylenetetramine; the ketone includes but is not limited to one or more of ACE, MEK, MIBK, MIPK, MTBK, DIPK, preferably one or more of MIBK, MIPK, MTBK, DIPK with a longer molecular chain.
[0019] Furthermore, the ketimine in the present invention preferably has a structure containing a secondary amine group (—NH—) in the molecule.
[0020] The Schiff base in the present invention is prepared by reacting lactams or their polymers with oxides or hydroxides of alkali metals or alkaline earth metals, or mixtures thereof. The structural formula of the Schiff base is n=3-11, preferably 3≤n≤5; lactams include but are not limited to one or more of laurolactam, decanolactam, enantholactam, ε-caprolactam, pyrrolidone lactam, preferably one or two of pyrrolidone lactam and ε-caprolactam. The preferred structural formula of Schiff base is
[0021] Furthermore, the mass ratio of ketimine to Schiff base is 5-1:1, preferably 4-1:1.
[0022] The present invention also provides a method for preparing a polyurethane road material, comprising the following steps:
[0023] 1) placing an organic porous material, ketimine, Schiff base and isocyanate in a reaction kettle, stirring at 25-45° C. for 1-5 hours under nitrogen protection to perform a prepolymerization reaction to obtain a modified one-component polyurethane binder;
[0024] 2) Mix the stone and modified one-component polyurethane adhesive evenly; weigh a certain amount of the mixture and place it at room temperature for curing for ≥3 hours, then put the mixture into a mold and compact the sample on both sides using a Marshall compactor; place the sample at a temperature of 20-40°C and a humidity of 60-90% for curing for ≤5 hours to obtain a high-strength polyurethane pavement sample.
[0025] Preferably, the sample is compacted on both sides 45-75 times using a Marshall compactor.
[0026] The polyurethane road material prepared by the invention has excellent performance, splitting strength ≥3MPa, freeze-thaw splitting strength ≥90%, expansion rate ≤1%, and initial operable time ≥3h.
[0027] In the present invention, the organic porous material, ketimine, and Schiff base can all react with isocyanate groups for prepolymerization to form a one-component adhesive with terminal isocyanate groups. Stir evenly with the stone in a certain proportion, let stand at room temperature, and then perform a Marshall compaction test, and then perform moisture curing on the sample block. Ketimine and Schiff base hydrolyze in a humid environment to generate primary amines, which react with isocyanates for rapid chain growth and rapid curing, and can be quickly opened to traffic in practical applications. The unreacted residual isocyanate groups will continue to react slowly with water in the air, and the generated CO2 can be adsorbed by porous MOFs / COFs materials with large specific surface areas, reducing the expansion rate and extending the service life of the road surface.
[0028] The positive effects of the present invention are:
[0029] 1) The present invention provides a feasible solution for the use of polyurethane for road paving, solves the disadvantages of polyurethane adhesives during use, has a long initial opening time, a fast curing speed in the later stage, high strength, low expansion deformation rate, and a long road life;
[0030] 2) The present invention partially blocks the isocyanate group by introducing a variety of substances containing active hydrogen, thereby reducing the -NCO% content, improving storage stability, reducing the initial sensitivity to water, and extending the operability time; the selected ketimine and Schiff base are long-chain structures, which can increase the structural flexibility after prepolymerization with isocyanate, reduce the rigidity of isocyanate, and increase the bonding performance of the polyurethane adhesive to the stone;
[0031] 3) The ketimine and Schiff base in the present invention both contain blocked amino groups. The isocyanate modified by them is mixed with stone and subjected to a Marshall compaction test. The sample is then subjected to moisture curing. The ketimine and Schiff base undergo hydrolysis reaction in a humid environment to generate primary amines, which undergo a rapid chain growth reaction with isocyanate. The sample is rapidly cured. In practical application, the construction period can be shortened and rapid traffic can be achieved.
