Electrically insulating thermoplastic composite material with core layer structure and preparation method and application thereof

By using a multi-component material system design in long fiber reinforced thermoplastic composite materials to form a core layer structure, the problems of improving electrical insulation performance and difficult to control the doping behavior of nanoparticles are solved, and the fiber fluidity and surface performance are improved, and the expansion is achieved. Application scope.

CN116063778BActive Publication Date: 2024-11-19CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111278004.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-30
Publication Date
2024-11-19
Estimated Expiration
2041-10-30

AI Technical Summary

Technical Problem

There is room for improvement in the electrical insulation performance of existing long fiber reinforced thermoplastic composites, and the doping behavior of nanoparticles is difficult to control, resulting in a degradation of insulation performance, limiting its application in actual engineering.

Method used

Designed with a multi-component material system, an electrically insulating thermoplastic composite material with a core layer structure is formed, including an inner layer material and an outer layer material. The inner layer material is composed of a continuous fiber bundle, a first thermoplastic resin and a first additive, and the outer layer is The material consists of a second thermoplastic resin and a second additive, and achieves excellent electrical insulation properties by adjusting the performance of each component.

Benefits of technology

It improves the flowability of fibers in resin melt and the surface performance of composite materials, expands the scope of application, and achieves excellent electrical insulation performance and comprehensive performance improvement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116063778B_ABST
    Figure CN116063778B_ABST
Patent Text Reader

Abstract

The present invention discloses an electrically insulating thermoplastic composite material with a core layer structure, and a preparation method and application thereof. The electrically insulating thermoplastic composite material comprises an inner layer material and at least one outer layer material, wherein the inner layer material is a core layer comprising a fiber bundle, a first thermoplastic resin and a first auxiliary agent, and the at least one outer layer material wraps the core layer and is a resin layer comprising a second thermoplastic resin and a second auxiliary agent, wherein the fiber bundle extends continuously from one end of the core layer to its opposite end, and the first auxiliary agent and the second auxiliary agent each independently comprise a polypropylene graft containing anhydride groups, which comprises a structural unit derived from copolymerized polypropylene, a structural unit derived from a maleic anhydride monomer, and a structural unit derived from an olefin-containing polymerization monomer. The electrically insulating thermoplastic composite material of the present invention is designed based on a multi-component material system, which can achieve a synergistic effect of performance between the components, and at the same time has excellent electrical insulation properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer composite materials, specifically relating to an electrically insulating thermoplastic composite material with a core layer structure, its preparation method, and its application. Background Technology

[0002] Long fiber reinforced thermoplastic composites are a common type of thermoplastic composite material and one of the fastest-growing materials in the composite materials market today. As both semi-structural and structural materials, long fiber reinforced thermoplastic composites are being developed for various industrial and civilian applications, including automotive, machinery, entertainment, food processing, communications, electronics, power tools, and horticulture.

[0003] Long-fiber reinforced thermoplastic materials have fiber lengths equal to particle lengths and highly consistent fiber orientation, possessing characteristics such as low density, easy molding, high specific strength, high modulus, good fatigue resistance, and non-absorbency. Furthermore, this material exhibits good dimensional stability, excellent impact resistance, chemical stability (resistance to salt, oil, and fuels), and recyclability. Polypropylene, as a simple-structured polymer, possesses good electrical insulation properties and a high melting point; however, the mechanical properties of pure polypropylene, especially at low temperatures, are brittle and cannot meet operational requirements. Long-fiber polypropylene materials show significant improvements in mechanical properties, while their electrical insulation properties still have room for adjustment and improvement. With the continuous improvement of long-fiber reinforced thermoplastic composite technology and the expansion of application cases, in addition to excellent mechanical and processing properties, good electrical insulation properties are also required. Currently, a large amount of literature and data indicates that modification with nanoparticles is an effective way to improve electrical insulation performance. However, in actual preparation, difficulties arise in controlling the doping behavior of nanoparticles, leading to the problem that nanoparticles easily aggregate, resulting in a decrease in insulation performance, thus limiting its widespread application in practical engineering.

[0004] The existing technology is far from meeting the needs of practical applications in addressing the aforementioned problems. Summary of the Invention

[0005] To address the aforementioned problems in existing technologies, this invention provides an electrically insulating thermoplastic composite material with a core layer structure, its preparation method, and its applications. This electrically insulating thermoplastic composite material is designed based on a multi-component material system, enabling synergistic performance among the components while exhibiting excellent electrical insulation properties. Furthermore, this electrically insulating thermoplastic composite material can significantly improve the flowability of fibers in the resin melt, greatly enhancing the surface properties of the composite material and expanding its application range.

[0006] A first aspect of the present invention provides an electrically insulating thermoplastic composite material having a core layer structure, comprising an inner layer material and at least one outer layer material. The inner layer material is a core layer comprising fiber bundles, a first thermoplastic resin, and a first additive. The at least one outer layer material encapsulates the core layer and is a resin layer comprising a second thermoplastic resin and a second additive. The fiber bundles extend continuously from one end of the core layer to its opposite end. The first additive and the second additive each independently comprise a polypropylene graft containing anhydride groups, comprising structural units derived from copolymer polypropylene, structural units derived from maleic anhydride monomers, and structural units derived from alkenyl-containing polymeric monomers.

[0007] The inventors of this application have discovered that by impregnating a continuous fiber bundle with a first component comprising a first thermoplastic resin and a first additive to form a core layer, and uniformly coating the outside of the core layer with a second component comprising a second thermoplastic resin, an electrically insulating thermoplastic composite material is formed, with a continuous fiber-reinforced resin as the core layer (inner layer material) and a resin layer surrounding the core layer as the outer layer material. Such a thermoplastic composite material exhibits excellent electrical insulation properties. Furthermore, by adjusting the properties and functions of the first thermoplastic resin in the core layer and the second thermoplastic resin in the resin layer, the electrically insulating thermoplastic composite material can be made to have different properties and functions.

[0008] In some embodiments of the electrically insulating thermoplastic composite material according to the present invention, the outer layer material (resin layer) may substantially continuously cover the inner layer material (core layer). Although not preferred, in the electrically insulating thermoplastic composite material of the present invention, the outer layer material (resin layer) covers at least 80% of the inner layer material (core layer), for example, 80-99% or 85-95% of the inner layer material (core layer).

[0009] In this invention, the terms "one end" and / or "opposite end" are generally used in relation to the longitudinal direction of the electrically insulating thermoplastic composite material.

[0010] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, the electrically insulating thermoplastic composite material can be in the form of strips, rods, or granules. Of course, the electrically insulating thermoplastic composite material of the present invention can also be in other shapes, such as continuous filaments. In the present invention, the strip-shaped, rod-shaped, or granular electrically insulating thermoplastic composite material can be cut from continuous filament electrically insulating thermoplastic composite material.

[0011] In some embodiments, the electrically insulating thermoplastic composite material is in the form of strips, rods, or granules. The length (longitudinal dimension) of the strip, rod, or granular electrically insulating thermoplastic composite material can be 5-30 mm, preferably 5-25 mm, and more preferably 6-15 mm.

[0012] In other embodiments, although not preferred, the electrically insulating thermoplastic composite material may also have a relatively small length dimension. For example, the electrically insulating thermoplastic composite material may be granular, and the particle size (length) of the granular electrically insulating thermoplastic composite material may be 2-5 mm, preferably 3-4 mm.

[0013] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, the present invention does not have special requirements on the cross-sectional shape of the electrically insulating thermoplastic composite material. In some embodiments, the cross-section of the granular or rod-shaped electrically insulating thermoplastic composite material is circular or near-circular. In other embodiments, the cross-section of the granular or strip-shaped electrically insulating thermoplastic composite material can be rectangular or square.

[0014] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, in the inner layer material, the amount of the first thermoplastic resin is 1-90 parts by weight, and the amount of the fiber bundle is 10-110 parts by weight.

[0015] In some specific embodiments, the amount of the first thermoplastic resin in the inner layer material can be 1 part by weight, 10 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, or a range thereof; and in some specific embodiments, the amount of the fiber bundle can be 1 part by weight, 10 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, 100 parts by weight, 110 parts by weight, or a range thereof.

[0016] In some preferred embodiments, the amount of the first thermoplastic resin in the inner layer material can be 20-70 parts by weight, preferably 20-55 parts by weight, more preferably 24-45 parts by weight; and / or the amount of the fiber bundle can be 20-110 parts by weight, more preferably 25-110 parts by weight.

[0017] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, the amount of the second thermoplastic resin in the outer layer material is 1-110 parts by weight.

[0018] In some specific embodiments, the amount of the second thermoplastic resin in the outer layer material can be 1 part by weight, 10 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight, 90 parts by weight, 95 parts by weight, 100 parts by weight, 105 parts by weight, 110 parts by weight, or a range thereof.

[0019] In some preferred embodiments, the amount of the second thermoplastic resin in the outer layer material can be 10-99 parts by weight, more preferably 10-90 parts by weight, and more preferably 40-90 parts by weight.

[0020] According to some specific embodiments of the electrically insulating thermoplastic composite material of the present invention, in the inner layer material, the amount of the first thermoplastic resin is 1-90 parts by weight, preferably 20-70 parts by weight, more preferably 20-55 parts by weight, and even more preferably 24-45 parts by weight; and / or the amount of the fiber bundle is 10-99 parts by weight, preferably 20-80 parts by weight, and more preferably 25-50 parts by weight.

[0021] According to some specific embodiments of the electrically insulating thermoplastic composite material of the present invention, in the inner layer material, the amount of the first thermoplastic resin is 50-70 parts by weight, more preferably 50-60 parts by weight; and / or the amount of the fiber bundle is 90-110 parts by weight, preferably 100-110 parts by weight; and / or in the outer layer material, the amount of the second thermoplastic resin is 90-110 parts by weight, more preferably 95-105 parts by weight.

[0022] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, in the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin is 0.25-6:1. For example, in the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin is 0.25:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, 0.55:1, 0.6:1, 0.65:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.2:1, 1.5:1, 1.7:1, 1.8:1, 1.9:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 6:1, or a range thereof.

[0023] In some preferred embodiments, the weight ratio of the fiber bundle to the first thermoplastic resin in the inner layer material can be 0.35-4.5:1, preferably 1.7-4.5:1.

[0024] In this invention, the dosage of the first and second adjuvants is limited in order to achieve the desired effect of the adjuvants.

[0025] In different embodiments of the present invention, the number of outer layer materials is not limited; the outer layer material may be one layer or multiple layers. When the outer layer material is multi-layered, the multi-layered outer layer material may be formed using one type of outer layer material or multiple types of outer layer materials.

[0026] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, the first thermoplastic resin and the second thermoplastic resin may be the same or different, and each is independently selected from at least one of polypropylene, polyethylene, polystyrene, polyvinyl chloride, polyacrylonitrile-butadiene-styrene copolymer, polyacrylonitrile-styrene copolymer, polyoxymethylene, polyamide, polyethylene terephthalate, polybutylene terephthalate, polymethyl methacrylate, polycarbonate, polyphenylene ether, polyurethane, polyetheretherketone and polyphenylene sulfide, and their alloy polymers.

[0027] According to a preferred embodiment of the electrically insulating thermoplastic composite material of the present invention, the first thermoplastic resin and the second thermoplastic resin are each independently selected from at least one of polypropylene, polyethylene, polyamide (also known as nylon), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyphenylene sulfide, polyurethane, and polyetheretherketone (PEEK).

[0028] According to a preferred embodiment of the electrically insulating thermoplastic composite material of the present invention, the first thermoplastic resin and the second thermoplastic resin are each independently selected from at least one of homopolymer polypropylene, copolymer polypropylene, a mixture of homopolymer polypropylene and copolymer polypropylene, nylon 6 (PA6), nylon 66 (PA66), and a mixture of nylon 6 and nylon 66.

[0029] In other embodiments of the electrically insulating thermoplastic composite material according to the present invention, the first thermoplastic resin and the second thermoplastic resin may also be selected from thermoplastic polyurethane elastomer (TPU) and / or high-temperature nylon (PPA).

[0030] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg is 60-8000 g / 10 min. For example, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg can be 60 g / 10 min, 100 g / 10 min, 200 g / 10 min, 450 g / 10 min, 500 g / 10 min, 1000 g / 10 min, 1500 g / 10 min, 2000 g / 10 min, 3000 g / 10 min, 4000 g / 10 min, 5000 g / 10 min, 6000 g / 10 min, 7000 g / 10 min, 7500 g / 10 min, 8000 g / 10 min, or a range thereof.

[0031] In some preferred embodiments, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg can be 100-8000 g / 10 min, preferably 1000-7500 g / 10 min, and more preferably 1900-7500 g / 10 min.

[0032] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is 0.1-8000 g / 10 min. For example, the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg can be 0.1 g / 10 min, 1 g / 10 min, 1.5 g / 10 min, 3 g / 10 min, 10 g / 10 min, 20 g / 10 min, 30 g / 10 min, 40 g / 10 min, 45 g / 10 min, 50 g / 10 min, 55 g / 10 min, 60 g / 10 min, 70 g / 10 min, 80 g / 10 min, etc. 90g / 10min, 100g / 10min, 450g / 10min, 500g / 10min, 800g / 10min, 1000g / 10min, 1500g / 10min, 1900g / 10min, 2500g / 10min, 3000g / 10min, 4000g / 10min, 5000g / 10min, 6000g / 10min, 7000g / 10min, 8000g / 10min, or a range thereof.

[0033] In some preferred embodiments, the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg can be 3-55 g / 10 min or 450-8000 g / 10 min, preferably 3-45 g / 10 min or 1900-8000 g / 10 min.

[0034] In different embodiments of the present invention, the melt flow rates of the first thermoplastic resin and the second thermoplastic resin are not particularly specific, and the melt flow rates of the first thermoplastic resin and the second thermoplastic resin can be selected according to the desired performance.

