A method for distributing materials in a blast furnace from central focusing to non-central focusing
By gradually adjusting the blast furnace distribution angle and air volume, the instability and fluctuation problems when the blast furnace switches from central coking to non-center coking are solved, achieving stable operation of the blast furnace and reducing fuel consumption.
Patent Information
- Application Number
- CN202310130283.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-17
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-02-17
AI Technical Summary
When the blast furnace switches from central coking to non-central coking, there are instability and blast furnace fluctuations, which lead to huge fluctuations in gas flow distribution and may even cause blast furnace abnormalities.
By gradually adjusting the distribution angle of the blast furnace, increasing the distribution angle of coke and ore in the center, reducing the distribution angle at other positions, and controlling the static pressure and heat load fluctuations of the furnace body by reducing the air volume, the transition from central coking to non-center coking is gradually realized. conversion.
It achieves a stable and smooth transition of the blast furnace from central coking to non-central coking, reduces blast furnace fluctuations, improves gas utilization, and reduces fuel consumption and fuel costs.
Abstract
Description
Technical Field
[0001] The present application relates to the field of steelmaking, and in particular to a method for distributing a blast furnace from center-coking to non-center-coking. Background Art
[0002] At present, the gas flow distribution in the upper part of the blast furnace is mainly adjusted by changing the order and position of the ore and coke distribution. The main distribution equipment of the blast furnace is the distribution chute, which can rotate up and down at a certain angle in the vertical plane to put the charge into the blast furnace at different distribution angles, so as to realize the distribution of charge at different positions in the blast furnace.
[0003] At present, the top charging system of blast furnace can be divided into center coking and non-center coking. Among them, the center coking charging system has the advantages of increasing air volume, which is conducive to improving oxygen enrichment rate and thus increasing production. However, the blast furnace gas utilization is low during center coking, and the blast furnace fuel consumption is high, which is not conducive to energy saving and consumption reduction and low-carbon smelting. At the same time, the blast furnace body is easy to thicken, which is not conducive to blast furnace maintenance. Therefore, most blast furnaces with center coking operation mode are trying to switch to non-center coking (also known as platform funnel) operation mode. However, the change of blast furnace charging system will cause huge fluctuations in the distribution of gas flow in the blast furnace, resulting in instability of the blast furnace, and even blast furnace malfunction, resulting in failure of the blast furnace when switching from center coking to non-center coking. Summary of the invention
[0004] The purpose of the present application is to provide a method for distributing materials when a blast furnace is switched from center-focusing to non-center-focusing, which can ensure stable and smooth operation of the blast furnace when it is switched from center-focusing to non-center-focusing, thereby reducing fluctuations in the blast furnace.
[0005] This application is implemented as follows:
[0006] The present application provides a method for distributing a blast furnace from center-focusing to non-center-focusing, which comprises the following steps:
[0007] When the blast furnace is operated using the center coking method, the distribution angle of coke and ore fed into the center of the blast furnace is increased to 3-5° above the critical tilting angle, and the distribution angle of coke and ore fed into other positions of the blast furnace is reduced by 0.5-0.8°, keeping the distribution weight unchanged, and operating the blast furnace stably for 48-72 hours;
[0008] The distribution angle of coke and ore fed into the center of the blast furnace will be increased by 1-1.5° every 24 hours, and the distribution angle of coke and ore fed into other positions of the blast furnace will be reduced by 0.2-0.3° every 24 hours, until the blast furnace switches from center-coking to non-center-coking to achieve the required distribution angle.
[0009] In some optional implementation schemes, when adjusting the blast furnace charge distribution angle, the blast furnace air volume is reduced to control the change of the static pressure of the blast furnace body within 10%.
[0010] In some optional implementation schemes, when adjusting the blast furnace charge distribution angle, the blast furnace air volume is reduced to control the heat load fluctuation of the blast furnace body within 20%.
[0011] In some optional embodiments, the critical tilting angle α=arctg(E / L), E is the vertical distance between the chute hanging point and the chute bottom, and L is the chute length.
[0012] In some optional embodiments, the critical tilt angle is 12-18°.
[0013] In some optional embodiments, when the blast furnace is operated using the central coking method, the charging angles of the various areas from the edge to the center of the blast furnace are 43.5°, 41.5°, 39°, 36°, 32.5°, 28.5°, 22.5° and 11.5 respectively.