[0032] 4) Ketimine and Schiff base in the present invention have good synergistic effect:
[0033] (a) Prepolymerization process: The prepolymerization of ketimine containing secondary amine groups with isocyanate has a slow reaction and a long prepolymerization time, which is prone to incomplete reaction, resulting in unstable performance indicators of the obtained adhesive. The present application adds a Schiff base containing a primary amine group to react with isocyanate for prepolymerization, thereby increasing the reaction rate of isocyanate and accelerating the rapid release of heat, so that the heat is released steadily during the polymerization process and the viscosity increases steadily. The final one-component polyurethane adhesive has good molecular weight distribution and storage stability.
[0034] (b) Hydrolysis process: This application uses a Schiff base with a specific n value range in combination with ketimine, which can better regulate the reaction rate of the Schiff base with ketimine and isocyanate and the curing and hardening speed. It not only improves the slow hydrolysis rate and curing and hardening rate of ketimine during curing, and the problem that the road material cannot be quickly hardened and opened to traffic; it can also make the viscosity of the entire system increase steadily during the hydrolysis process, and the curing rate proceeds steadily. When the two are used at the same time, the stress distribution of the entire bonding surface layer is uniform, avoiding stress concentration that affects the road life;
[0035] (c) Mechanical properties: After hydrolysis, ketimine unblocks four active hydrogen atoms and acts as a crosslinking agent when combined with isocyanate, which can increase the crosslinking strength of the polymer and improve the hardness of the final product. However, the product is relatively brittle, with poor adhesion and toughness, resulting in poor rutting resistance. After adding Schiff base, the Schiff base can react with isocyanate after hydrolysis to extend the chain, increase the polymer chain length, make it have strong adhesion, and increase the flexibility of the polymer, improve the rutting resistance of the pavement material, and improve the comprehensive mechanical properties of the polyurethane highway material.
[0036] 5) After the polyurethane pavement is paved, the residual isocyanate groups will continue to slowly react with water in the air to release CO2, causing the pavement to expand. The present invention uses a porous MOFs / COFs material with a large specific surface area containing amino functionalization to adsorb the gas generated by the reaction of the residual isocyanate groups. In addition, the amino group can react with the isocyanate to graft the porous material to the isocyanate group, preventing the porous material from sinking in the system, improving the gas adsorption efficiency, solving the pavement expansion problem caused by insufficient reaction of the polyurethane road, and extending the pavement life. DETAILED DESCRIPTION
[0037] The following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the rights claimed by the present invention.
[0038] The raw materials used in the following examples and comparative examples are described as follows:
[0039] PM200: Wanhua Chemical Group Co., Ltd.
[0040] Ketimine: prepared by the reaction of diethylenetriamine and methyl isopropyl ketone (MIPK), with the structural formula
[0041] Schiff base: Prepared by using an alkali metal hydroxide to initiate the anionic ring-opening polymerization of lactam. The specific method is as follows: add 50 parts of N, N-dimethylpropylene urea to a container, heat to 60°C, add 20 parts of bis(2,6-diisopropylphenyl)carbodiimide with stirring, mix evenly, control the temperature not to exceed 90°C after forming a transparent liquid, and add 20 parts of sodium hydroxide. Add the above liquid phase system and lactam at a ratio of 1:50 at 170°C with stirring to initiate polymerization. Remove stirring and keep the temperature constant for 1h to obtain Schiff base. Different lactam types determine the structure of the final Schiff base.
[0042] Schiff base-C3: The structural formula is The lactam used was pyrrolidone lactam, Anhui Wotu Chemical Co., Ltd.;
[0043] Schiff base-C5: The structural formula is The lactam used was ε-caprolactam, Hangzhou Jinshiyuan Pharmaceutical Chemical Co., Ltd.;
[0044] Schiff base-C6: The structural formula is The lactam selected is enantholactam, West Asia Chemical Technology (Shandong) Co., Ltd.;
[0045] MOFs materials: MIL-125-NH2, MIL-101-NH2, Xi'an Qiyue Biotechnology Co., Ltd.;
[0046] COFs materials: COF-JLU2, COF-JLU3, Xi’an Ruixi Biotechnology Co., Ltd.