[0035] In particular, the inventors of this application have discovered that, according to the parameters of the present invention (e.g., melt flow rate), electrically insulating thermoplastic composite materials with high surface quality and overall performance can be prepared. For example, if the melt flow rate of the first thermoplastic resin is higher than that of the second thermoplastic resin, the electrically insulating thermoplastic composite material can have improved mechanical properties; conversely, if the melt flow rate of the second thermoplastic resin is higher than that of the first thermoplastic resin, the electrically insulating thermoplastic composite material can have improved gloss.

[0036] In some preferred embodiments of the electrically insulating thermoplastic composite material according to the present invention, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg is 60-450 g / 10 min, for example, 60-200 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is 3-55 g / 10 min or 450-8000 g / 10 min. In some specific embodiments, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg is 60-450 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is 800-8000 g / 10 min.

[0037] According to some preferred embodiments of the electrically insulating thermoplastic composite material of the present invention, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg is 450 g / 10 min or more, particularly greater than 450 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is less than 100 g / 10 min, preferably 1.5-55 g / 10 min, more preferably 3-50 g / 10 min.

[0038] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is 0.05-12.5:1. For example, the weight ratio of the second thermoplastic resin to the first thermoplastic resin can be 0.05:1, 0.1:1, 0.14:1, 0.15:1, 0.18:1, 0.2:1, 0.25:1, 0.3:1, 0.5:1, 0.8:1, 1:1, 1.2:1, 1.3:1, 1.4:1, 1.7:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 5:1, 8:1, 10:1, 12.5:1, or a range thereof.

[0039] In some preferred embodiments, the weight ratio of the second thermoplastic resin to the first thermoplastic resin can be 0.1-4:1, preferably 0.14-3.5:1.

[0040] According to a preferred embodiment of the electrically insulating thermoplastic composite material of the present invention, when the melt flow rate of the second thermoplastic resin is 800-8000 g / 10 min at 230°C and a load of 2.16 kg, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is less than 0.25:1, preferably less than 0.18:1, and more preferably less than 0.15:1.

[0041] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, when the first thermoplastic resin and the second thermoplastic resin are selected from at least one of nylon 6, nylon 66, and a mixture of nylon 6 and nylon 66, the viscosity of the selected nylon 6 and nylon 66 is 1.8-3.5. Wherein, the viscosity of nylon in the present invention is the relative viscosity measured according to the Engler viscosity determination method GB / T266-88.

[0042] According to a specific embodiment of the electrically insulating thermoplastic composite material of the present invention, the first thermoplastic resin and the second thermoplastic resin can be prepared in-house or commercially available.

[0043] For example, polypropylene resin of grade PPB-M100-GH purchased from Sinopec Yangzi Petrochemical Company, polypropylene resin of grade M60RHC purchased from Sinopec East China Branch, and nylon 6 of grade PA6-BL3200H purchased from Sinopec Baling Branch can be used as the first thermoplastic resin.

[0044] For example, polypropylene resin of grade PPB-M100-GH purchased from Sinopec Yangzi Petrochemical Company, polypropylene resin of grade PPH-T03 purchased from Sinopec Maoming Branch, polypropylene resin of grade M50RH purchased from Sinopec East China Branch, polypropylene resin of grade K8303 purchased from Yanshan Petrochemical Company, polypropylene resin of grade PF1500 purchased from Hunan Shengjin New Materials Co., Ltd., or polypropylene resin of grade PPH-Y450 purchased from Sinopec Shijiazhuang Refining and Chemical Branch, or nylon 6 of grade PA6-BL3200H purchased from Sinopec Baling Branch can be used as the second thermoplastic resin.

[0045] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, the fiber bundle is selected from at least one of glass fiber, carbon fiber, basalt fiber, aromatic polyamide fiber, stainless steel fiber, synthetic resin fiber and mineral fiber.

[0046] In a preferred embodiment of the electrically insulating thermoplastic composite material according to the present invention, the glass fiber is continuous glass fiber and / or fixed-length glass fiber.

[0047] Suitable fiber bundles for use in this invention may be alkali-free glass fiber of grade SE4805 purchased from Owens Corning (Shanghai) Glass Fiber Co., Ltd., alkali-free glass fiber of grade ER4301H purchased from Chongqing International Composite Materials Co., Ltd., carbon fiber of grade T700SC purchased from Toray Industries, Inc. of Japan, or basalt fiber purchased from Mudanjiang Jinshi Basalt Fiber Co., Ltd.

[0048] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, in the transverse cross-section of the electrically insulating thermoplastic composite material, a core layer and a resin layer are arranged sequentially from the inside to the outside; the fiber bundles are oriented longitudinally along the electrically insulating thermoplastic composite material. Preferably, in the present invention, the length of the fiber bundles is substantially the same as the length (longitudinal dimension) of the electrically insulating thermoplastic composite material, thereby the fiber bundles extend continuously from one end of the core layer in the longitudinal direction to the opposite end in the longitudinal direction.

[0049] In some preferred embodiments, the fiber bundles may be dispersed. Such dispersion methods are known in the art, and the present invention does not specifically limit them.

[0050] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, the inner layer material does not contain short fibers, particularly non-oriented short fibers.

[0051] In some specific embodiments, the inner layer material is composed of fiber bundles, a first thermoplastic resin, and a first additive.

[0052] In some embodiments of the electrically insulating thermoplastic composite material according to the present invention, the outer layer material is fiber-free. In some preferred embodiments, the outer layer material is composed of a second thermoplastic resin and a second additive.

[0053] In some other embodiments of the electrically insulating thermoplastic composite material according to the present invention, the outer layer material contains fibers, such as short fibers.

[0054] In some specific embodiments, the weight ratio of the fiber to the second thermoplastic resin in the outer layer material is 1-50:100, preferably 5-50:100, and more preferably 20-45:100.

[0055] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, based on 100 parts by weight of the first thermoplastic resin and the second thermoplastic resin, each of the first and second additives independently comprises 2-30 parts by weight of an electrically insulating modifier, preferably each independently comprising 5-25 parts by weight of an electrically insulating modifier. This electrically insulating modified material is prepared according to CN202011190993.5.

[0056] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, the electrically insulating modifier is a polypropylene graft containing anhydride groups, comprising structural units derived from copolymer polypropylene, structural units derived from maleic anhydride monomers, and structural units derived from alkenyl polymeric monomers; based on the weight of the polypropylene graft containing anhydride groups, the content of structural units derived from maleic anhydride monomers and alkenyl polymeric monomers in the grafted state in the polypropylene graft containing anhydride groups is 0.1-5% by weight, preferably 0.4-3% by weight; and the molar ratio of structural units derived from maleic anhydride monomers to structural units derived from alkenyl polymeric monomers in the polypropylene graft containing anhydride groups is 1:1-20, preferably 1:1-10.

[0057] The polypropylene graft containing anhydride groups has at least one of the following characteristics: a melt flow rate of 0.01-30 g / 10 min at 230°C and 2.16 kg load, preferably 0.05-20 g / 10 min, more preferably 0.1-10 g / 10 min, and even more preferably 0.2-8 g / 10 min.

[0058] The polypropylene graft containing anhydride groups, wherein the comonomer of the copolymer polypropylene is selected from at least one of C2-C8 α-olefins other than propylene; preferably, the comonomer of the copolymer polypropylene is selected from at least one of ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-octene; more preferably, the comonomer of the copolymer polypropylene is ethylene and / or 1-butene; more preferably, the copolymer polypropylene is composed of propylene and ethylene.

[0059] The polypropylene graft containing anhydride groups, wherein the alkenyl-containing polymeric monomer is selected from at least one monomer having the structure shown in Formula VII.

[0060]

[0061] In Formula VII, R1, R2, and R3 are each independently selected from H, substituted or unsubstituted alkyl groups; R4 is selected from substituted or unsubstituted alkyl groups, substituted or unsubstituted alkoxy groups, substituted or unsubstituted aryl groups, substituted or unsubstituted ester groups, substituted or unsubstituted carboxyl groups, substituted or unsubstituted cycloalkyl or heterocyclic groups, and cyano groups.

[0062] Preferably, R1, R2, and R3 are each independently selected from H, substituted or unsubstituted C1-C6 alkyl groups; more preferably, R1 R1, R2, and R3 are each independently selected from H, substituted or unsubstituted C1-C3 alkyl groups; preferably, R4 is selected from substituted or unsubstituted C1-C3 alkyl groups. 20 Alkyl, substituted or unsubstituted C1-C 20 Alkoxy, substituted or unsubstituted C6-C 20 aryl, substituted or unsubstituted C1-C 20 Ester group, substituted or unsubstituted C1-C 20 Carboxyl, substituted or unsubstituted C3-C 20 The substituted group is a cycloalkyl or heterocyclic group, or a cyano group, wherein the substituted group is a halogen, hydroxyl, amino, C1-C6 alkyl, or C3-C6 cycloalkyl; more preferably, R4 is selected from substituted or unsubstituted C1-C6 groups. 12 Alkyl, substituted or unsubstituted C1-C 18 Alkoxy, substituted or unsubstituted C6-C 12 aryl, substituted or unsubstituted C1-C 12 Ester group, substituted or unsubstituted C1-C 12 Carboxyl group, substituted or unsubstituted C3-C 12 The substituted group is a cycloalkyl or heterocyclic group, or a cyano group, wherein the substituted group is a halogen, a C1-C6 alkyl group, or a C3-C6 cycloalkyl group; more preferably, R4 is selected from substituted or unsubstituted C1-C6 alkyl groups, substituted or unsubstituted C1-C6 cycloalkyl groups, or C3-C6 cycloalkyl groups. 12Alkoxy, substituted or unsubstituted C6 -C8 aryl, substituted or unsubstituted C1-C6 ester, substituted or unsubstituted C1-C6 carboxyl, substituted or unsubstituted C3-C6 cycloalkyl or heterocyclic, cyano; preferably, the heterocyclic group is selected from imidazole, pyrazol, carbazole, pyrrolidone, pyridinyl, piperidinyl, caprolactam, pyrazinyl, thiazolyl, purine, morpholinyl, oxazolinyl.

[0063] The polypropylene graft containing anhydride groups, wherein R1, R2, and R3 are each independently selected from H, substituted or unsubstituted C. 1- C6 alkyl;

[0064] R4 is selected from the group shown in Formula VIII, the group shown in Formula IX, the group shown in Formula X, the group shown in Formula XI, a combination of the group shown in Formula XI and the group shown in Formula XII, and heterocyclic groups;

[0065]

[0066] In formula VIII, R4-R8 are each independently selected from H, halogen, hydroxyl, amino, phosphate group, sulfonic acid group, substituted or unsubstituted C1-C. 12 Alkyl, substituted or unsubstituted C3-C 12 cycloalkyl, substituted or unsubstituted C1-C 12 alkoxy, substituted or unsubstituted C1-C 12 ester group, substituted or unsubstituted C1-C 12 The substituted amino group, wherein the substituted group is selected from halogen, hydroxyl, amino, phosphate, sulfonic acid, C1-C 12 Alkyl, C3-C 12 cycloalkyl, C1-C 12 alkoxy groups, C1-C 12 ester group, C1-C 12 The amino group; preferably, R4-R8 are each independently selected from H, halogen, hydroxyl, amino, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C1-C6 alkoxy;

[0067]

[0068] In equation IX, R4-R 10 Each is independently selected from H, halogen, hydroxyl, amino, phosphate group, sulfonic acid group, substituted or unsubstituted C1-C. 12 Alkyl, substituted or unsubstituted C3-C 12 cycloalkyl, substituted or unsubstituted C1-C 12 alkoxy, substituted or unsubstituted C1-C 12 ester group, substituted or unsubstituted C1-C12 The substituted amino group, wherein the substituted group is selected from halogen, hydroxyl, amino, phosphate, sulfonic acid, C1-C 12 Alkyl, C3-C 12 cycloalkyl, C1-C 12 alkoxy groups, C1-C 12 ester group, C1-C 12 The amino group; preferably, R4-R 10 Each of the groups is independently selected from H, halogen, hydroxyl, amino, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C1-C6 alkoxy, wherein the substituted group is selected from halogen, hydroxyl, amino, C1-C6 alkyl, C1-C6 alkoxy;

[0069]

[0070] In formula X, R4'-R 10 Each group is independently selected from H, halogen, hydroxyl, amino, phosphate, sulfonic acid, substituted or unsubstituted C1-C. 12 Alkyl, substituted or unsubstituted C3-C 12 cycloalkyl, substituted or unsubstituted C1-C 12 alkoxy, substituted or unsubstituted C1-C 12 ester group, substituted or unsubstituted C1-C 12 The substituted amino group, wherein the substituted group is selected from halogen, hydroxyl, amino, phosphate, sulfonic acid, C1-C 12 Alkyl, C3-C 12 cycloalkyl, C1-C 12 alkoxy, C 1- C 12 ester group, C1-C 12 The amino group; preferably, R4'-R 10 Each of the following is independently selected from H, halogen, hydroxyl, amino, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C1-C6 alkoxy, wherein the substituted group is selected from halogen, hydroxyl, amino, C1-C6 alkyl, C1-C6 alkoxy;

[0071]

[0072] In formula XI, Rm is selected from the following groups, substituted or unsubstituted: C1-C 20 Straight-chain alkyl, C3-C 20 Branched alkyl, C3-C 12 cycloalkyl, C3-C 12 Epoxyalkyl, C3-C 12 Epoxyalkyl, wherein the substituted group is selected from at least one of halogen, amino and hydroxyl groups.

[0073] The polypropylene graft containing anhydride groups, wherein the alkenyl-containing polymeric monomer is selected from at least one of vinyl acetate, styrene, α-methylstyrene, (meth)acrylate, vinyl alkyl ether, vinylpyrrolidone, vinylpyridine, vinylimidazolium, and acrylonitrile; the (meth)acrylate is preferably at least one of methyl (meth)acrylate, ethyl (meth)acrylate, and glycidyl (meth)acrylate; preferably, the alkenyl-containing polymeric monomer is selected from vinyl acetate, styrene, and α-methylstyrene; more preferably, the alkenyl-containing polymeric monomer is styrene.