[0014] The beneficial effects of the present application are as follows: the distribution method for the blast furnace provided by the present application from the center coking to the non-center coking includes the following steps: when the blast furnace is operated by the center coking method, the distribution angle of the coke and ore put into the center of the blast furnace is increased to exceed the critical tilting angle by 3-5°, and the distribution angle of the coke and ore put into other positions of the blast furnace is reduced by 0.5-0.8°, the distribution weight is kept unchanged, and the blast furnace is operated stably for 48-72 hours; the distribution angle of the coke and ore put into the center of the blast furnace is increased by 1-1.5° every 24 hours, and the distribution angle of the coke and ore put into other positions of the blast furnace is reduced by 0.2-0.3° every 24 hours, until the blast furnace is converted from the center coking to the distribution angle required for the non-center coking. The distribution method for the blast furnace converted from the center coking to the non-center coking provided by the present application can ensure that the blast furnace is stable and smooth when it is converted from the center coking to the non-center coking, and reduce the fluctuation of the blast furnace. DETAILED DESCRIPTION
[0015] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Therefore, the following detailed description of the embodiments of the present application is not intended to limit the scope of the application claimed for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians of the art without making creative work are within the scope of protection of the present application.
[0016] The characteristics and performance of the charging method for converting the blast furnace from center-coking to non-center-coking in the present application are further described in detail below in conjunction with the embodiments.
[0017] The present application provides a method for distributing a blast furnace from center-focusing to non-center-focusing, which comprises the following steps:
[0018] When the blast furnace is operated using the center coking method, the distribution angle of coke and ore fed into the center of the blast furnace is increased to 3-5° above the critical tilting angle, and the distribution angle of coke and ore fed into other positions of the blast furnace is reduced by 0.5-0.8° to keep the distribution weight unchanged and operate the blast furnace stably for 48-72 hours; wherein, the critical tilting angle α=arctg(E / L), E is the vertical distance between the chute hanging point and the bottom of the chute, and L is the chute length; in some optional embodiments, the critical tilting angle is 12-18°.
[0019] Increase the distribution angle of coke and ore fed into the center of the blast furnace by 1-1.5° every 24 hours, and reduce the distribution angle of coke and ore fed into other positions of the blast furnace by 0.2-0.3° every 24 hours, until the blast furnace is switched from center coking to non-center coking. When adjusting the distribution angle of the blast furnace, control the static pressure change of the blast furnace within 10% by reducing the blast furnace air volume, and control the heat load fluctuation of the blast furnace within 20%;
[0020] The charging method for switching a blast furnace from center coking to non-center coking provided in the present embodiment increases the charging angle of the coke and ore fed into the center of the blast furnace to a value exceeding the critical tilting angle by 3-5° at one time, and slightly reduces the charging angle of the coke and ore fed into other positions of the blast furnace to achieve highly stable operation for 2-3 days, and then further increases the charging angle of the coke and ore fed into the center of the blast furnace by 1-1.5° every 24 hours, and reduces the charging angle of the coke and ore fed into other positions of the blast furnace by 0.2-0.3° every 24 hours, until the blast furnace reaches the required charging angle when switching from center coking to non-center coking. At the same time, when adjusting the charging angle of the blast furnace, the blast furnace air volume is reduced to control the static pressure change of the blast furnace body within 10%, and the heat load fluctuation of the blast furnace body is controlled within 20%, so as to ensure the stable and smooth operation of the blast furnace when switching from center coking to non-center coking, and reduce blast furnace fluctuation.
[0021] Example 1
[0022] The effective volume of a blast furnace in Wuhan Iron and Steel is 3200m 3 The length of the distribution chute is 3800mm, the vertical distance from the hanging point of the distribution chute to the bottom of the distribution chute is 950mm, the blast furnace uses the center coking distribution mode, and the blast furnace distribution matrix is C (876541 333223), O (8765433322).
[0023] In the distribution matrix described in the embodiment of the present application, C represents coke, O represents ore, and when distributing the material, 11 distribution areas of equal area are divided from the inside to the outside along the radial direction of the blast furnace throat and are numbered 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, and 11 respectively. C (876541 333223) represents that coke is added to the numbered areas 8, 7, 6, 5, 4, and 1, and the mass ratio of the distribution material is 3:3:3:2:2:3, and O (87654 33322) means that ore is put into the numbered areas 8, 7, 6, 5, and 4, and the mass ratio of the distribution is 3:3:3:2:2; the inclination angles of the distribution chute during distribution in each numbered area are: 43.5° for area 8; 41.5° for area 7; 39° for area 6; 36° for area 5; 32.5° for area 4; 28.5° for area 3; 22.5° for area 2; and 11.5° for area 1.
