Water-resistant wood paint and preparation method thereof
Through the combination of polyvinyl alcohol modified water-based polyurethane-acrylate emulsion and water-based polyurethane modified acrylate emulsion and the combined application of silicone slip agent, the problem of poor water resistance in traditional wood paint is solved, and high water resistance and hardness are achieved and improve mechanical properties, low cost and excellent paint film performance.
Patent Information
- Application Number
- CN202211662794.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-23
AI Technical Summary
Due to the uneven molecular mass distribution of traditional acrylate water-based wood paint, the emulsifier is prone to surface migration during film formation, resulting in poor water resistance.
The combination of polyvinyl alcohol modified water-based polyurethane-acrylate emulsion and water-based polyurethane modified acrylate emulsion is combined with silicone slip agent and photoinitiator to improve the water resistance of wood paint through specific preparation methods and process steps. Hardness and mechanical properties.
It significantly improves the water resistance, adhesion, hardness and mechanical properties of wood paint, is low in cost, and has excellent paint film performance, and significantly improves stain resistance and wear resistance.
Smart Images

Figure BDA0004013598470000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a water-resistant wood paint and a preparation method thereof. Background Art
[0002] Wood paint is a protective and decorative coating used on wood, wood boards, density boards, furniture, kitchen cabinets, office desks, paper panels and other places. In my country, the production and use of wood paint is second only to industrial paint, and the annual consumption has exceeded 400,000 tons.
[0003] Traditional acrylic water-based wood paint has become one of the main products in the market due to its good environmental resistance, high temperature resistance and low VOC. However, due to the uneven molecular weight distribution of traditional water-based wood paint, the emulsifier is easy to migrate on the surface during film formation, which affects the water resistance. In order to solve the problem that the traditional acrylic wood paint emulsion has poor water resistance, the present invention provides a water-resistant wood paint and a preparation method thereof. Summary of the invention
[0004] Based on this, the present invention provides a water-resistant wood paint and a preparation method thereof, aiming to solve the problems of the background technology.
[0005] In order to achieve the above-mentioned purpose, the present invention provides the following technical solutions:
[0006] A water-resistant wood paint is composed of the following components in percentage by weight: 78-85% of modified acrylate emulsion, 1-3% of matting agent, 0.1-0.5% of slip agent, 0.5-2% of photoinitiator, 0.2-1% of auxiliary agent, and the balance of deionized water; the modified acrylate emulsion is a mixture of polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion and waterborne polyurethane modified acrylate emulsion, and the mass ratio of the polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion to the waterborne polyurethane modified acrylate emulsion is 1:(1-3).
[0007] The invention uses polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion in combination with waterborne polyurethane modified acrylate emulsion to significantly improve the comprehensive performance of wood paint, which has good fullness, good hardness, quick drying, high gloss, good water resistance and low cost.
[0008] Furthermore, the polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion is prepared by the following method: adding an acrylic monomer mixture to a polyurethane prepolymer, stirring evenly, then adding a polyvinyl alcohol aqueous solution, stirring quickly to evenly disperse the polyurethane prepolymer, adding a neutralizing agent, heating to 60°C for insulation reaction, controlling the temperature not to exceed 70°C, and cooling to 40-50°C for maturation after the reaction is completed.
[0009] The invention introduces polyvinyl alcohol and acrylic resin to modify waterborne polyurethane. The polyvinyl alcohol contains more hydroxyl groups, which are grafted with isocyanate groups in polyurethane prepolymers. After the polyurethane prepolymers are dispersed, the acrylic monomers and the polyurethane-polyvinyl alcohol macromolecules with terminal hydroxyl groups are copolymerized by heating and the action of an initiator to obtain a highly cross-linked macromolecular polymer having the advantages of polyurethane, acrylate and polyvinyl alcohol, and having excellent bonding performance, water resistance and mechanical properties.
[0010] Furthermore, the acrylic acid monomer mixture is prepared by mixing acrylic acid monomers and initiators, and the mass ratio of the acrylic acid monomers to the initiators is (20-100):1.