[0074] The polypropylene graft containing anhydride groups, wherein the molar ratio of structural units derived from anhydride monomers to structural units derived from alkenyl-containing polymeric monomers in the polypropylene graft containing anhydride groups is 1:1-20, preferably 1:1-10.

[0075] The polypropylene graft containing anhydride groups, wherein the anhydride is selected from anhydrides having at least one degree of olefin unsaturation; preferably, the anhydride is selected from maleic anhydride and / or itaconic anhydride; more preferably, the anhydride is maleic anhydride.

[0076] According to a specific embodiment of the electrically insulating thermoplastic composite material of the present invention, the modified material of the polypropylene grafted heterocyclic is polypropylene-g-styrene / maleic anhydride, with a melt flow rate of 2-8 g / 10 min at 230°C and 2.16 kg load, and the content of the structural units in the grafted state is 1-8%.

[0077] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, with each of the first and second thermoplastic resins being 100 parts by weight, the first and second additives each independently comprise at least one of the following: 0.5-15 parts by weight of a compatibilizer, 0.05-3 parts by weight of an antioxidant, and 0.05-2.5 parts by weight of a lubricant. Preferably, the first and second additives each independently comprise at least one of the following: 1-15 parts by weight, preferably 1-6 parts by weight, more preferably 3-6 parts by weight of a compatibilizer, 0.1-1 parts by weight, preferably 0.1-0.5 parts by weight of an antioxidant, and 0.5-2.5 parts by weight of a lubricant.

[0078] In some embodiments of the electrically insulating thermoplastic composite material according to the present invention, the compatibilizer is selected from at least one of polar monomer graft-modified polymers. Preferably, the polar monomer is selected from at least one of maleic anhydride, maleic anhydride derivatives, acrylic acid, and acrylate derivatives. Preferably, the polymer is selected from at least one of polyethylene, polypropylene, ethylene-α-olefin copolymers, and propylene-α-olefin (α-olefins other than propylene) copolymers.

[0079] According to a specific embodiment of the electrically insulating thermoplastic composite material of the present invention, maleic anhydride-grafted polypropylene (PP-g-MAH) purchased from Pulilong Plastics Industry Co., Ltd., maleic anhydride-grafted ethylene-octene copolymer (POE-g-MAH) purchased from Shanghai Rizhisheng Technology Co., Ltd., titanate coupling agent purchased from Nanjing Shuguang Chemical Group Co., Ltd., or aluminate coupling agent purchased from Nanjing Youpu Chemical Co., Ltd., can be used as the compatibilizer.

[0080] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, the antioxidant is selected from at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (antioxidant 1010), tris[2,4-di-tert-butylphenyl] phosphite (antioxidant 168), octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (antioxidant 1076), 2,2'-methylenebis(4-methyl-6-tert-butylphenol) (antioxidant 2246), 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane (antioxidant CA), and pentaerythritol diphosphite (2,4-di-tert-butylphenol) (antioxidant 626).

[0081] According to a specific embodiment of the electrically insulating thermoplastic composite material of the present invention, antioxidant 1010 and / or antioxidant 168 purchased from BASF can be used as the antioxidant.

[0082] According to some embodiments of the electrically insulating thermoplastic composite material of the present invention, the lubricant is selected from at least one of ethylene bis-stearamide, calcium stearate, polyethylene wax, pentaerythritol stearate, silicone, polyethylene glycol and fluorinated resin.

[0083] According to a specific embodiment of the electrically insulating thermoplastic composite material of the present invention, oxidized polyethylene wax with the brand name XH-201 purchased from Xianghe Coatings Group can be used as the lubricant.

[0084] In different embodiments of the present invention, the first additive may further include at least one of slip agent, antistatic agent and plasticizer, and / or the second additive may further include at least one of slip agent, antistatic agent, plasticizer, nucleating agent, light stabilizer, heat stabilizer, color masterbatch, antistatic agent and filler, and the specific types and amounts of these additives are not limited, and a wide range of choices can be made.

[0085] A second aspect of the present invention provides a method for preparing an electrically insulating thermoplastic composite material, the method comprising the following steps:

[0086] Step A: The first thermoplastic resin and the first additive are mixed and melted to obtain the first component melt;

[0087] Step B: The continuous fiber bundle is subjected to a first impregnation treatment with the first component melt to form a filamentous core layer product;

[0088] Step C: The second thermoplastic resin and the second additive are mixed and melted to obtain the second component melt;

[0089] Step D: The filamentous core layer product is subjected to a second impregnation treatment with the second component melt to form a resin layer that continuously encapsulates the core layer.

[0090] According to some embodiments of the preparation method described in this invention, the preparation method can be carried out online continuously to obtain continuous filamentous products. Such continuous filamentous products can be directly stored and used, or they can be cut into strips, rods, or granules of a certain length.

[0091] According to some embodiments of the preparation method of the present invention, the mixing conditions of step A include: a temperature of 40-60°C and a time of 0.5-20 min, preferably 1-10 min, and more preferably 3-5 min.

[0092] According to some embodiments of the preparation method described in this invention, the melting temperature in step A is 200-380°C. In this invention, the melting time can have a wide range of options, with the aim of ensuring that the first thermoplastic resin and the first additive are fully melted to obtain a melt.

[0093] According to some embodiments of the preparation method of the present invention, preferably, in step B, before subjecting the continuous fibers to the first impregnation treatment with the first component melt, the continuous fibers are further subjected to dispersion treatment and preheating treatment, wherein the preheating treatment temperature is preferably 80-250°C. The dispersion treatment process in the present invention employs conventional fiber dispersion treatment processes in the art.

[0094] According to some embodiments of the preparation method of the present invention, the mixing conditions in step C include: a temperature of 40-60°C and a time of 0.5-20 min, preferably 1-10 min, and more preferably 3-5 min.

[0095] In some embodiments of the preparation method according to the present invention, the melting temperature in step C is 200-380°C. In the present invention, the melting time can have a wide range of selection, with the aim of ensuring sufficient melting of the second thermoplastic resin and optionally the second additive.

[0096] According to some embodiments of the preparation method of the present invention, the first impregnation treatment in step B can be performed in a first impregnation mold. The first impregnation mold is an adjustable impregnation mold, which includes a fiber inlet, a fiber outlet, and a melt flow channel. At least one first guide roller is provided in the mold cavity of the first impregnation mold. The first guide roller is movable between the fiber inlet and the fiber outlet. And / or, the first guide roller is movable along a direction perpendicular to the line connecting the fiber inlet and the fiber outlet.

[0097] According to some embodiments of the preparation method of the present invention, the first impregnation treatment in step B can be performed in a second impregnation mold. The second impregnation mold is a combined impregnation mold, which includes a first module, an intermediate module, and a second module connected in sequence. The first module is provided with a fiber inlet and a first module flow channel, and the second module is provided with a fiber outlet and a second module flow channel. The intermediate module is provided with an intermediate module flow channel. After the first module, the intermediate module, and the second module are connected in sequence, the first module flow channel, the intermediate module flow channel, and the second module flow channel are connected to form a combined flow channel for the fiber to pass through.

[0098] According to some embodiments of the preparation method of the present invention, the first impregnation treatment in step B can also be carried out in a third impregnation mold. The third impregnation mold is a strong turbulent flow impregnation mold. The third impregnation mold includes a fiber inlet channel, an impregnation outlet, and a melt gap flow channel. The fiber inlet channel, the impregnation outlet, and the melt gap flow channel are all connected to the mold cavity inside the third impregnation mold. A second guide roller is provided inside the mold cavity of the third impregnation mold. The second guide roller includes at least one active guide roller, which is driven to rotate by a driving device.

[0099] The first impregnation mold, the second impregnation mold, and the third impregnation mold used in this invention are described in Chinese patent applications CN 202011193483.3, 202011191450.5, and 202011199839.4, the entire contents of which are incorporated herein by reference.

[0100] It should be noted that the first impregnation mold, the second impregnation mold and the third impregnation mold described above in this invention can be applied to any existing manufacturing system and preparation technology for electrically insulating thermoplastic composite materials, and in particular, can be applied to any existing manufacturing system and preparation technology for continuous fiber reinforced expandable flame retardant thermoplastic composite materials.

[0101] According to some embodiments of the preparation method described in this invention, the second impregnation treatment in step D can be performed in a molding die. The molding die consists of a core, an outer jacket, and an outer jacket opening template. The core is located inside the outer jacket, forming a cavity with it. The resin melt can enter the cavity from the bottom, top, or both sides of the outer jacket. The core can move back and forth within the outer jacket, and the pressure of the melt in the cavity is determined by adjusting the size of the formed cavity space. The pressure of the melt in the cavity can also be adjusted by the angle between the core and the outer jacket.

[0102] The working principle of this molding die is as follows: after passing through the impregnation mold, the strip of inner impregnated material is guided through the hole in the middle of the core, and then the composite structure of inner and outer layer materials is formed in the cavity filled with mixed melt formed by the core and the outer jacket. Finally, it is exported through the outer jacket template.

[0103] According to some embodiments of the preparation method of the present invention, after step D, the obtained electrically insulating thermoplastic composite material is further subjected to drawing, stretching, cooling, drying, and pelletizing processes. The process conditions for drawing, stretching, cooling, drying, and pelletizing are not particularly limited and are all within a wide range of selection, with the aim of obtaining electrically insulating thermoplastic composite materials that meet different specification requirements.

[0104] According to some embodiments of the preparation method of the present invention, in the inner layer material, the amount of the first thermoplastic resin is 1-90 parts by weight, and the amount of the fiber bundle is 10-110 parts by weight.

[0105] In some specific embodiments, the amount of the first thermoplastic resin in the inner layer material can be 1 part by weight, 10 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, or a range thereof; and in some specific embodiments, the amount of the fiber bundle can be 1 part by weight, 10 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, 100 parts by weight, 110 parts by weight, or a range thereof.

[0106] In some preferred embodiments, the amount of the first thermoplastic resin in the inner layer material can be 20-70 parts by weight, preferably 20-55 parts by weight, more preferably 24-45 parts by weight; and / or the amount of the fiber bundle can be 20-110 parts by weight, preferably 25-110 parts by weight.

[0107] According to some embodiments of the preparation method of the present invention, the amount of the second thermoplastic resin in the outer layer material is 1-110 parts by weight.

[0108] In some specific embodiments, the amount of the second thermoplastic resin in the outer layer material can be 1 part by weight, 10 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight, 90 parts by weight, 95 parts by weight, 100 parts by weight, 105 parts by weight, 110 parts by weight, or a range thereof.

[0109] In some preferred embodiments, the amount of the second thermoplastic resin in the outer layer material can be 10-90 parts by weight, preferably 40-90 parts by weight.

[0110] According to some specific embodiments of the preparation method of the present invention, in the inner layer material, the amount of the first thermoplastic resin is 1-90 parts by weight, preferably 20-70 parts by weight, more preferably 20-55 parts by weight, and even more preferably 24-45 parts by weight; and / or the amount of the fiber bundle is 10-99 parts by weight, preferably 20-80 parts by weight, and more preferably 25-50 parts by weight.

[0111] According to some specific embodiments of the preparation method of the present invention, in the inner layer material, the amount of the first thermoplastic resin is 50-70 parts by weight, more preferably 50-60 parts by weight; and / or the amount of the fiber bundle is 90-110 parts by weight, preferably 100-110 parts by weight; and / or in the outer layer material, the amount of the second thermoplastic resin is 90-110 parts by weight, more preferably 95-105 parts by weight.

[0112] According to some embodiments of the preparation method of the present invention, in the inner layer material, the weight ratio of the fiber to the first thermoplastic resin is 0.25-6:1. For example, in the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin is 0.25:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, 0.55:1, 0.6:1, 0.65:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.2:1, 1.5:1, 1.7:1, 1.8:1, 1.9:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 6:1, or a range thereof.

[0113] In some preferred embodiments, the weight ratio of the fiber bundle to the first thermoplastic resin in the inner layer material can be 0.35-4.5:1, preferably 0.43-4.5:1.

[0114] In different embodiments of the present invention, the number of outer layer materials is not limited; the outer layer material may be one layer or multiple layers. When the outer layer material is multi-layered, the multi-layered outer layer material may be formed using one type of outer layer material or multiple types of outer layer materials.

[0115] According to some embodiments of the preparation method of the present invention, the first thermoplastic resin and the second thermoplastic resin may be the same or different, and each is independently selected from at least one of polypropylene, polyethylene, polystyrene, polyvinyl chloride, polyacrylonitrile-butadiene-styrene copolymer, polyacrylonitrile-styrene copolymer, polyoxymethylene, polyamide, polyethylene terephthalate, polybutylene terephthalate, polymethyl methacrylate, polycarbonate, polyphenylene ether, polyurethane, polyetheretherketone and polyphenylene sulfide, and their alloy polymers.

[0116] According to a preferred embodiment of the preparation method of the present invention, the first thermoplastic resin and the second thermoplastic resin are each independently selected from at least one of polypropylene, polyethylene, polyamide (also known as nylon), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyphenylene sulfide, polyurethane and polyetheretherketone (PEEK).

[0117] According to a preferred embodiment of the preparation method of the present invention, the first thermoplastic resin and the second thermoplastic resin are each independently selected from at least one of homopolymer polypropylene, copolymer polypropylene, a mixture of homopolymer polypropylene and copolymer polypropylene, nylon 6 (PA6), nylon 66 (PA66), and a mixture of nylon 6 and nylon 66.

[0118] In other embodiments of the preparation method according to the present invention, the first thermoplastic resin and the second thermoplastic resin may also be selected from thermoplastic polyurethane elastomer (TPU) and / or high-temperature nylon (PPA).