[0024] The method for distributing materials in a blast furnace from center-focusing to non-center-focusing provided in this embodiment includes the following steps:
[0025] Determine the critical tilting angle of the distribution chute. The critical tilting angle of the distribution chute is the minimum tilting angle α that the material must be lifted from the central throat of the blast furnace to the distribution chute. α=arctg(E / L), E is the tilting distance of the distribution chute, that is, the vertical distance from the hanging point of the distribution chute to the bottom of the distribution chute, L is the length of the distribution chute, α=arctg(E / L)=arctg(950 / 3800)=13.8°, take 14°.
[0026] When the blast furnace is operated using the center coking method, the distribution angle of coke and ore fed into the center of the blast furnace is increased to exceed the critical tilting angle of 4°, that is, the coke angle No. 1 in the center of the blast furnace is increased from 11.5° to 18°, and at the same time, the maximum distribution angles of ore and coke in other areas are reduced by 0.5°, that is, 43° for area No. 8; 41° for area No. 7; 38.5° for area No. 6; 35.5° for area No. 5; 32° for area No. 4; 28° for area No. 3; 22° for area No. 2; and 11° for area No. 1. The original distribution weight ratio is kept unchanged and the blast furnace is operated for 2 days (48 hours).
[0027] The operation of the blast furnace is basically stable. The distribution angle of coke and ore put into the center of the blast furnace is increased by 1° every 24 hours, and the distribution angle of coke and ore put into other positions of the blast furnace is reduced by 0.2° every 24 hours. After 8 days, the distribution angle of coke and ore put into the center of the blast furnace is 26°. The distribution angles of coke and ore put into other positions of the blast furnace are: 42.2° in area 8; 40.2° in area 7; 37.7° in area 6; 34.7° in area 5; 31.2° in area 4; 27.2° in area 3, realizing the transition from the center coking mode to the non-center coking mode of the blast furnace. In the above process of adjusting the distribution angle, the static pressure of the blast furnace body and the heat load of the blast furnace body fluctuated three times, and the blast furnace air volume was reduced by 300m each time. 3 / min Wait for 2 hours and then restore the air volume.
[0028] Through the above operations, the blast furnace is transformed from the central coking mode to the non-central coking mode, which increases the gas utilization rate of the blast furnace from the original 46% to 48%, reduces the blast furnace fuel ratio by 10kg / t, and reduces the fuel cost by 20 yuan / t.
[0029] Example 2
[0030] The effective volume of a blast furnace in Wuhan Iron and Steel is 2600m 3 The length of the distribution chute is 3600mm, and the vertical distance from the hanging point of the distribution chute to the bottom of the distribution chute is 950mm. The blast furnace uses the central coking distribution mode, and the blast furnace distribution matrix is C (876541 333223), O (8765433322); the inclination angles of the distribution chute during distribution in each numbered area are: 43.5° in area 8; 41.5° in area 7; 39° in area 6; 36° in area 5; 32.5° in area 4; 28.5° in area 3; 22.5° in area 2; and 11.5° in area 1.
[0031] The method for distributing materials in a blast furnace from center-focusing to non-center-focusing provided in this embodiment includes the following steps:
[0032] Determine the critical tilting angle of the distribution chute. The critical tilting angle of the distribution chute is the minimum tilting angle α that the material must be lifted from the central throat of the blast furnace to the distribution chute. α=arctg(E / L), E is the tilting distance of the distribution chute, that is, the vertical distance from the hanging point of the distribution chute to the bottom of the distribution chute, L is the length of the distribution chute, α=arctg(E / L)=arctg(950 / 3600)=14.8°, take 15°.
[0033] When the blast furnace is operated using the center coking method, the distribution angle of the coke and ore fed into the center of the blast furnace is increased to exceed the critical tilting angle of 4°, that is, the No. 1 coke angle in the center of the blast furnace is increased from 11.5° to 19°, and at the same time, the maximum distribution angles of ore and coke in other areas are reduced by 0.5°, that is, 43° for area 8; 41° for area 7; 38.5° for area 6; 35.5° for area 5; 32° for area 4; and 28° for area 3. The original distribution weight ratio is kept unchanged and the blast furnace is operated for 3 days (72 hours).
[0034] The operation of the blast furnace is basically stable. The distribution angle of coke and ore put into the center of the blast furnace is increased by 1° every 24 hours, and the distribution angle of coke and ore put into other positions of the blast furnace is reduced by 0.2° every 24 hours. After 8 days, the distribution angle of coke and ore put into the center of the blast furnace is 27°. The distribution angles of coke and ore put into other positions of the blast furnace are: 42.2° in area 8; 40.2° in area 7; 37.7° in area 6; 34.7° in area 5; 31.2° in area 4; 27.2° in area 3, realizing the transition from the center coking mode to the non-center coking mode of the blast furnace. In the above process of adjusting the distribution angle, the static pressure of the blast furnace body and the heat load of the blast furnace body fluctuated three times, and the blast furnace air volume was reduced by 260m each time. 3 / min Wait for 1 hour and then restore the air volume.