[0011] Furthermore, the acrylic acid monomer is a mixture of methacrylic acid and ethyl acrylate, the mass ratio of methacrylic acid to ethyl acrylate is 1:1, and the initiator is benzoyl peroxide or azobisisosuccinonitrile.
[0012] Furthermore, the polyurethane prepolymer is prepared by the following method: 1) adding polyester polyol to a reaction kettle, evacuating the system, controlling the temperature at 90°C-110°C, and stirring for 1 hour; 2) cooling the system to 40°C-50°C, and passing nitrogen through the system for protection; 3) adding toluene diisocyanate to the reaction kettle, stirring, controlling the temperature at 60°C-80°C, and reacting for 2 hours; 4) after the reaction is completed, evacuating the system to remove bubbles, and obtaining a polyurethane prepolymer.
[0013] Furthermore, the polyester polyol is a liquid polyester polyol with a molecular weight between 500 and 1500, and the liquid polyester polyol is obtained by reacting an alcohol and an acid, wherein the acid is one or more of adipic acid, sebacic acid, terephthalic acid, isophthalic acid, and phthalic acid, and the alcohol is one or more of 1,2-ethylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, diethylene glycol, and neopentyl alcohol.
[0014] By setting the molecular weight of the polyester polyol to between 500 and 1500, the mechanical properties of the polyurethane prepolymer can be well improved, and the hardness and mechanical properties of the wood coating can be increased.
[0015] The polyvinyl alcohol aqueous solution is prepared by adding polyvinyl alcohol into deionized water, heating the water to 85-95° C. and stirring the water until the water is completely dissolved.
[0016] Furthermore, the matting agent is at least one of Acematt TS 100, Ceraflour 920, Ultralube D816, and Sylysia256NF, and the slip agent is an organic silicone slip agent.
[0017] Organic silicon slip agents can improve the flatness of the paint film, enhance surface smoothness, enhance anti-rebound properties, and provide a good feel. The combined application of organic silicon slip agents and matting agents in wood paints can improve the performance of the paint film, enhance the matting effect of the paint film, and significantly improve the stain resistance, abrasion resistance, and water resistance.
[0018] Furthermore, the photoinitiator is at least one of Irgacure 500, Irgacure 819W, Irgacure 184, and Irgacure 369.
[0019] Furthermore, the auxiliary agent is at least one of a wetting agent, a defoaming agent, an anti-settling agent and a dispersing agent. The wetting agent, the defoaming agent, the anti-settling agent and the dispersing agent in the present invention can be selected from commercial products.
[0020] The present invention also provides a method for preparing a water-resistant wood paint, comprising the following steps: 1) adding a modified acrylic emulsion, a slip agent and a photoinitiator to a production cylinder, washing the cylinder with part of deionized water and adjusting the dispersion state, dispersing at a speed of 2000-2500 rpm for 10-15 minutes, wherein the washing machine is used to clean the inner periphery and the dispersion axis of the production cylinder; 2) adding a matting agent to the production cylinder of step 1), washing the cylinder with part of deionized water and adjusting the dispersion state, dispersing at a speed of 2000-2500 rpm for 10-15 minutes, and detecting the fineness of the dispersion liquid to be ≤25 microns; 3) adding an auxiliary agent to the production cylinder of step 2), dispersing at a speed of 1200-1500 rpm for 10-15 minutes; 4) adding the remaining deionized water, washing the cylinder and stirring evenly.
[0021] The water-resistant wood paint and preparation method thereof provided by the present invention have the following beneficial effects compared with the prior art:
[0022] The invention uses polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion in combination with waterborne polyurethane modified acrylate emulsion to significantly improve the comprehensive performance of wood paint, which has good fullness, good hardness, quick drying, high gloss, good water resistance and low cost.
[0023] The present invention prepares polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion by a specific method and adds the emulsion into the wood paint formula system, thereby improving the water resistance, adhesion, hardness and mechanical properties of the wood paint.