[0119] According to some embodiments of the preparation method of the present invention, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg is 60-8000 g / 10 min. For example, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg can be 60 g / 10 min, 100 g / 10 min, 200 g / 10 min, 450 g / 10 min, 500 g / 10 min, 1000 g / 10 min, 1500 g / 10 min, 2000 g / 10 min, 3000 g / 10 min, 4000 g / 10 min, 5000 g / 10 min, 6000 g / 10 min, 7000 g / 10 min, 7500 g / 10 min, 8000 g / 10 min, or a range thereof.

[0120] In some preferred embodiments, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg can be 100-8000 g / 10 min, preferably 1000-7500 g / 10 min, and more preferably 1900-7500 g / 10 min.

[0121] According to some embodiments of the preparation method of the present invention, the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is 0.1-8000 g / 10 min. For example, the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg can be 0.1 g / 10 min, 1 g / 10 min, 1.5 g / 10 min, 3 g / 10 min, 10 g / 10 min, 20 g / 10 min, 30 g / 10 min, 40 g / 10 min, 45 g / 10 min, 50 g / 10 min, 55 g / 10 min, 60 g / 10 min, 70 g / 10 min, 80 g / 10 min, etc. 90g / 10min, 100g / 10min, 450g / 10min, 500g / 10min, 800g / 10min, 1000g / 10min, 1500g / 10min, 1900g / 10min, 2500g / 10min, 3000g / 10min, 4000g / 10min, 5000g / 10min, 6000g / 10min, 7000g / 10min, 8000g / 10min, or a range thereof.

[0122] In some preferred embodiments, the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg can be 3-55 g / 10 min or 450-8000 g / 10 min, preferably 3-45 g / 10 min or 1900-8000 g / 10 min.

[0123] In different embodiments of the present invention, the melt flow rates of the first thermoplastic resin and the second thermoplastic resin are not particularly limited, and the melt flow rates of the first thermoplastic resin and the second thermoplastic resin can be selected according to the desired performance. In particular, the inventors of this application have discovered that, according to the preparation conditions (e.g., melt flow rates) of the present invention, electrically insulating thermoplastic composite materials with high surface quality and overall performance can be prepared. For example, if the melt flow rate of the first thermoplastic resin is higher than that of the second thermoplastic resin, the electrically insulating thermoplastic composite material can have improved mechanical properties; conversely, if the melt flow rate of the second thermoplastic resin is higher than that of the first thermoplastic resin, the electrically insulating thermoplastic composite material can have improved gloss.

[0124] According to some preferred embodiments of the preparation method of the present invention, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg is 60-450 g / 10 min, for example, 60-200 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is 3-55 g / 10 min or 450-8000 g / 10 min. In some specific embodiments, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg is 60-450 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is 800-8000 g / 10 min.

[0125] According to some preferred embodiments of the preparation method of the present invention, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg is 450 g / 10 min or more, particularly greater than 450 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is less than 100 g / 10 min, preferably 1.5-55 g / 10 min, more preferably 3-50 g / 10 min.

[0126] According to some embodiments of the preparation method of the present invention, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is 0.05-12.5:1. For example, the weight ratio of the second thermoplastic resin to the first thermoplastic resin can be 0.05:1, 0.1:1, 0.14:1, 0.15:1, 0.18:1, 0.2:1, 0.25:1, 0.3:1, 0.5:1, 0.8:1, 1:1, 1.2:1, 1.3:1, 1.4:1, 1.7:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 5:1, 8:1, 10:1, 12.5:1, or a range thereof.

[0127] In some preferred embodiments, the weight ratio of the second thermoplastic resin to the first thermoplastic resin can be 0.14-4:1, preferably 0.14-3.5:1.

[0128] According to a preferred embodiment of the preparation method of the present invention, when the melt flow rate of the second thermoplastic resin is 800-8000 g / 10 min at 230°C and a load of 2.16 kg, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is less than 0.25:1, preferably less than 0.18:1, and more preferably less than 0.15:1.

[0129] According to some embodiments of the preparation method of the present invention, when the first thermoplastic resin and the second thermoplastic resin are selected from at least one of nylon 6, nylon 66, and a mixture of nylon 6 and nylon 66, the viscosity of the selected nylon 6 and nylon 66 is 1.8-3.5.

[0130] According to a specific embodiment of the preparation method of the present invention, the first thermoplastic resin and the second thermoplastic resin can be prepared in-house or commercially available.

[0131] For example, polypropylene resin of grade PPB-M100-GH purchased from Sinopec Yangzi Petrochemical Company, polypropylene resin of grade M60RHC purchased from Sinopec East China Branch, and nylon 6 of grade PA6-BL3200H purchased from Sinopec Baling Branch can be used as the first thermoplastic resin.

[0132] For example, polypropylene resin of grade PPB-M100-GH purchased from Sinopec Yangzi Petrochemical Company, polypropylene resin of grade PPH-T03 purchased from Sinopec Maoming Branch, polypropylene resin of grade M50RH purchased from Sinopec East China Branch, polypropylene resin of grade K8303 purchased from Yanshan Petrochemical Company, polypropylene resin of grade PF1500 purchased from Hunan Shengjin New Materials Co., Ltd., or polypropylene resin of grade PPH-Y450 purchased from Sinopec Shijiazhuang Refining and Chemical Branch, or nylon 6 of grade PA6-BL3200H purchased from Sinopec Baling Branch can be used as the second thermoplastic resin.

[0133] According to some embodiments of the preparation method of the present invention, the fiber bundle is selected from at least one of glass fiber, carbon fiber, basalt fiber, aromatic polyamide fiber, stainless steel fiber, synthetic resin fiber and mineral fiber.

[0134] In a preferred embodiment of the preparation method according to the present invention, the glass fiber is a continuous glass fiber and / or a fixed-length glass fiber.

[0135] According to some embodiments of the preparation method of the present invention, with each of the first thermoplastic resin and the second thermoplastic resin being 100 parts by weight, the first and second additives each independently comprise at least one of the following: 0.5-15 parts by weight of a compatibilizer, 0.05-3 parts by weight of an antioxidant, and 0.05-2.5 parts by weight of a lubricant. Preferably, the first and second additives each independently comprise at least one of the following: 1-15 parts by weight, preferably 1-6 parts by weight, more preferably 3-6 parts by weight of a compatibilizer, 0.1-1 parts by weight, preferably 0.1-0.5 parts by weight of an antioxidant, and 0.5-2.5 parts by weight of a lubricant.

[0136] According to some embodiments of the preparation method of the present invention, the compatibilizer is selected from at least one of polar monomer grafted modified polymers. Preferably, the polar monomer is selected from at least one of maleic anhydride, maleic anhydride derivatives, acrylic acid, and acrylate derivatives. Preferably, the polymer is selected from at least one of polyethylene, polypropylene, ethylene-α-olefin copolymers, and propylene-α-olefins (α-olefins other than propylene).

[0137] According to some embodiments of the preparation method of the present invention, the lubricant is selected from at least one of ethylene bis-stearamide, calcium stearate, polyethylene wax, pentaerythritol stearate, silicone, polyethylene glycol and fluorinated resin.

[0138] In different embodiments of the present invention, the first additive may further include at least one of slip agent, antistatic agent and plasticizer, and the second additive may further include at least one of slip agent, antistatic agent, plasticizer, nucleating agent, light stabilizer, flame retardant, heat stabilizer, color masterbatch, antistatic agent and filler, and the specific types and amounts of these additives are not limited, and the amounts can be selected within a wide range.

[0139] In some embodiments of the present invention, the preparation method of the present invention is as follows: Figure 2 or Figure 3 The manufacturing process is carried out in the electrically insulating thermoplastic composite material manufacturing system shown, and the specific structure and connection method of the electrically insulating thermoplastic composite material manufacturing system are described in the detailed implementation section.

[0140] A third aspect of this invention provides the application of the above-described electrically insulating thermoplastic composite material and the electrically insulating thermoplastic composite material prepared by the above-described method in the automotive industry, machinery manufacturing, electronics and electrical appliances, chemical and environmental protection, aerospace and communications, and construction industries. Preferably, it is used in large automotive parts and / or high-precision electronic and electrical components, more preferably in automotive front-end modules and / or all-plastic tailgate inner panels. However, it is not limited thereto.

[0141] The beneficial effects of this invention are:

[0142] 1. The electrically insulating thermoplastic composite material prepared by this invention has a core layer and an outer layer composite structure. Based on the design of this multi-material composite system, the performance synergy between different components of the inner and outer layer materials can be achieved. This can effectively improve the processing performance of the electrically insulating thermoplastic composite material and the lubricity between the fiber and the resin matrix during injection molding, and enhance the flowability of the fiber in the resin matrix melt. This improves the bonding state between the two and reduces the separation state between them, thereby improving the flowability of the entire material system. As a result, the comprehensive performance and surface quality of the prepared electrically insulating thermoplastic composite material are greatly improved. At the same time, the requirements of the injection molding process are reduced, expanding the application range of the electrically insulating thermoplastic composite material, which has broad application prospects and economic significance.

[0143] 2. The electrically insulating thermoplastic composite material of the present invention has low cost, short injection molding cycle, high part dimensional stability, high material strength, and good electrical insulation performance. It requires no secondary mixing during use and functional materials can be added to the first and / or second components, especially the second component (resin layer), making it widely applicable. Furthermore, the outer layer material of the electrically insulating thermoplastic composite material of the present invention can be fiber-free, offering advantages such as good surface quality, no loose fibers, and improved gloss. Attached Figure Description

[0144] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the following detailed description to explain the invention, but do not constitute a limitation thereof. In the drawings:

[0145] Figure 1 This is a schematic diagram of an electrically insulating thermoplastic composite material structure according to one embodiment of the present invention;

[0146] Figure 2 This is a schematic diagram of the structure of an electrically insulating thermoplastic composite material manufacturing system according to one embodiment of the present invention;

[0147] Figure 3 This is a schematic diagram of the structure of an electrically insulating thermoplastic composite material manufacturing system according to another embodiment of the present invention;

[0148] Figure 4 This is a cross-sectional view of the first impregnation mold in one embodiment of the present invention;

[0149] Figure 5 This is a cross-sectional view of the second impregnation mold in one embodiment of the present invention;

[0150] Figure 6 This is a cross-sectional view of the third impregnation mold in one embodiment of the present invention;

[0151] Figure 7 This is a schematic diagram of the second impregnation treatment in one embodiment of the present invention;

[0152] Figure 8 This is a cross-sectional view of the molding die used in the second impregnation process according to one embodiment of the present invention.

[0153] Explanation of reference numerals in the attached figures:

[0154] 0-1, Core layer; 0-2, Fiber bundle; 0-3, Resin layer;

[0155] 1. Fiber rack and fiber guiding device; 2. Fiber pretreatment device; 3. First impregnation mold; 4. Melting and plasticizing feeding device; 5. Molding mold; 6. Cooling water tank; 7. Dryer; 8. Traction machine; 9. Pelletizer; 10. Collection box;

[0156] A300, First impregnation die head; A1, Fiber inlet; A2, Second chute; A3, Melt flow channel; A4, First chute; A5, Upper die cover; A6, Fiber outlet; A7, Impregnation die body; A8, First guide roller;

[0157] B300, Second impregnation die head; B1, Fiber inlet; B2, Melt channel; B3, First module; B31, First module channel; B4, Combined channel; B5, Standardized connector; B6, Intermediate module; B61, Intermediate module channel; B7, Second module; B71, Second module channel; B8, Fiber outlet;

[0158] C300, Third impregnation die head; C1, Melt flow channel; C2, Impregnation die body; C3, Fiber inlet channel; C4, Active guide roller; C5, Driven guide roller; C6, Impregnation outlet;

[0159] 4-1. Extruder I; 4-2. Extruder II;

[0160] 5-1 Core; 5-2 Outer shell; 5-3 Outer shell opening template; 5-4 Material strip; 5-5 Second resin inlet. Detailed Implementation

[0161] To make the present invention easier to understand, the present invention will be described in detail below with reference to embodiments. These embodiments are for illustrative purposes only and are not limited to the scope of application of the present invention.

[0162] The testing method and equipment used in this invention are as follows:

[0163] (1) Tensile strength test was conducted in accordance with ISO527-2 standard, with a tensile speed of 5 mm / min.

[0164] (2) The bending strength test was conducted in accordance with ISO178 standard, with a bending speed of 2 mm / min.

[0165] (3) The notched impact strength test shall be conducted in accordance with ISO179 standard.

[0166] (4) Surface gloss test shall be conducted in accordance with ISO2813 standard.

[0167] Some of the reagents used in this invention are from the following sources:

[0168] (1) PPB-M100-GH, melt flow rate of 100g / 10min, test conditions of 230℃ and 2.16Kg load, produced by Sinopec Yangzi Petrochemical Company.

[0169] (2) PF1500, melt flow rate 1500g / 10min, produced by Hunan Shengjin New Materials Co., Ltd.

[0170] (3) PPH-Y450, melt flow rate 450g / 10min, produced by Sinopec Shijiazhuang Refining & Chemical Branch.

[0171] (4) BL3200H, viscosity 1.8, produced by Sinopec Baling Branch.

[0172] (5) SE4805, alkali-free glass fiber, with a diameter of 17μm and a linear density of 2400tex, is produced by Owens Corning (Shanghai) Glass Fiber Co., Ltd.

[0173] (6)ER4301H, alkali-free glass fiber, with a diameter of 17μm and a linear density of 2400tex, is produced by Chongqing International Composite Materials Co., Ltd.

[0174] (7) T700SC, carbon fiber, filament 1200-50C, produced by Toray Industries, Inc. of Japan.

[0175] (8) Basalt fiber, single fiber diameter 12μm, produced by Mudanjiang Jinshi Basalt Fiber Co., Ltd.

[0176] (9) PP-g-MAH grade is BONDYRAM 1001, produced by Pulilang Plastics Industry Co., Ltd.

[0177] (10) POE-g-MAH grade is CMG9805, produced by Shanghai Rizhisheng Technology Co., Ltd.