[0047] Example 1
[0048] Preparation of polyurethane adhesive: 2g MIL-125-NH2, 1g COF-JLU2, 4g ketimine, 1g Schiff base-C3, and 92g PM200 were placed in a reactor, and stirred at 35°C for 2h under nitrogen protection for prepolymerization to obtain a modified one-component polyurethane binder;
[0049] Preparation of polyurethane highway specimens: 1900g aggregate gravel and 100g polyurethane binder were weighed according to the grade AC-13, and mixed in a mixing pot for 30s; the mixture was flattened and placed at room temperature for curing for 3h, then the mixture was placed in a mold, and the specimen was compacted 75 times on both sides using a Marshall compactor to produce a cylindrical specimen of 101.6mm±0.25mm and 63.5mm±1.3mm in height; the specimen was then placed in a constant temperature and humidity chamber at 30℃ and 80% humidity for curing for 5h to obtain a high-strength polyurethane pavement specimen. The splitting strength, expansion rate, and freeze-thaw splitting strength tests were then carried out.
[0050] The curing process of Examples 2-3 is the same as that of Example 1, except that the formula composition is different, as shown in Table 1; the formula composition of Examples 4-5 is the same as that of Example 1, except that the curing process is different, as shown in Table 2; the curing process of Comparative Examples 1-5 is the same as that of Example 1, except that the formula composition is different, as shown in Table 3.
[0051] The performance comparison of the materials obtained in various embodiments and comparative examples is shown in Table 4.
[0052] Table 1: Example formula (added amount is mass fraction)
[0053] raw material Embodiment 1, 4-5 Example 2 Example 3 Example 6 <![CDATA[MIL-125-NH2]]> 2 0 0 2 <![CDATA[MIL-101-NH2]]> 0 2 0 0 <![CDATA[COF-JLU2]]> 1 0 1 1 <![CDATA[COF-JLU3]]> 0 2 0 0 Ketimine 4 6 1.5 4 Schiff base-C3 1 3 0 0 Schiff base-C5 0 1 0.5 0 Schiff base-C6 0 0 0 1 PM200 92 86 97 92 Graded Stone 1900 4900 1011 1900
[0054] Table 2: Comparative Example Formula (Amount added is by mass)
[0055] raw material Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 <![CDATA[MIL-125-NH2]]> 0 3 0 2 2 <![CDATA[COF-JLU2]]> 0 0 0 1 1 Ketimine 4 0 4 0 4 Schiff base-C3 1 0 0 1 0 PM200 95 97 96 96 93 Graded Stone 1900 1900 1900 1900 1900
[0056] Table 3: Curing process of mixture and compacted samples
[0057]
[0058]
[0059] Table 4: Performance comparison of materials obtained from various examples and comparative examples
[0060] Splitting strength / MPa Expansion rate / % Freeze-thaw splitting strength / % Example 1 4.52 0.14 97.2 Example 2 4.14 0.24 96.5 Example 3 4.08 0.26 96.1 Example 4 4.48 0.17 96.9 Example 5 4.39 0.18 96.4 Example 6 4.01 0.27 95.9 Comparative Example 1 3.14 1.24 94.3 Comparative Example 2 3.24 1.03 93.5 Comparative Example 3 3.08 1.39 93.1 Comparative Example 4 4.09 0.25 96.2 Comparative Example 5 3.98 0.28 95.8
[0061] The freeze-thaw splitting strength is the retention rate of the splitting strength after a freeze-thaw cycle, with a low temperature of -18°C and a high temperature of 60°C. The expansion rate is the dimensional change rate of the sample before and after curing.
[0062] Those skilled in the art will appreciate that, based on the teachings of this specification, some modifications or adjustments may be made to the present invention, and these modifications or adjustments should also be within the scope defined by the claims of the present invention.
Claims
1. A polyurethane road material, characterized in that: Includes the following components: Modified one-component polyurethane adhesive 1-10wt%, Stone 90-99wt%, Based on the total mass of the above components; The modified one-component polyurethane adhesive comprises the following components: Based on the total mass of the above components; The organic porous material includes one or more of MOFs or COFs; The ketimine is prepared by reacting aliphatic amines and ketones; The Schiff base is prepared by reacting lactam or its polymer with oxide or hydroxide of alkali metal or alkaline earth metal, or a mixture thereof.