[0024] The present invention can improve the performance of the paint film, enhance the matting effect of the paint film, and significantly improve the stain resistance, wear resistance and water resistance by jointly applying the organosilicon slip agent and the matting agent to the wood paint.
[0025] In summary, the wood paint of the present invention has the advantages of high hardness, strong water resistance, high adhesion, good stain resistance and good fullness. DETAILED DESCRIPTION
[0026] The present invention is described in detail below in conjunction with specific embodiments.
[0027] The aqueous polyurethane modified acrylate emulsion of the present invention can be prepared by conventional techniques, or by the following method:
[0028] (1) polytetrahydrofuran ether diol is dehydrated under the condition of 100 ℃ and vacuum tightness of 0.06Mpa, and the dehydration time is 1 hour, and cooling is performed to obtain the polytetrahydrofuran ether diol after dehydration, and it is standby;
[0029] (2) Add 80 g of dehydrated polytetramethylene glycol, 90 g of isophorone diisocyanate, 1 g of 1,4-butanediol, 1 g of trimethylolpropane and 10 g of dimethylolpropionic acid into a reaction kettle, react at 85° C. for 2 hours, then cool to 60° C., add 4 g of hydroxyethyl acrylate, react for 2 hours, then cool to 45° C., add 6 g of triethylamine for neutralization, add 1000 g of water for emulsification after neutralization, and add 5 g of ethylenediamine for chain extension after emulsification for 40 minutes to obtain a waterborne polyurethane emulsion;
[0030] (3) 150 g of methyl methacrylate, 30 g of butyl acrylate and 20 g of ethyl acetoacetate methacrylate were added to the aqueous polyurethane emulsion obtained in step (2) for emulsification. After standing and swelling for 1 hour, the temperature was raised to 80° C., 25 g of an aqueous solution of potassium persulfate (the mass ratio of ammonium persulfate to water was 1:24) was added dropwise for 4 hours, and the temperature was lowered to 35° C. after keeping the temperature for 2 hours. 8 g of CoatOSil 2287, 12 g of an aqueous solution of zinc carbonate (the mass ratio of zinc carbonate to water was 4:8) and 5 g of ethylenediamine were added. The mixture was stirred evenly and then discharged to obtain an aqueous polyurethane modified acrylate emulsion.
[0031] The waterborne polyurethane modified acrylate emulsion prepared by the above method not only improves the anti-adhesion performance of the film obtained after the emulsion is made into a film, but also improves the hardness and water resistance of the film. In particular, when compounded with polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion, the water resistance of wood coating is significantly improved.
[0032] Example 1
[0033] A water-resistant wood paint is composed of the following components in percentage by weight: 78% of modified acrylate emulsion, 1% of Ceraflour 920, 0.1% of silicone slip agent, 1% of Irgacure 500, 1% of Irgacure 369, 0.1% of wetting agent, 0.1% of defoaming agent, and the balance of deionized water; the modified acrylate emulsion is a mixture of polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion and waterborne polyurethane modified acrylate emulsion, and the mass ratio of the polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion to the waterborne polyurethane modified acrylate emulsion is 1:1.
[0034] The polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion is prepared by the following method: adding an acrylic monomer mixture to a polyurethane prepolymer, stirring evenly, then adding a polyvinyl alcohol aqueous solution, stirring quickly to evenly disperse the polyurethane prepolymer, adding triethylamine, heating to 60° C. for heat preservation and reaction, controlling the temperature not to exceed 70° C., and cooling to 50° C. for maturation after the reaction is completed.
[0035] The acrylic acid monomer mixture is prepared by mixing acrylic acid monomers and initiators, and the mass ratio of the acrylic acid monomers to the initiators is 100:1.
[0036] The acrylic acid monomer is a mixture of methacrylic acid and ethyl acrylate, the mass ratio of the methacrylic acid to the ethyl acrylate is 1:1, and the initiator is benzoyl peroxide.