[0178] (11)NDZ12, produced by Nanjing Shuguang Chemical Group Co., Ltd.

[0179] (12)XHY-501, produced by Nanjing Youpu Chemical Co., Ltd.

[0180] (13) Antioxidant 1010, manufactured by BASF.

[0181] (14) Antioxidant 168, manufactured by BASF.

[0182] (15) Polypropylene-g-styrene / maleic anhydride, self-made by Beijing Chemical Research Institute; melt flow rate of 5.84 g / 10 min at 230℃ and 2.16 kg load, content of structural units derived from maleic anhydride monomer and alkenyl polymer monomer in graft state of 0.84%, grafting efficiency of 23%.

[0183] (16)XH-201, produced by Xianghe Coatings Group.

[0184] The invention will now be further described with reference to the accompanying drawings.

[0185] Figure 1 The structure of the electrically insulating thermoplastic composite material of the present invention is shown. For example... Figure 1As shown, the cross-section of the electrically insulating thermoplastic composite material of the present invention is circular, and from the inside out, it includes a core layer 0-1 and a resin layer 0-3. Fiber bundles 0-2 are distributed in the core layer 0-1 with longitudinal orientation, and the fiber bundles 0-2 are uniformly dispersed in the core layer 0-1.

[0186] like Figure 2 and Figure 3 As shown, the manufacturing system of the present invention includes a fiber rack and fiber guiding device 1, a fiber pretreatment device 2, a first impregnation mold 3, a melt plasticizing feeding device 4, a molding mold 5, a cooling water tank 6, a dryer 7, a traction machine 8, a pelletizer 9, a collection box 10, and an electrical control system (not shown in the figure), which are connected in sequence.

[0187] In the manufacturing system, molding die 5 is used for molding the inner and outer layer composite material, and its structure is as follows: Figure 8 As shown.

[0188] In the manufacturing system, the first impregnation mold 3 is used for impregnating the fiber with the resin melt.

[0189] like Figure 4 As shown, in one embodiment, the first impregnation mold is an impregnation device with an adjustable guide roller position, including a first impregnation mold head A300. The first impregnation mold head A300 includes an impregnation mold body A7, a fiber inlet A1, a fiber outlet A6, and a melt flow channel A3. At least one first guide roller A8 is provided in the mold cavity, wherein the first guide roller A8 is movable between the fiber inlet A1 and the fiber outlet A6, or the first guide roller A8 is movable along a direction perpendicular to the line connecting the fiber inlet A1 and the fiber outlet A6; or, the first guide roller A8 is movable both between the fiber inlet A1 and the fiber outlet A6 and along a direction perpendicular to the line connecting the fiber inlet A1 and the fiber outlet A6.

[0190] Taking a rectangular first impregnation mold head A300 as an example, the first impregnation mold head A300 is provided with a plurality of first guide rollers A8. The axial direction of each first guide roller A8 is the width direction of the first impregnation mold head A300. Therefore, each first guide roller A8 can move along the length direction of the first impregnation mold head A300 or along the height direction, thereby changing the position of the first guide roller A8 within the first impregnation mold head A300.

[0191] Understandably, the axial direction of the first guide roller A8 can also be the length direction of the first impregnation mold head A300. In this case, each first guide roller A8 can move along the width direction of the first impregnation mold head A300 or along the height direction of the first impregnation mold head A300, thereby changing the position of the first guide roller A8 within the first impregnation mold head A300.

[0192] Since the fiber (fiber bundle) needs to pass around the first guide roller A8 in sequence within the mold cavity of the first impregnation mold head A300, the fiber's path within the mold cavity can be altered by changing the position of the first guide roller A8 within the first impregnation mold head A300 (horizontal position, longitudinal position, etc.). Therefore, when the required impregnation conditions change, it is not necessary to replace the mold; only the position of the first guide roller A8 within the first impregnation mold head A300 needs to be adjusted. This improves production efficiency and continuity. It also reduces the number of first impregnation mold heads A300, saving production costs.

[0193] Specifically, the inventive concept of this invention is to achieve the purpose of adjusting the position of the first guide roller A8 by slotting the inner wall of the mold cavity of the first impregnation mold head A300.

[0194] A first groove A4 is provided on the first inner wall of the first impregnation mold head A300, and the first groove A4 extends between the fiber inlet A1 and the fiber outlet A6 (i.e., Figure 4 (As shown in the X-axis direction), the first guide roller A8 moves along the first groove A4 to change its horizontal position within the first impregnation mold head A300.

[0195] Furthermore, a second groove A2 is also provided on the first inner wall of the first impregnation mold head A300, and the second groove extends in a direction perpendicular to the first groove A4 (i.e. Figure 4 (As shown in the Y-axis direction), the first guide roller A8 moves along the second slide groove A2 to change its vertical position in the die head.

[0196] It should be noted that the first groove A4 and the second groove A2 can be connected. Therefore, the first guide roller A8 can move arbitrarily in the longitudinal or transverse direction, thereby changing its position.

[0197] The cross-sections of the first groove A4 and the second groove A2 can be trapezoidal, circular, arc-shaped, or rectangular, etc., and the present invention does not limit them.

[0198] Both ends of the first guide roller A8 are provided with adjustment devices (not shown in the figure). The adjustment devices are used to adjust the axial length of the first guide roller A8. The minimum axial length of the first guide roller A8 is less than the distance between the first inner wall and the second inner wall, and the maximum axial length of the first guide roller A8 is greater than the distance between the first inner wall and the second inner wall.

[0199] like Figure 5As shown, in another embodiment of the present invention, the second impregnation mold is a combined impregnation mold, including a second impregnation mold head B300. The second impregnation mold head B300 includes a first module B3, an intermediate module B6, and a second module B7 connected in sequence. The first module B3 is provided with a fiber inlet B1 and a first module flow channel B31, the second module B7 is provided with a fiber outlet B8 and a second module flow channel B71, and the intermediate module B6 is provided with an intermediate module flow channel B61.

[0200] After sequentially connecting the first module B3, intermediate module B6, and second module B7, the first module flow channel B31, intermediate module flow channel B61, and second module flow channel B71 are connected to form a combined flow channel B4 for the fiber to pass through. The number of intermediate modules B6 is at least one. That is, the first module B3 is the head module, the second module B7 is the tail module, and there are one or more intermediate modules B6 between them. It should be noted that these intermediate modules B6 are also sequentially connected.

[0201] In other words, the number of intermediate modules B6 can be increased or decreased as needed, so that when the impregnation requirements change, different intermediate modules B6 can be combined to form a combined second impregnation mold head B300, thereby improving production continuity and efficiency and saving the cost of additional mold opening.

[0202] Furthermore, by selecting different intermediate modules B6, the shape parameters (such as curvature) of the formed combined flow channel B4 can be changed, thereby altering the flow path of the fiber and melt. This allows for changes in the impregnation angle and fiber tension at different stations in the mold, ultimately achieving the goal of adjusting and optimizing the entire fiber impregnation process and improving the adaptability of the second impregnation mold head B300 to different resin matrices and fibers.

[0203] The first module B3, the intermediate module B6, and the second module B7 are placed in the mold frame. The mold frame provides a constraint, ensuring that they are in close contact with each other and thus guaranteeing the sealing of the combined flow channel B4.

[0204] like Figure 5 As shown, an implementation with two intermediate modules B6 is illustrated. Figure 5 In the embodiment shown, the downstream end of the first module flow channel B31 is connected to the upstream end of one of the intermediate module flow channels B61, the two intermediate module flow channels B61 are connected to each other, and the downstream section of the other intermediate module flow channel B61 is connected to the upstream end of the second intermediate module flow channel B71, thereby forming a combined flow channel B4 extending from the fiber inlet B1 to the fiber outlet B8.

[0205] Understandably, different combinations of flow channels B4 can be obtained by selecting different intermediate modules B6.

[0206] like Figure 5 As shown, the downstream end of the first module flow channel B31, the upstream end of the second module flow channel B71, and both ends of the intermediate module flow channel B61 are all located in the same plane and are constructed with standardized connectors B5. In other words, the connections between the first module flow channel B31, the intermediate module flow channel B61, and the second module B71 are made through standardized connectors B5. Since the standardized connectors B5 are all located in the same plane and have the same shape and size, it facilitates the combination and connection between different modules.

[0207] like Figure 6 As shown, in another embodiment of the present invention, the third impregnation mold is a strong turbulent impregnation mold, including a third impregnation mold head C300. The third impregnation mold head C300 includes an impregnation mold outer body C2. The impregnation mold outer body C2 is provided with a fiber inlet channel C3, an impregnation outlet C6, and a melt gap flow channel C1. The fiber inlet channel C3, the impregnation outlet C6, and the melt gap flow channel C1 are all connected to the mold cavity inside the impregnation mold outer body C2.

[0208] The impregnation mold outer body C2 has a second guide roller inside its cavity. This second guide roller includes at least one active guide roller C4, which is driven to rotate by a drive device (not shown in the figure). Since the rotation of the active guide roller C4 is driven by the drive device, rather than by the fiber's traction, the actively rotating active guide roller C4 helps reduce the fiber's traction tension and the friction between the fiber and the active guide roller C4 as the fiber passes through it. This reduces fiber breakage, ensures fiber integrity, and prevents fiber breakage, thereby improving the material's mechanical properties. Preferably, the second guide roller also includes at least one driven guide roller C5, which is driven by the fiber passing through the active guide roller C4; or the driven guide roller C5 and the active guide roller C4 are connected via a belt mechanism, gear mechanism, or chain mechanism. Figure 6 The diagram illustrates an example with one active guide roller C4 and two driven guide rollers C5, wherein the two driven guide rollers C5 are arranged one above the other to extend the impregnation path of the fibers passing through them. The active guide roller C4 and the driven guide rollers C5 may be at the same or different heights within the die cavity.

[0209] Furthermore, the driving device can be a motor, hydraulic mechanism, or gearbox, or any device capable of driving the active guide roller C4 to rotate.

[0210] Based on the fiber's traveling speed v1 in the mold cavity of the impregnation mold body C2, the corresponding tangential speed v2 of the active guide roller C4 can be selected. For example, the tangential speed v2 of the active guide roller C4 can be made the same as the fiber's traveling speed v1, i.e., v1 = v2. This reduces fiber breakage and wear, thus ensuring fiber integrity, promoting the degree of fiber impregnation, shortening impregnation time, and improving production efficiency.

[0211] like Figure 2 As shown, the melt plasticizing feeding device 4 consists of a twin-screw extruder used for melting and plasticizing materials. The twin-screw extruder is a co-rotating twin-screw extruder with a screw diameter of 25mm-95mm and a length-to-diameter ratio of 36:1-65:1. When the melt plasticizing feeding device 4 consists of a single extruder 4, the melt plasticizing material in the extruder is divided by a melt distributor and fed into the impregnation die and the forming die respectively, and the flow rate of each die is controlled by a melt flow control valve.

[0212] like Figure 3 As shown, when the melt plasticizing feeding device 4 consists of two extruders 4-1 and 4-2, the molten plasticized melts from extruder I 4-1 and extruder II 4-2 are respectively fed into the impregnation mold and the forming mold. In this embodiment, the melt plasticizing feeding device consists of two extruders, namely extruder I 4-1 and extruder II 4-2, which respectively feed the molten plasticized melts from extruder I 4-1 and extruder II 4-2 into the first impregnation mold 3 and the forming mold 5. Extruder I 4-1 and extruder II 4-2 can be fed with the same or different materials, thus enabling the preparation of composite materials with the same or different materials for the inner and outer layers.

[0213] The fiber pretreatment device 2 consists of a tension roller and a hot drying tunnel. This combination allows for some release of tension on the fibers as they enter the hot drying tunnel, thus accommodating fibers of different strengths and preventing fibers with lower strength from breaking before entering the impregnation die. The surface of the tension roller in the fiber pretreatment device 2 needs to be ceramic-coated to increase surface roughness and reduce friction on the fibers.

[0214] In the manufacturing system, the fiber frame and fiber guiding device 1 are used for fiber output and untwisting. The device is equipped with an automatic control untwisting device, which is linked with the traction machine 8 and electrically connected to the electrical control system (such as a PLC control device).

[0215] In the manufacturing system, the cooling water tank 6, dryer 7, traction machine 8, pelletizer 9, and collection box 10 are conventional equipment or devices known to those skilled in the art, and will not be described in detail here.

[0216] Figure 7 A schematic diagram showing the second impregnation process using a molding die is shown. Figure 8 A cross-sectional view of the molding die used in the second impregnation process is shown.

[0217] like Figure 8 As shown, in one embodiment, the molding die 5 consists of a core 5-1, an outer sleeve 5-2, and an outer sleeve opening template 5-3. The core 5-1 is located inside the outer sleeve 5-2, forming a cavity with the outer sleeve 5-2. The resin melt can enter the cavity from the bottom, top, or both sides of the outer sleeve 5-2. The core 5-1 can move back and forth within the outer sleeve 5-2, and the pressure of the melt in the cavity is determined by adjusting the size of the formed cavity space. The pressure of the melt in the cavity can also be adjusted by the angle between the core 5-1 and the outer sleeve 5-2. The working principle of the molding die 5 is as follows: the strip of inner impregnated material formed after passing through the impregnation mold 3 is guided through the hole in the middle of the core 5-1, and then the composite structure of the inner and outer layer materials is formed in the cavity filled with mixed melt formed by the core 5-1 and the outer sleeve 5-2. Finally, it is discharged through the outer sleeve opening template 5-3.

[0218] like Figure 7 As shown, the material strip 5-4 enters the cavity filled with the second component melt formed by the core (not shown) and the outer sleeve 5-2 for processing, wherein the second component melt is fed into the cavity from the second resin inlet 5-5.

[0219] In the following embodiments and comparative examples, the following methods are employed: Figure 3 The manufacturing system shown prepares electrically insulating thermoplastic composite materials, wherein the first impregnation treatment is selected from... Figure 4 The first immersion mold shown, the second immersion treatment adopts Figure 8 The molding die shown.