2. The polyurethane road material according to claim 1, characterized in that: Includes the following components: Modified one-component polyurethane adhesive 2-9wt%, Stone 91-98wt%; Based on the total mass of the above components.
3. The polyurethane road material according to claim 1, characterized in that: The modified one-component polyurethane adhesive comprises the following components: Based on the total mass of the above components.
4. The polyurethane road material according to claim 1, characterized in that: The isocyanate is selected from one or more aromatic diisocyanates with NCO functionality ≥ 2 and their derivatives.
5. The polyurethane road material according to claim 4, characterized in that: The isocyanate is polymethylene polyphenyl polyisocyanate.
6. The polyurethane road material according to claim 1, characterized in that: The gradation of the stone selected is AC-13.
7. The polyurethane road material according to claim 1, characterized in that: The MOFs or COFs are amino-functionalized MOFs or COFs materials.
8. The polyurethane road material according to claim 7, characterized in that: The amino-functionalized MOFs include but are not limited to MIL-125-NH2 and MIL-101-NH2, and the amino-functionalized COFs include but are not limited to COF-JLU2 and COF-JLU3.
9. The polyurethane road material according to any one of claims 1 to 7, characterized in that: The fatty amine includes one or more of diethylenetriamine, metaphenylenediamine, metaphenylenediamine, triethylenetetramine, and 1,3-BAC.
10. The polyurethane road material according to claim 9, characterized in that: The fatty amine is selected from diethylenetriamine or triethylenetetramine.
11. The polyurethane road material according to any one of claims 1 to 5, characterized in that: The ketones include one or more of ACE, MEK, MIBK, MIPK, MTBK, and DIPK.
12. The polyurethane road material according to claim 11, characterized in that: The ketones are selected from one or more of MIBK, MIPK, MTBK, and DIPK; 13. The polyurethane road material according to any one of claims 1 to 5, characterized in that: The ketimine molecule contains a secondary amine structure.
14. The polyurethane road material according to any one of claims 1 to 5, characterized in that: The structural formula of the Schiff base is n=3-11.
15. The polyurethane road material according to claim 14, characterized in that: In the structural formula of the Schiff base, 3≤n≤5.
16. The polyurethane road material according to claim 15, characterized in that: The structural formula of Schiff base is 17. The polyurethane road material according to any one of claims 1 to 5, characterized in that: The lactam includes, but is not limited to, one or more of laurolactam, caprolactam, enantholactam, ε-caprolactam, and pyrrolidone lactam.
18. The polyurethane road material according to claim 17, characterized in that: The lactam is one or both of pyrrolidone lactam and ε-caprolactam.
19. The polyurethane road material according to any one of claims 1 to 5, characterized in that: The mass ratio of ketimine to Schiff base is 5-1:
1.
20. The polyurethane road material according to claim 19, characterized in that: The mass ratio of ketimine to Schiff base is 4-1:
1.
21. A method for preparing the polyurethane road material according to any one of claims 1 to 20, comprising the following steps: 1) placing an organic porous material, ketimine, Schiff base and isocyanate in a reaction kettle, stirring at 25-45° C. for 1-5 hours under nitrogen protection to perform a prepolymerization reaction to obtain a modified one-component polyurethane binder; 2) Mix the stone and modified one-component polyurethane adhesive evenly; weigh a certain amount of the mixture and place it at room temperature for curing for ≥3 hours, then put the mixture into a mold and compact the sample on both sides using a Marshall compactor; place the sample at a temperature of 20-40°C and a humidity of 60-90% for curing for ≤5 hours to obtain a high-strength polyurethane pavement sample.
22. The preparation method according to claim 21, characterized in that: The specimens were compacted 45-75 times on both sides using a Marshall compactor.
Citation Information
Patent Citations
A method for preparing castor oil-based polyurethane modified bitumen and its mixture
CN106317371B
Pouring type concrete with polyurethane as binding material and preparation method of pouring type concrete
CN111170678A
Polyurethane polyurea modified asphalt mixture as well as preparation and application thereof
CN106145776A
Method for improving water stability of porous polyurethane mixture
CN110255972A