[0037] The polyurethane prepolymer is prepared by the following method: 1) adding polyester polyol to a reaction kettle, evacuating the system, controlling the temperature at 110°C, and stirring for 1 hour; 2) cooling the system to 50°C, and passing nitrogen through the system for protection; 3) adding toluene diisocyanate to the reaction kettle, stirring, controlling the temperature at 60°C, and reacting for 2 hours; 4) after the reaction is completed, evacuating the system to remove bubbles, and obtaining a polyurethane prepolymer.
[0038] The polyester polyol is a liquid polyester polyol with a molecular weight between 500 and 1500. The liquid polyester polyol is obtained by reacting an alcohol and an acid. The acid is adipic acid and the alcohol is 1,2-ethylene glycol.
[0039] The polyvinyl alcohol aqueous solution is prepared by adding polyvinyl alcohol to deionized water, heating to 95° C. and stirring until completely dissolved, and the mass ratio of polyvinyl alcohol to deionized water is 1:2.
[0040] A method for preparing a water-resistant wood paint comprises the following steps: 1) adding a modified acrylic emulsion, an organic silicon slip agent, Irgacure 500 and Irgacure 369 to a production cylinder, washing the cylinder with part of deionized water and adjusting the dispersion state, and dispersing the cylinder at a speed of 2500 rpm for 15 minutes, wherein the washing machine is used to clean the inner periphery and the dispersion axis of the production cylinder; 2) adding Ceraflour 920 to the production cylinder of step 1), washing the cylinder with part of deionized water and adjusting the dispersion state, and dispersing the cylinder at a speed of 2500 rpm for 10 minutes, and detecting the fineness of the dispersion liquid to be ≤25 microns; 3) adding a wetting agent and a defoaming agent to the production cylinder of step 2), and dispersing the cylinder at a speed of 1200 rpm for 10 minutes; and 4) adding the remaining deionized water, washing the cylinder and stirring the cylinder evenly.
[0041] Example 2
[0042] A water-resistant wood paint is composed of the following components in percentage by weight: 85% of modified acrylate emulsion, 1% of Acematt TS 100, 2% of Sylysia 256NF, 0.5% of silicone slip agent, 0.5% of Irgacure 819W, 0.1% of wetting agent, 0.1% of defoaming agent, 0.4% of anti-settling agent, 0.4% of dispersant, and the balance of deionized water; the modified acrylate emulsion is a mixture of polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion and waterborne polyurethane modified acrylate emulsion, and the mass ratio of the polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion to the waterborne polyurethane modified acrylate emulsion is 1:3.
[0043] The polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion is prepared by the following method: adding an acrylic monomer mixture to a polyurethane prepolymer, stirring evenly, then adding a polyvinyl alcohol aqueous solution, stirring quickly to evenly disperse the polyurethane prepolymer, adding diethanolamine, heating to 60°C for insulation reaction, controlling the temperature not to exceed 70°C, and cooling to 40°C for maturation after the reaction is completed.
[0044] Furthermore, the acrylic monomer mixture is prepared by mixing acrylic monomers and initiators, and the mass ratio of the acrylic monomers to the initiator is 20:1.
[0045] Furthermore, the acrylic acid monomer is a mixture of methacrylic acid and ethyl acrylate, the mass ratio of methacrylic acid to ethyl acrylate is 1:1, and the initiator is azobisisosuccinonitrile.
[0046] Furthermore, the polyurethane prepolymer is prepared by the following method: 1) adding polyester polyol to a reaction kettle, evacuating the system, controlling the temperature at 110°C, and stirring for 1 hour; 2) cooling the system to 40°C, and passing nitrogen through the system for protection; 3) adding toluene diisocyanate to the reaction kettle, stirring, controlling the temperature at 80°C, and reacting for 2 hours; 4) after the reaction is completed, evacuating the system to remove bubbles, and obtaining a polyurethane prepolymer.