[0220]

Example 1

[0221] (1) Weigh 50 parts by weight of dry PPB-M100-GH polypropylene resin (melt flow rate of 100g / 10min), 5 parts by weight of polypropylene-g-styrene / maleic anhydride, 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir in a high-speed mixer at 50°C for 3min to obtain the first component melt, and send it into the first impregnation mold.

[0222] (2) 30 parts by weight of glass fiber SE4805 enter the first impregnation mold under the action of the traction machine, where it is impregnated and dispersed with the first component melt to form a strip, which is used as the inner layer material.

[0223] (3) Weigh 49 parts by weight of dried PPH-Y450 polypropylene resin (melt flow rate of 450 g / 10 min), 5 parts by weight of polypropylene-g-styrene / maleic anhydride, 2.5 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir them in a high-speed mixer at 50°C for 3 min. Use this as the outer layer material and feed it into a twin-screw extruder connected to the molding die to obtain the second component melt.

[0224] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity filled with the second component melt formed by the core and the outer jacket to realize the molding of the composite structure of the inner and outer layer materials. Finally, it is exported through the mold outlet.

[0225] (5) The coating amount of the outer layer material is adjusted by adjusting the extrusion rate of the extruder used for the outer layer material and the die exit diameter, so that it coats the material according to the amount specified in step (3). The cutting speed of the pelletizer is adjusted so that the pellet length of the prepared electrically insulating thermoplastic composite material is controlled to be 61.1 mm. In the composite material, the proportion of glass fiber SE4805 is 20.6% by weight.

[0226] (6) The polypropylene composite material obtained by the above method was injection molded into standard specimens and its performance was tested. The test results are shown in Table 1.

[0227]

Example 2

[0228] (1) Weigh 20 parts by weight of dried self-made high-flow polypropylene (melt flow rate of 1000g / 10min), 2 parts by weight of polypropylene-g-styrene / maleic anhydride, 0.6 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir in a high-speed mixer at 50°C for 3min to obtain the first component melt, and send it into the first impregnation mold.

[0229] (2) 50 parts by weight of glass fiber SE4805 enter the first impregnation mold under the action of the traction machine, where it is impregnated and dispersed with the melt to form a strip, which is used as the inner layer material.

[0230] (3) Weigh 59 parts by weight of dried PPH-T03 polypropylene resin (melt flow rate 3g / 10min), 10 parts by weight of polypropylene-g-styrene / maleic anhydride, 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir them in a high-speed mixer at 50°C for 3min. Use this as the outer layer material and feed it into a twin-screw extruder connected to the molding die to obtain the second component melt.

[0231] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity filled with the second component melt formed by the core and the outer jacket to realize the molding of the composite structure of the inner and outer layer materials. Finally, it is exported through the mold outlet.

[0232] (5) Adjust the coating amount of the outer layer material by adjusting the extrusion rate of the extruder used for the outer layer material and the die exit diameter, so that it coats the material according to the amount specified in step (3). Adjust the cutting speed of the pelletizer so that the pellet length of the prepared electrically insulating thermoplastic composite material is controlled to be 15 mm. In the composite material, the proportion of glass fiber SE4805 is 34.3% by weight.

[0233] (6) The polypropylene composite material obtained by the above method was injection molded into standard specimens and its performance was tested. The test results are shown in Table 1.

[0234]

Example 3

[0235] (1) Weigh 20 parts by weight of dried self-made high-flow polypropylene (melt flow rate 7500g / 10min), 6 parts by weight of polypropylene-g-styrene / maleic anhydride, 0.6 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir in a high-speed mixer at 50°C for 3min to obtain the first component melt, and send it into the first impregnation mold.

[0236] (2) 80 parts by weight of glass fiber SE4805 enter the first impregnation mold under the action of the traction machine, where it is impregnated and dispersed with the melt to form a strip, which is used as the inner layer material.

[0237] (3) Weigh 69 parts by weight of dried K8303 polypropylene resin (melt flow rate 1.5 g / 10 min), 20 parts by weight of polypropylene-g-styrene / maleic anhydride, 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir them in a high-speed mixer at 50°C for 3 min. Use this as the outer layer material and feed it into a twin-screw extruder connected to the molding die to obtain the second component melt.

[0238] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity filled with the second component melt formed by the core and the outer jacket to realize the molding of the composite structure of the inner and outer layer materials. Finally, it is exported through the mold outlet.

[0239] (5) Adjust the coating amount of the outer layer material by adjusting the extrusion rate of the extruder used for the outer layer material and the die exit diameter, so that it coats the material according to the amount specified in step (3). Adjust the cutting speed of the pelletizer so that the pellet length of the prepared electrically insulating thermoplastic composite material is controlled to be 18 mm. In the composite material, the proportion of glass fiber SE4805 is 40% by weight.

[0240] (6) The polypropylene composite material obtained by the above method was injection molded into standard specimens and its performance was tested. The test results are shown in Table 1.

[0241]

Example 4

[0242] (1) Weigh 70 parts by weight of dried PPB-M100-GH (melt flow rate 100g / 10min), 20 parts by weight of polypropylene-g-styrene / maleic anhydride, 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir in a high-speed mixer at 50°C for 3min to obtain the first component melt, and send it into the first impregnation mold.

[0243] (2) 25 parts by weight of glass fiber SE4805 enter the first impregnation mold under the action of the traction machine, where it is impregnated and dispersed with the melt to form a strip, which is used as the inner layer material.

[0244] (3) Weigh 10 parts by weight of dried self-made high-flow polypropylene (melt flow rate 1900g / 10min), 3 parts by weight of polypropylene-g-styrene / maleic anhydride, 0.5 parts by weight of BONDYRAM 1001, 0.05 parts by weight of antioxidant 1010, and 0.25 parts by weight of XH-201. Stir them in a high-speed mixer at 50°C for 3min. Use this as the outer layer material and feed it into a twin-screw extruder connected to the molding die to obtain the second component melt.

[0245] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity filled with the second component melt formed by the core and the outer jacket to realize the molding of the composite structure of the inner and outer layer materials. Finally, it is exported through the mold outlet.

[0246] (5) Adjust the coating amount of the outer layer material by adjusting the extrusion rate of the extruder used for the outer layer material and the die exit diameter, so that it coats the material according to the amount specified in step (3). Adjust the cutting speed of the pelletizer so that the pellet length of the prepared electrically insulating thermoplastic composite material is controlled to be 5 mm. In the composite material, the proportion of glass fiber SE4805 is 18.9% by weight.

[0247] (6) The polypropylene composite material obtained by the above method was injection molded into standard specimens and its performance was tested. The test results are shown in Table 1.

[0248]

Example 5

[0249] (1) Weigh 57 parts by weight of dried M60RHC polypropylene resin (melt flow rate 60g / 10min), 17 parts by weight of polypropylene-g-styrene / maleic anhydride, 2.5 parts by weight of BONDYRAM 1001, 0.5 parts by weight of NDZ12, 0.1 parts by weight of antioxidant 168 and 0.25 parts by weight of XH-201, stir in a high-speed mixer at 50°C for 3min to obtain the first component melt, and send it into the first impregnation mold.

[0250] (2) 40 parts by weight of glass fiber SE4805 enter the first impregnation mold under the action of the traction machine, where it is impregnated and dispersed with the melt to form a strip, which is used as the inner layer material.

[0251] (3) Weigh 97 parts by weight of dried M50RH polypropylene resin (melt flow rate 50g / 10min), 25 parts by weight of polypropylene-g-styrene / maleic anhydride, 4 parts by weight of BONDYRAM 1001, 0.8 parts by weight of NDZ12, 0.1 parts by weight of antioxidant 168, and 0.8 parts by weight of XH-201. Stir them in a high-speed mixer at 50°C for 3min. Use this as the outer layer material and feed it into a twin-screw extruder connected to the molding die to obtain the second component melt.

[0252] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity filled with the second component melt formed by the core and the outer jacket to realize the molding of the composite structure of the inner and outer layer materials. Finally, it is exported through the mold outlet.

[0253] (5) Adjust the coating amount of the outer layer material by adjusting the extrusion rate of the extruder used for the outer layer material and the die exit diameter, so that it coats the material according to the amount specified in step (3). Adjust the cutting speed of the pelletizer so that the pellet length of the prepared electrically insulating thermoplastic composite material is controlled to be 10 mm. In the composite material, the proportion of glass fiber SE4805 is 16.3% by weight.

[0254] (6) The polypropylene composite material obtained by the above method was injection molded into standard specimens and its performance was tested. The test results are shown in Table 1.

[0255]

Example 6

[0256] (1) Weigh 57 parts by weight of dried PA6-BL3200H, 17 parts by weight of polypropylene-g-styrene / maleic anhydride, 3 parts by weight of CMG9805, 0.1 parts by weight of antioxidant 1010 and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50°C for 3 minutes to obtain the first component melt, and send it into the first impregnation mold.

[0257] (2) ER4301H enters the first impregnation mold under the action of the traction machine, where it is impregnated and dispersed with the first component melt to form a strip, which is used as the inner layer material.

[0258] (3) Weigh 72 parts by weight of dried PA6-BL3200H, 25 parts by weight of polypropylene-g-styrene / maleic anhydride, 3 parts by weight of CMG9805, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir them in a high-speed mixer at 50°C for 3 minutes. Use them as the outer layer material and feed them into a twin-screw extruder connected to the molding die to obtain the second component melt.

[0259] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity filled with the second component melt formed by the core and the outer jacket to realize the molding of the composite structure of the inner and outer layer materials. Finally, it is exported through the mold outlet.

[0260] (5) Adjust the coating amount of the outer layer material by adjusting the extrusion rate of the extruder used for the outer layer material and the die exit diameter, so that it coats the material according to the amount specified in step (3). Adjust the cutting speed of the pelletizer so that the pellet length of the prepared electrically insulating thermoplastic composite material is controlled to be 12 mm. In the composite material, ER4301H accounts for 40% by weight.

[0261] (6) The long glass fiber reinforced PA6 composite material prepared by the above method was injection molded into standard specimens and its performance was tested. The test results are shown in Table 1.

[0262]

Example 7

[0263] (1) Weigh 57 parts by weight of dried PPB-M100-GH, 17 parts by weight of polypropylene-g-styrene / maleic anhydride, 3 parts by weight of BONDYRAM 1001, 0.5 parts by weight of XHY-501, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir in a high-speed mixer at 50°C for 3 minutes to obtain the first component melt, and then send it into the first impregnation mold.

[0264] (2) Continuous basalt fibers enter the first impregnation mold under the action of the traction machine, where they are impregnated and dispersed with the first component melt to form strips, which are used as inner layer materials.

[0265] (3) Weigh 72 parts by weight of dried PPB-M100-GH, 25 parts by weight of polypropylene-g-styrene / maleic anhydride, 3 parts by weight of BONDYRAM 1001, 0.5 parts by weight of XHY-501, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir them in a high-speed mixer at 50°C for 3 minutes. Use them as the outer layer material and feed them into a twin-screw extruder connected to the molding die to obtain the second component melt.

[0266] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity filled with the second component melt formed by the core and the outer jacket to realize the molding of the composite structure of the inner and outer layer materials. Finally, it is exported through the mold outlet.

[0267] (5) Adjust the coating amount of the outer layer material by adjusting the extrusion rate of the extruder used for the outer layer material and the die exit diameter, so that it coats the material according to the amount specified in step (3). Adjust the cutting speed of the pelletizer so that the pellet length of the prepared electrically insulating thermoplastic composite material is controlled to be 12 mm. In the composite material, the proportion of continuous basalt fiber is 40% by weight.

[0268] (6) The basalt fiber reinforced PP composite material prepared by the above method was injection molded into standard specimens and its performance was tested. The test results are shown in Table 1.

[0269]

Example 8

[0270] The preparation process is the same as in Example 1, except that 70 parts by weight of PPB-M100-GH are weighed in step (1) and 85 parts by weight of PPH-Y450 are weighed in step (3). The performance of the prepared composite material was tested, and the results are shown in Table 1. In the composite material, the proportion of glass fiber SE4805 is 14.8% by weight.

[0271]

Example 9

[0272] The preparation process is the same as in Example 1, except that: in step (1), 45 parts by weight of PPB-M100-GH, 2.5 parts by weight of BONDYRAM 1001, 0.08 parts by weight of antioxidant 1010, and 0.4 parts by weight of XH-201 are weighed; and in step (3), 65 parts by weight of PPH-Y450 are weighed. The performance of the prepared composite material was tested, and the results are shown in Table 1. In the composite material, the proportion of glass fiber SE4805 is 19% by weight.

[0273]

Example 10

[0274] The preparation process is the same as in Example 1, except that: in step (1), 25 parts by weight of PPB-M100-GH, 1.5 parts by weight of BONDYRAM 1001, 0.05 parts by weight of antioxidant 1010, and 0.25 parts by weight of XH-201 are weighed; and in step (3), 45 parts by weight of PPH-Y450 are weighed. The performance of the prepared composite material was tested, and the results are shown in Table 1. In the composite material, the proportion of glass fiber SE4805 is 25.6% by weight.

[0275]

Example 11

[0276] The preparation process is the same as in Example 1, except that 55 parts by weight of PPB-M100-GH are weighed in step (1) and 70 parts by weight of PPH-Y450 are weighed in step (3). The performance of the prepared composite material was tested, and the results are shown in Table 1. In the composite material, the proportion of glass fiber SE4805 is 17.4% by weight.

[0277]

Example 12

[0278] (1) Weigh 50 parts by weight of dry PPB-M100-GH polypropylene resin (melt flow rate of 100g / 10min), 5 parts by weight of polypropylene-g-styrene / maleic anhydride, 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir in a high-speed mixer at 50°C for 3min to obtain the first component melt, and send it into the first impregnation mold.