[0047] Furthermore, the polyester polyol is a liquid polyester polyol with a molecular weight between 500 and 1500, and the liquid polyester polyol is obtained by reacting an alcohol and an acid, wherein the acid is one or more of adipic acid, sebacic acid, terephthalic acid, isophthalic acid, and phthalic acid, and the alcohol is one or more of 1,2-ethylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, diethylene glycol, and neopentyl alcohol.
[0048] The polyvinyl alcohol aqueous solution is prepared by adding polyvinyl alcohol to deionized water, heating to 95° C. and stirring until completely dissolved, and the mass ratio of polyvinyl alcohol to deionized water is 1:3.
[0049] A method for preparing a water-resistant wood paint comprises the following steps: 1) adding a modified acrylic emulsion, an organic silicon slip agent and Irgacure 819W to a production cylinder, washing the cylinder with part of deionized water and adjusting the dispersion state, and dispersing the cylinder at a speed of 2000 rpm for 15 minutes, wherein the washing cylinder is used to clean the inner periphery and the dispersion axis of the production cylinder; 2) adding Acematt TS100 and Sylysia 256NF to the production cylinder of step 1), washing the cylinder with part of deionized water and adjusting the dispersion state, and dispersing the cylinder at a speed of 2000 rpm for 10 minutes, and detecting the fineness of the dispersion liquid to be ≤25 microns; 3) adding a wetting agent, a defoaming agent, an anti-settling agent and a dispersant to the production cylinder of step 2), and dispersing the cylinder at a speed of 1500 rpm for 15 minutes; 4) adding the remaining deionized water, washing the cylinder and stirring the cylinder evenly.
[0050] Example 3
[0051] A water-resistant wood paint is composed of the following components in percentage by weight: 80% of modified acrylate emulsion, 1% of Acematt TS 100, 1% of Ceraflour 920, 0.3% of silicone slip agent, 0.5% of Irgacure 500, 0.5% of Irgacure 184, 0.1% of wetting agent, 0.1% of defoaming agent, 0.2% of anti-settling agent, 0.1% of dispersant, and the balance of deionized water; the modified acrylate emulsion is a mixture of polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion and waterborne polyurethane modified acrylate emulsion, and the mass ratio of the polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion to the waterborne polyurethane modified acrylate emulsion is 1:2.
[0052] The polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion is prepared by the following method: adding an acrylic monomer mixture to a polyurethane prepolymer, stirring evenly, then adding a polyvinyl alcohol aqueous solution, stirring quickly to evenly disperse the polyurethane prepolymer, adding triethanolamine, heating to 60°C for insulation reaction, controlling the temperature not to exceed 70°C, and cooling to 50°C for maturation after the reaction is completed.
[0053] Furthermore, the acrylic monomer mixture is prepared by mixing acrylic monomers and initiators, and the mass ratio of the acrylic monomers to the initiators is 60:1.
[0054] Furthermore, the acrylic acid monomer is a mixture of methacrylic acid and ethyl acrylate, the mass ratio of methacrylic acid to ethyl acrylate is 1:1, and the initiator is benzoyl peroxide.
[0055] Furthermore, the polyurethane prepolymer is prepared by the following method: 1) adding polyester polyol to a reaction kettle, evacuating the system, controlling the temperature at 100°C, and stirring for 1 hour; 2) cooling the system to 40°C, and passing nitrogen through the system for protection; 3) adding toluene diisocyanate to the reaction kettle, stirring, controlling the temperature at 770°C, and reacting for 2 hours; 4) after the reaction is completed, evacuating the system to remove bubbles, and obtaining a polyurethane prepolymer.
[0056] Furthermore, the polyester polyol is a liquid polyester polyol with a molecular weight between 500 and 1500, and the liquid polyester polyol is obtained by reacting an alcohol and an acid, wherein the acid is one or more of adipic acid, sebacic acid, terephthalic acid, isophthalic acid, and phthalic acid, and the alcohol is one or more of 1,2-ethylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, diethylene glycol, and neopentyl alcohol.
[0057] The polyvinyl alcohol aqueous solution is prepared by adding polyvinyl alcohol to deionized water, heating to 90° C. and stirring until completely dissolved, and the mass ratio of polyvinyl alcohol to deionized water is 1:4.
[0058] A method for preparing a water-resistant wood paint comprises the following steps: 1) adding a modified acrylic emulsion, a slip agent, Irgacure 500 and Irgacure 184 to a production tank, washing the tank with part of deionized water and adjusting the dispersion state, and dispersing the mixture at a speed of 2300 rpm for 12 minutes, wherein the washing machine is used to clean the inner periphery and the dispersion axis of the production tank; 2) adding Acematt TS 100 and Ceraflour 920 to the production tank of step 1), washing the tank with part of deionized water and adjusting the dispersion state, and dispersing the mixture at a speed of 2500 rpm for 10 minutes, and detecting the fineness of the dispersion liquid to be ≤25 microns; 3) adding a wetting agent, a defoaming agent, an anti-settling agent and a dispersant to the production tank of step 2), and dispersing the mixture at a speed of 1500 rpm for 15 minutes; and 4) adding the remaining deionized water, washing the tank and stirring the mixture evenly.
[0059] Comparative Example 1
[0060] The difference from Example 3 is that in Comparative Example 1, no polyvinyl alcohol-modified aqueous polyurethane-acrylate emulsion is added.
[0061] Comparative Example 2
[0062] The difference from Example 3 is that in Comparative Example 2, no waterborne polyurethane modified acrylate emulsion is added.
[0063] Comparative Example 3
[0064] The difference from Example 3 is that in the preparation method of polyvinyl alcohol-modified water-based polyurethane-acrylate emulsion in Comparative Example 3, the preparation of the polyurethane prepolymer is as follows: polyester diol 2000, polyether triol 5000 and dihydroxymethylbutyric acid are added to a four-necked flask, stirred evenly, heated to 100°C for vacuum dehydration for 1 hour, cooled to 60°C after dehydration, and then diisocyanate IPDI is added, and organic bismuth is added dropwise, and the temperature is raised to 75°C for reaction for 3 hours.
[0065] The performance of the wood coatings prepared in Examples 1-3 and Comparative Examples 1-3 was tested, and the results are shown in Table 1:
[0066] Table 1
[0067]
[0068] Note: ① Adhesion is best at level 0 and worst at level 5, and the national standard limit is ≤ level 1; ② Pencil hardness increases from 4B to 6H; ③ Paint film surface pollution resistance: level 1 is best and level 5 is worst.
[0069] Refer to GB / T 9286-1998 "Determination of paint film adhesion" to evaluate paint film adhesion; GB / T6739-2006 "Determination of paint film hardness by pencil method for paints and varnishes" to test paint film hardness; refer to GB / T23999-2009 "Water-based wood coatings for interior decoration and renovation" to prepare alcohol, vinegar, tea and boiling water, and then follow GB / T 4893.1-2005 "Determination of cold liquid resistance of furniture surface" to evaluate the boiling water resistance, alcohol resistance and stain resistance of the paint film surface.