[0279] (2) 30 parts by weight of glass fiber SE4805 enter the first impregnation mold under the action of the traction machine, where it is impregnated and dispersed with the first component melt to form a strip, which is used as the inner layer material.

[0280] (3) Weigh 49 parts by weight of dried M60RHC polypropylene resin (melt flow rate of 60g / 10min), 5 parts by weight of polypropylene-g-styrene / maleic anhydride, 20 parts by weight of short glass fibers cut from glass fiber SE4805 with a length of 3mm, 2.5 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir them in a high-speed mixer at 50°C for 3min. Use this as the outer layer material and feed it into a twin-screw extruder connected to the molding die to obtain the second component melt.

[0281] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity filled with the second component melt formed by the core and the outer jacket to realize the molding of the composite structure of the inner and outer layer materials. Finally, it is exported through the mold outlet.

[0282] (5) Adjust the coating amount of the outer layer material by adjusting the extrusion rate of the extruder used for the outer layer material and the die exit diameter, so that it coats the material according to the amount specified in step (3). Adjust the cutting speed of the pelletizer so that the pellet length of the prepared electrically insulating thermoplastic composite material is controlled to be 6.1 mm. In the composite material, the proportion of glass fiber SE4805 is 30% by weight.

[0283] (6) The polypropylene composite material obtained by the above method was injection molded into standard specimens and its performance was tested. The test results are shown in Table 1.

[0284] Comparative Example 1

[0285] (1) Weigh 57 parts by weight of dried PPB-M100-GH, 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010 and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50°C for 3 minutes to obtain a melt, and send it into an impregnation mold.

[0286] (2) SE4805 enters the impregnation mold under the action of the traction machine, where it is impregnated and dispersed with the melt. The content of SE4805 in the composite material is adjusted by selecting the size of the mold plate (6mm) of the impregnation mold. The content of SE4805 is controlled to be 22% by weight. The cutting speed of the pelletizer is adjusted so that the pellet length of the prepared polypropylene composite material is controlled to be 12mm.

[0287] (3) The polypropylene composite material obtained by the above method was injection molded into standard specimens and its performance was tested. The test results are shown in Table 1.

[0288] Comparative Example 2

[0289] (1) Weigh 50 parts by weight of dry PPB-M100-GH polypropylene resin (melt flow rate of 100g / 10min), 30 parts by weight of short glass fiber cut from glass fiber SE4805 with a length of 3mm, 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir them in a high-speed mixer at 50°C for 3min as the inner layer resin.

[0290] (2) Weigh 49 parts by weight of dried M60RHC polypropylene resin (melt flow rate of 60g / 10min), 20 parts by weight of short glass fiber cut from SE4805 glass fiber with a length of 3mm, 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201. Stir them in a high-speed mixer at 50°C for 3min and use them as the outer layer material.

[0291] (3) The inner layer material was added to extruder No. 1, and the outer layer material was added to extruder No. 2. The two extruders simultaneously extruded the raw materials, and the materials were extruded through a die with an inner and outer layer structure to obtain a continuous filament material with an inner layer containing short glass fiber resin and an outer layer containing short glass fiber resin. The filament material was then pelletized to obtain the comparative raw material. Performance tests are shown in Table 1.

[0292] Table 1

[0293]

[0294] Note: In Table 1, D1 and D2 are Comparative Example 1 and Comparative Example 2, respectively, and S1-S12 are Examples 1-12.

[0295] By comparing Examples 1-5 and Examples 8-12 with Comparative Examples 1-2, it was found that the tensile strength, flexural strength, notched impact strength of simply supported beams, and surface gloss of the long glass fiber reinforced polypropylene material prepared by the present invention are significantly higher than those of the material prepared in Comparative Example 1, and the surface quality of the parts is also higher.

[0296] As can be seen from Examples 6-7 of the present invention, the preparation method proposed in this invention is not only applicable to long glass fiber reinforced polypropylene composites, but also applicable to the preparation of continuous glass fiber reinforced PA6 and continuous basalt fiber reinforced polypropylene.

[0297] Furthermore, as can be seen from the data in Table 1, the thermoplastic composite material of the present invention has good electrical insulation properties. By selecting the melt flow rate of the thermoplastic resins of the inner and outer layer materials, the prepared composite material can have an ideal surface gloss.

[0298] The preparation method of the present invention is simple to operate, can realize online continuous production, can ensure high production capacity and low energy consumption, and is suitable for industrial production and application.

[0299] The above description is merely a preferred embodiment of the present invention. It should be noted that, for those skilled in the art, based on the technical teachings provided by the present invention and as common knowledge in the field, other equivalent modifications and improvements can be made, and these should also be considered within the scope of protection of the present invention.

Claims

1. An electrically insulating thermoplastic composite material having a core layer structure, comprising an inner layer material and at least one outer layer material, wherein the inner layer material is a core layer comprising a fiber bundle, a first thermoplastic resin and a first additive, and the at least one outer layer material wraps the core layer and is a resin layer comprising a second thermoplastic resin and a second additive, wherein: The fiber bundle extends continuously from one end of the core layer to the opposite end thereof, the first auxiliary agent and the second auxiliary agent each independently comprise a polypropylene graft containing anhydride groups, which comprises a structural unit derived from copolymerized polypropylene, a structural unit derived from maleic anhydride monomers and a structural unit derived from olefin-containing polymer monomers, On the transverse cross section of the electrically insulating thermoplastic composite material, there are a core layer and a resin layer from the inside to the outside, and the first thermoplastic resin and the second thermoplastic resin are of the same type. The first thermoplastic resin has a melt flow rate of 60-8000 g / 10 min at 230° C. and a load of 2.16 kg, The melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 0.1-8000 g / 10 min, The melt flow rate of the first thermoplastic resin is higher than the melt flow rate of the second thermoplastic resin, or, the melt flow rate of the second thermoplastic resin is higher than the melt flow rate of the first thermoplastic resin, Wherein, in the inner layer material, the amount of the first thermoplastic resin is 1-90 parts by weight; the amount of the fiber bundle is 10-110 parts by weight; and in the outer layer material, the amount of the second thermoplastic resin is 1-110 parts by weight.

2. The electrically insulating thermoplastic composite material according to claim 1, characterized in that: The electrically insulating thermoplastic composite material is in the form of strips, rods or particles.

3. The electrically insulating thermoplastic composite material according to claim 2, characterized in that: The length of the strip, rod or granular electrically insulating thermoplastic composite material is 5-30 mm.

4. The electrically insulating thermoplastic composite material according to claim 3, characterized in that: The length of the strip, rod or granular electrically insulating thermoplastic composite material is 5-25 mm.

5. The electrically insulating thermoplastic composite material according to claim 4, characterized in that: The length of the strip, rod or granular electrically insulating thermoplastic composite material is 6-15 mm.

6. The electrically insulating thermoplastic composite material according to claim 1, characterized in that: In the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin is 0.25-6:

1.

7. The electrically insulating thermoplastic composite material according to claim 6, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 20-70 parts by weight; the amount of the fiber bundle is 20-110 parts by weight; and / or, In the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin is 0.35-4.5:1; and / or, In the outer layer material, the amount of the second thermoplastic resin is 10-99 parts by weight.

8. The electrically insulating thermoplastic composite material according to claim 6, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 20-55 parts by weight; the amount of the fiber bundle is 25-110 parts by weight; and / or, In the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin is 0.43-4.5:1; and / or, In the outer layer material, the amount of the second thermoplastic resin is 40-90 parts by weight.

9. The electrically insulating thermoplastic composite material according to claim 6, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 24-45 parts by weight.

10. The electrically insulating thermoplastic composite material according to claim 6, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 1-90 parts by weight; and / or the amount of the fiber bundle is 10-99 parts by weight; or, In the inner layer material, the amount of the first thermoplastic resin is 50-70 parts by weight; and / or the amount of the fiber bundle is 90-110 parts by weight; and / or in the outer layer material, the amount of the second thermoplastic resin is 90-110 parts by weight.

11. The electrically insulating thermoplastic composite material according to claim 10, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 20-70 parts by weight; and / or the amount of the fiber bundle is 20-80 parts by weight; or, In the inner layer material, the amount of the first thermoplastic resin is 50-60 parts by weight; and / or the amount of the fiber bundle is 100-110 parts by weight; and / or in the outer layer material, the amount of the second thermoplastic resin is 95-105 parts by weight.

12. The electrically insulating thermoplastic composite material according to claim 11, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 20-55 parts by weight; and / or the amount of the fiber bundle is 25-50 parts by weight.

13. The electrically insulating thermoplastic composite material according to claim 12, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 24-45 parts by weight.

14. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: The inner layer material does not contain non-oriented short fibers.

15. The electrically insulating thermoplastic composite material according to claim 14, characterized in that: The inner layer material consists of a fiber bundle, a first thermoplastic resin and a first auxiliary agent.

16. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: The outer material contains no fibres; or The outer layer material contains fibers.

17. The electrically insulating thermoplastic composite material according to claim 16, characterized in that: The outer layer material is composed of a second thermoplastic resin and a second auxiliary agent; or The outer layer material contains short fibers; in the outer layer material, the weight ratio of the short fibers to the second thermoplastic resin is 1-50:

100.

18. The electrically insulating thermoplastic composite material according to claim 17, characterized in that: In the outer layer material, the weight ratio of the short fibers to the second thermoplastic resin is 5-50:

100.

19. The electrically insulating thermoplastic composite material according to claim 18, characterized in that: In the outer layer material, the weight ratio of the short fibers to the second thermoplastic resin is 20-45:

100.

20. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: The first thermoplastic resin and the second thermoplastic resin are selected from at least one of polypropylene, polyethylene, polystyrene, polyvinyl chloride, polyacrylonitrile-butadiene-styrene copolymer, polyacrylonitrile-styrene copolymer, polyoxymethylene, polyamide, polyethylene terephthalate, polybutylene terephthalate and polymethyl methacrylate and alloy polymers thereof; and / or, The fiber bundle is selected from at least one of glass fiber, carbon fiber, stainless steel fiber, synthetic resin fiber and mineral fiber.

21. The electrically insulating thermoplastic composite material according to claim 20, characterized in that: The first thermoplastic resin and the second thermoplastic resin are selected from at least one of polypropylene, polyethylene, polyamide, polyethylene terephthalate and polybutylene terephthalate; And / or, the fiber bundle is selected from at least one of basalt fiber and aromatic polyamide fiber.

22. The electrically insulating thermoplastic composite material according to claim 20, characterized in that: The first thermoplastic resin and the second thermoplastic resin are at least one selected from homopolypropylene, copolymer polypropylene, a mixture of homopolypropylene and copolymer polypropylene, nylon 6, nylon 66, and a mixture of nylon 6 and nylon 66.

23. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: The melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg is 100-8000 g / 10 min; the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 3-55 g / 10 min or 450-8000 g / 10 min.

24. The electrically insulating thermoplastic composite material according to claim 23, characterized in that: The melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg is 1000-7500 g / 10 min; the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 3-45 g / 10 min or 1900-8000 g / 10 min.

25. The electrically insulating thermoplastic composite material according to claim 23, characterized in that: The first thermoplastic resin has a melt flow rate of 1900-7500 g / 10 min at 230° C. and a load of 2.16 kg.

26. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: The melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg is 60-450 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 3-55 g / 10 min or 450-8000 g / 10 min; or The melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg is greater than 450 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is less than 100 g / 10 min; And / or, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is 0.05-12.5:

1.

27. The electrically insulating thermoplastic composite material according to claim 26, characterized in that The first thermoplastic resin has a melt flow rate of 60-200 g / 10 min at 230° C. and a load of 2.16 kg; or The melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg is greater than 450 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 1.5-55 g / 10 min; And / or, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is 0.1-4:

1.

28. The electrically insulating thermoplastic composite material according to claim 27, characterized in that: The melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg is 60-450 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 800-8000 g / 10 min; or The melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 3-50 g / 10 min; And / or, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is 0.14-3.5:

1.

29. The electrically insulating thermoplastic composite material according to claim 23, characterized in that: When the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 800-8000 g / 10 min, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is less than 0.25:1; and / or, When the first thermoplastic resin and the second thermoplastic resin are selected from at least one of nylon 6, nylon 66, and a mixture of nylon 6 and nylon 66, the viscosity of nylon 6 and nylon 66 is 1.8-3.

5.

30. The electrically insulating thermoplastic composite material according to claim 29, characterized in that: When the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 800-8000 g / 10 min, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is less than 0.18:

1.

31. The electrically insulating thermoplastic composite material according to claim 30, characterized in that: When the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 800-8000 g / 10 min, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is less than 0.15:

1.

32. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: Based on the weight of the polypropylene graft containing anhydride groups, the content of structural units derived from maleic anhydride monomers and olefinic polymerization monomers and in a grafted state in the polypropylene graft containing anhydride groups is 0.1-5% by weight; and / or the molar ratio of structural units derived from maleic anhydride monomers to structural units derived from olefinic polymerization monomers in the polypropylene graft containing anhydride groups is 1:1-20.

33. The electrically insulating thermoplastic composite material according to claim 32, characterized in that: Based on the weight of the polypropylene graft containing anhydride groups, the content of structural units derived from maleic anhydride monomers and olefinic polymerization monomers and in a grafted state in the polypropylene graft containing anhydride groups is 0.4-3% by weight; and / or the molar ratio of structural units derived from maleic anhydride monomers to structural units derived from olefinic polymerization monomers in the polypropylene graft containing anhydride groups is 1:1-10.

34. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: The comonomer of the copolymerized polypropylene is selected from at least one of C2-C8 α-olefins except propylene.

35. The electrically insulating thermoplastic composite material according to claim 34, characterized in that The comonomer of the copolymerized polypropylene is selected from at least one of ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene and 1-octene.

36. The electrically insulating thermoplastic composite material according to claim 35, characterized in that The comonomer of the copolymerized polypropylene is ethylene and / or 1-butene.