[0070] In the absence of conflict, the above embodiments and features in the embodiments can be combined with each other. Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it should be understood by those skilled in the art that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A water-resistant wood paint, comprising the following components in percentage by weight: Modified acrylic emulsion 78%, Ceraflour 920 1%, silicone slip agent 0.1%, Irgacure 500 1%, Irgacure369 1%, wetting agent 0.1%, defoaming agent 0.1%, and deionized water as the balance; the modified acrylic emulsion is a mixture of polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion and waterborne polyurethane modified acrylic emulsion, and the mass ratio of the polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion to the waterborne polyurethane modified acrylic emulsion is 1:1; The polyvinyl alcohol modified waterborne polyurethane-acrylate emulsion is prepared by the following method: adding an acrylic monomer mixture to a polyurethane prepolymer, stirring evenly, then adding a polyvinyl alcohol aqueous solution, stirring rapidly to uniformly disperse the polyurethane prepolymer, adding triethylamine, heating to 60° C. for heat preservation and reaction, controlling the temperature not to exceed 70° C., and cooling to 50° C. for maturation after the reaction is completed; The acrylic acid monomer mixture is prepared by mixing acrylic acid monomer and initiator, and the mass ratio of the acrylic acid monomer to the initiator is 100:1; The acrylic acid monomer is a mixture of methacrylic acid and ethyl acrylate, the mass ratio of methacrylic acid to ethyl acrylate is 1:1, and the initiator is benzoyl peroxide; The polyurethane prepolymer is prepared by the following steps: 1) adding polyester polyol to a reaction kettle, evacuating the system, controlling the temperature at 110°C, and stirring for 1 hour; 2) cooling the system to 50°C, and passing nitrogen gas through the system for protection; 3) adding toluene diisocyanate to the reaction kettle, stirring, controlling the temperature at 60°C, and reacting for 2 hours; 4) after the reaction is completed, evacuating the system to remove bubbles, and obtaining a polyurethane prepolymer; The polyester polyol is a liquid polyester polyol with a molecular weight between 500 and 1500, and the liquid polyester polyol is obtained by reacting an alcohol and an acid, wherein the acid is adipic acid and the alcohol is 1,2-ethylene glycol; The polyvinyl alcohol aqueous solution is prepared by adding polyvinyl alcohol to deionized water, heating to 95° C. and stirring until completely dissolved, wherein the mass ratio of polyvinyl alcohol to deionized water is 1:2; A method for preparing a water-resistant wood paint comprises the following steps: 1) adding a modified acrylic emulsion, an organic silicon slip agent, Irgacure 500 and Irgacure 369 to a production tank, washing the tank with part of deionized water and adjusting the dispersion state, dispersing the mixture at a speed of 2500 rpm for 15 minutes, wherein the washing machine is used to clean the inner periphery and the dispersion axis of the production tank; 2) adding Ceraflour 920 to the production tank of step 1), washing the tank with part of deionized water and adjusting the dispersion state, dispersing the mixture at a speed of 2500 rpm for 10 minutes, and detecting the fineness of the dispersion liquid to be ≤25 microns; 3) adding a wetting agent and a defoaming agent to the production tank of step 2), dispersing the mixture at a speed of 1200 rpm for 10 minutes; 4) adding the remaining deionized water, washing the tank and stirring the mixture evenly; The aqueous polyurethane modified acrylate emulsion is prepared by the following method: (1) polytetrahydrofuran ether diol is dehydrated under the condition of 100 ℃ and vacuum tightness of 0.06Mpa, and the dehydration time is 1 hour, and cooling is performed to obtain the polytetrahydrofuran ether diol after dehydration, and it is standby; (2) Add 80 g of dehydrated polytetramethylene glycol, 90 g of isophorone diisocyanate, 1 g of 1,4-butanediol, 1 g of trimethylolpropane and 10 g of dimethylolpropionic acid into a reaction kettle, react at 85° C. for 2 hours, then cool to 60° C., add 4 g of hydroxyethyl acrylate, react for 2 hours, then cool to 45° C., add 6 g of triethylamine for neutralization, add 1000 g of water for emulsification after neutralization, and add 5 g of ethylenediamine for chain extension after emulsification for 40 minutes to obtain a waterborne polyurethane emulsion; (3) To the aqueous polyurethane emulsion obtained in step (2), 150 g of methyl methacrylate, 30 g of butyl acrylate and 20 g of ethyl acetoacetate methacrylate were added for emulsification, and the mixture was allowed to stand for swelling for 1 hour, and then the temperature was raised to 80° C., 25 g of an aqueous solution of potassium persulfate was added dropwise for 4 hours, and the temperature was lowered to 35° C. after 2 hours of heat preservation, and then 8 g of CoatOSil2287, 12 g of an aqueous solution of zinc carbonate and 5 g of ethylenediamine were added, and the mixture was uniformly stirred and discharged to obtain an aqueous polyurethane modified acrylate emulsion.