37. The electrically insulating thermoplastic composite material according to claim 36, characterized in that The copolymerized polypropylene consists of propylene and ethylene.

38. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: The olefin-containing polymerizable monomer is selected from at least one monomer having a structure shown in Formula VII, In formula VII, R1, R2, and R3 are each independently selected from H, a substituted or unsubstituted alkyl group; R4 is selected from a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted aryl group, a substituted or unsubstituted ester group, a substituted or unsubstituted carboxyl group, a substituted or unsubstituted cycloalkyl group or heterocyclic group, and a cyano group.

39. The electrically insulating thermoplastic composite material according to claim 38, characterized in that In Formula VII, R1, R2, and R3 are each independently selected from H, substituted or unsubstituted C1-C6 alkyl; R4 is selected from substituted or unsubstituted C1-C 20 Alkyl, substituted or unsubstituted C1-C 20 Alkoxy, substituted or unsubstituted C6-C 20 Aryl, substituted or unsubstituted C1-C 20 Ester group, substituted or unsubstituted C1-C 20 Carboxyl, substituted or unsubstituted C3-C 20 Cycloalkyl or heterocyclic group, cyano group, the substituted group is halogen, hydroxyl, amino, C1-C6 alkyl, C3-C6 cycloalkyl.

40. The electrically insulating thermoplastic composite material according to claim 39, characterized in that In Formula VII, R1, R2, and R3 are each independently selected from H, substituted or unsubstituted C1-C3 alkyl; R4 is selected from substituted or unsubstituted C1-C 12 Alkyl, substituted or unsubstituted C1-C 18 Alkoxy, substituted or unsubstituted C6-C 12 Aryl, substituted or unsubstituted C1-C 12 Ester group, substituted or unsubstituted C1-C 12 Carboxyl, substituted or unsubstituted C3-C 12 Cycloalkyl or heterocyclic group, cyano group, the substituted group is halogen, C1-C6 alkyl, C3-C6 cycloalkyl.

41. The electrically insulating thermoplastic composite material according to claim 40, characterized in that In Formula VII, R4 is selected from substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C1-C 12 Alkoxy, substituted or unsubstituted C6 -C8 aryl, substituted or unsubstituted C1-C6 ester, substituted or unsubstituted C1-C6 carboxyl, substituted or unsubstituted C3-C6 cycloalkyl or heterocyclic group, cyano.

42. The electrically insulating thermoplastic composite material according to claim 38, characterized in that The heterocyclic group is selected from imidazolyl, pyrazolyl, carbazolyl, pyrrolidone, pyridyl, piperidinyl, caprolactam, pyrazinyl, thiazolyl, purinyl, morpholinyl, and oxazolinyl.

43. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: The polypropylene graft containing anhydride groups, wherein R1, R2, and R3 are independently selected from H, substituted or unsubstituted C 1- C6 alkyl; R4 is selected from the group represented by formula VIII, the group represented by formula IX, the group represented by formula X, the group represented by formula XI, the combination of the group represented by formula XI and the group represented by formula XII, and a heterocyclic group; In Formula VIII, R4-R8 are each independently selected from H, halogen, hydroxyl, amino, phosphate, sulfonic acid, substituted or unsubstituted C1-C 12 Alkyl, substituted or unsubstituted C3-C 12 Cycloalkyl, substituted or unsubstituted C1-C 12 Alkoxy, substituted or unsubstituted C1-C 12 Ester group, substituted or unsubstituted C1-C 12 The substituted group is selected from halogen, hydroxyl, amino, phosphoric acid, sulfonic acid, C1-C 12 Alkyl, C3-C 12 Cycloalkyl, C1-C 12 Alkoxy, C1-C 12 Ester group, C1-C 12 The amine group; In Formula IX, R4-R 10 Each is independently selected from H, halogen, hydroxyl, amino, phosphate, sulfonic acid, substituted or unsubstituted C1-C 12 Alkyl, substituted or unsubstituted C3-C 12 Cycloalkyl, substituted or unsubstituted C1-C 12 Alkoxy, substituted or unsubstituted C1-C 12 Ester group, substituted or unsubstituted C1-C 12 The substituted group is selected from halogen, hydroxyl, amino, phosphoric acid, sulfonic acid, C1-C 12 Alkyl, C3-C 12 Cycloalkyl, C1-C 12 Alkoxy, C1-C 12 Ester group, C1-C 12 The amine group; In Formula X, R4'-R 10 ' are each independently selected from H, halogen, hydroxyl, amino, phosphate, sulfonic acid, substituted or unsubstituted C1-C 12 Alkyl, substituted or unsubstituted C3-C 12 Cycloalkyl, substituted or unsubstituted C1-C 12 Alkoxy, substituted or unsubstituted C1-C 12 Ester group, substituted or unsubstituted C1-C 12 The substituted group is selected from halogen, hydroxyl, amino, phosphoric acid, sulfonic acid, C1-C 12 Alkyl, C3-C 12 Cycloalkyl, C1-C 12 Alkoxy, C 1- C 12 Ester group, C1-C 12 The amine group; In formula XI, Rm is selected from the following substituted or unsubstituted groups: C1-C 20 Straight chain alkyl, C3-C 20 Branched alkyl, C3-C 12 Cycloalkyl, C3-C 12 The alkylene oxide group is selected from at least one of halogen, amino and hydroxyl groups.

44. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: In formula VIII, R4-R8 are each independently selected from H, halogen, hydroxyl, amino, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C1-C6 alkoxy; In Formula IX, R4-R 10 Each is independently selected from H, halogen, hydroxyl, amino, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C1-C6 alkoxy, the substituted group is selected from halogen, hydroxyl, amino, C1-C6 alkyl, C1-C6 alkoxy, In Formula X, R4'-R 10 ' are each independently selected from H, halogen, hydroxyl, amino, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C1-C6 alkoxy, and the substituted group is selected from halogen, hydroxyl, amino, C1-C6 alkyl, C1-C6 alkoxy.

45. The electrically insulating thermoplastic composite material according to claim 38, characterized in that The olefin-containing polymerization monomer is selected from at least one of vinyl acetate, styrene, α-methylstyrene, (meth)acrylate, vinyl alkyl ether, vinyl pyrrolidone, vinyl pyridine, vinyl imidazole and acrylonitrile; the (meth)acrylate is at least one of methyl (meth)acrylate, ethyl (meth)acrylate and glycidyl (meth)acrylate.

46. ​​The electrically insulating thermoplastic composite material according to claim 45, characterized in that The olefin-containing polymerizable monomer is selected from vinyl acetate, styrene, and α-methylstyrene.

47. The electrically insulating thermoplastic composite material according to claim 46, characterized in that The olefin-containing polymerizable monomer is styrene.

48. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: In the polypropylene graft containing anhydride groups, the molar ratio of the structural unit derived from the anhydride monomer to the structural unit derived from the olefin-containing polymerization monomer is 1:1-20.

49. The electrically insulating thermoplastic composite material according to claim 48, characterized in that In the polypropylene graft containing anhydride groups, the molar ratio of the structural unit derived from the anhydride monomer to the structural unit derived from the olefin-containing polymerization monomer is 1:1-10.

50. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: The polypropylene graft containing anhydride groups has at least one of the following characteristics: a melt flow rate of 0.01-30 g / 10 min at 230° C. and a load of 2.16 kg; Based on 100 parts by weight of the first thermoplastic resin and 100 parts by weight of the second thermoplastic resin, the first auxiliary agent and the second auxiliary agent each independently include 2-30 parts by weight of an electrical insulation modifier.

51. The electrically insulating thermoplastic composite material according to any one of claims 50, characterized in that: The polypropylene graft containing anhydride groups has at least one of the following characteristics: a melt flow rate of 0.05-20 g / 10 min at 230° C. and a load of 2.16 kg; Based on 100 parts by weight of the first thermoplastic resin and the second thermoplastic resin, the first auxiliary agent and the second auxiliary agent each independently include 5-25 parts of an electrical insulation modifier.

52. The electrically insulating thermoplastic composite material according to claim 51, characterized in that The polypropylene graft containing anhydride groups has at least one of the following characteristics: a melt flow rate of 0.1-10 g / 10 min at 230° C. and a load of 2.16 kg.

53. The electrically insulating thermoplastic composite material according to claim 52, characterized in that The polypropylene graft containing anhydride groups has at least one of the following characteristics: a melt flow rate of 0.2-8 g / 10 min at 230° C. and a load of 2.16 kg.

54. The electrically insulating thermoplastic composite material according to any one of claims 1 to 13, characterized in that: Based on 100 parts by weight of the first thermoplastic resin and the second thermoplastic resin, the first auxiliary agent and the second auxiliary agent each independently include at least one of 0.5-15 parts by weight of a compatibilizer, 0.05-3 parts by weight of an antioxidant, and 0.05-2.5 parts by weight of a lubricant; and / or, The compatibilizer is selected from at least one of the polar monomer graft-modified polymers; and / or, The antioxidant is at least one selected from tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol, tris[2,4-di-tert-butylphenyl]phosphite, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane and bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite; and / or, The lubricant is selected from at least one of ethylene bisstearamide, calcium stearate, polyethylene wax, pentaerythritol stearate, silicone, polyethylene glycol and fluorine-containing resin; and / or, The first auxiliary agent also includes at least one of a lubricant, an antistatic agent and a plasticizer; And / or the second auxiliary agent further includes at least one of a lubricant, a plasticizer, a nucleating agent, a light stabilizer, a flame retardant, a heat stabilizer, a masterbatch, an antistatic agent and a filler.

55. The electrically insulating thermoplastic composite material according to claim 54, characterized in that The first auxiliary agent and the second auxiliary agent each independently include 1-15 parts by weight of a compatibilizer, 0.1-1 parts by weight of an antioxidant and 0.5-2.5 parts by weight of a lubricant; and / or, The polar monomer is selected from at least one of maleic anhydride, maleic anhydride derivatives, acrylic acid and acrylate derivatives; and / or the polymer is selected from at least one of polyethylene, polypropylene, ethylene-α-octene copolymer and propylene-α-olefin copolymer.

56. The electrically insulating thermoplastic composite material according to claim 55, characterized in that The first auxiliary agent and the second auxiliary agent each independently include at least one of 1-6 parts by weight of a compatibilizer and 0.1-0.5 parts by weight of an antioxidant.

57. The electrically insulating thermoplastic composite material according to claim 56, characterized in that The first auxiliary agent and the second auxiliary agent each independently include 3-6 parts by weight of a compatibilizer.

58. The method for preparing the electrically insulating thermoplastic composite material according to any one of claims 1 to 57, characterized in that: The method comprises the following steps: Step A, a first thermoplastic resin and a first auxiliary agent are mixed and melted to obtain a first component melt; Step B, performing a first impregnation treatment on the continuous fiber bundle and the first component melt to form a filamentous core layer product; Step C, the second thermoplastic resin and the second auxiliary agent are mixed and melted to obtain a second component melt; Step D: subjecting the filamentous core layer product to a second impregnation treatment with the second component melt to form a resin layer wrapping the core layer.

59. The preparation method according to claim 58, characterized in that The mixing conditions of step A include: temperature of 40-60°C, time of 0.5-20 min; melting temperature of step A of 200-380°C; and / or, The mixing conditions of step C include: temperature of 40-60° C., time of 0.5-20 min; and melting temperature of step C of 200-380° C.

60. The preparation method according to claim 59, characterized in that: The mixing conditions of step A include: a time of 1-10 min; and / or, The mixing conditions of step C include: time is 1-10 minutes.

61. The preparation method according to claim 60, characterized in that: The mixing conditions of step A include: a time of 3-5 min and / or, The mixing conditions of step C include: time is 3-5 minutes.

62. The preparation method according to any one of claims 58 to 61, characterized in that: In step B, the first impregnation treatment is carried out in a first impregnation mold, which is an adjustable impregnation mold. The first impregnation mold includes a fiber inlet, a fiber outlet and a melt flow channel, and at least one first guide roller is arranged in the mold cavity of the first impregnation mold; the first guide roller can move between the fiber inlet and the fiber outlet; and / or the first guide roller can move in a direction perpendicular to the line connecting the fiber inlet and the fiber outlet.

63. The preparation method according to any one of claims 58 to 61, characterized in that: In step B, the first impregnation treatment is carried out in a second impregnation mold, and the second impregnation mold is a combined impregnation mold, which includes a first module, an intermediate module and a second module connected in sequence, the first module is provided with a fiber inlet and a first module flow channel, the second module is provided with a fiber outlet and a second module flow channel, and the intermediate module is provided with an intermediate module flow channel; after the first module, the intermediate module and the second module are connected in sequence, the first module flow channel, the intermediate module flow channel and the second module flow channel are connected to form a combined flow channel for the fiber to pass through.

64. The preparation method according to any one of claims 58 to 61, characterized in that In step B, the first impregnation treatment is carried out in a third impregnation mold, and the third impregnation mold is a strong turbulence impregnation mold. The third impregnation mold includes a fiber inlet channel, an impregnation outlet and a melt gap flow channel, and the fiber inlet channel, the impregnation outlet and the melt gap flow channel are all connected to the mold cavity inside the third impregnation mold; wherein a second guide wire roller is arranged in the mold cavity of the third impregnation mold, and the second guide wire roller includes at least one active guide wire roller, and the active guide wire roller is driven to rotate by a driving device.

65. Application of the electrically insulating thermoplastic composite material described in any one of claims 1 to 57 or the electrically insulating thermoplastic composite material prepared by the preparation method described in any one of claims 58 to 64 in the fields of automobile industry, machinery manufacturing, electronic appliances, chemical industry and environmental protection, aerospace communications and construction industry.

66. The use according to claim 65, characterized in that The application is application in large automobile parts and / or high-precision electronic and electrical components.

67. The use according to claim 66, characterized in that The application is application in an automobile front-end module and / or an all-plastic tailgate inner panel.