[0035] Through the above operations, the blast furnace is transformed from the central coking mode to the non-central coking mode, and the gas utilization rate of the blast furnace is increased from the original 45% to 47%, the blast furnace fuel ratio is reduced by 10kg / t, and the fuel cost is reduced by 20 yuan / t.
[0036] Example 3
[0037] The effective volume of a blast furnace in Wuhan Iron and Steel is 1800m 3 The length of the distribution chute is 2800mm, and the vertical distance from the hanging point of the distribution chute to the bottom of the distribution chute is 800mm. The blast furnace uses the central coking distribution mode, and the blast furnace distribution matrix is C (76541 33223), O (76543322); the inclination angles of the distribution chute during distribution in each numbered area are: 41.5° in area 7; 39° in area 6; 36° in area 5; 32.5° in area 4; 28.5° in area 3; 22.5° in area 2; and 12° in area 1.
[0038] The method for distributing materials in a blast furnace from center-focusing to non-center-focusing provided in this embodiment includes the following steps:
[0039] Determine the critical tilting angle of the distribution chute. The critical tilting angle of the distribution chute is the minimum tilting angle α that the material must be lifted from the central throat of the blast furnace to the distribution chute. α=arctg(E / L), E is the tilting distance of the distribution chute, that is, the vertical distance from the hanging point of the distribution chute to the bottom of the distribution chute, L is the length of the distribution chute, α=arctg(E / L)=arctg(800 / 2800)=15.9°, take 16°.
[0040] When the blast furnace is operated using the center coking method, the distribution angle of the coke and ore fed into the center of the blast furnace is increased to exceed the critical tilting angle of 4°, that is, the No. 1 coke angle in the center of the blast furnace is increased from 12° to 20°, and at the same time, the maximum distribution angles of ore and coke in other areas are reduced by 0.5°, that is, 41° for area No. 7; 38.5° for area No. 6; 35.5° for area No. 5; 32° for area No. 4; and 28° for area No. 3. The original distribution weight ratio is maintained unchanged and the blast furnace is operated for 3 days (72 hours).
[0041] The operation of the blast furnace is basically stable. The distribution angle of coke and ore put into the center of the blast furnace is increased by 1° every 24 hours, and the distribution angle of coke and ore put into other positions of the blast furnace is reduced by 0.2° every 24 hours. After 8 days, the distribution angle of coke and ore put into the center of the blast furnace is 27°. The distribution angles of coke and ore put into other positions of the blast furnace are: 42.2° in area 8; 40.2° in area 7; 37.7° in area 6; 34.7° in area 5; 31.2° in area 4; 27.2° in area 3, realizing the transition from the center coking mode to the non-center coking mode of the blast furnace. In the above process of adjusting the distribution angle, the static pressure of the blast furnace body and the heat load of the blast furnace body fluctuated three times, and the blast furnace air volume was reduced by 200m each time. 3 / min Wait for 1 hour and then restore the air volume.
[0042] Through the above operations, the blast furnace is transformed from the central coking mode to the non-central coking mode, and the gas utilization rate of the blast furnace is increased from the original 45.5% to 48.5%, the blast furnace fuel ratio is reduced by 15kg / t, and the fuel cost is reduced by 30 yuan / t.
[0043] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
Claims
1. A method for distributing a blast furnace from center-coking to non-center-coking, characterized in that: It includes the following steps: When the blast furnace is operated using the center coking method, the distribution angle of coke and ore fed into the center of the blast furnace is increased to 3-5° above the critical tilting angle, and the distribution angle of coke and ore fed into other positions of the blast furnace is reduced by 0.5-0.8°, keeping the distribution weight unchanged, and operating the blast furnace stably for 48-72 hours; Increase the distribution angle of coke and ore fed into the center of the blast furnace by 1-1.5° every 24 hours, and reduce the distribution angle of coke and ore fed into other positions of the blast furnace by 0.2-0.3° every 24 hours, until the blast furnace switches from center coking to non-center coking to achieve the required distribution angle; When adjusting the blast furnace charging angle, the static pressure change of the blast furnace body is controlled within 10% by reducing the blast furnace air volume, and the heat load fluctuation of the blast furnace body is controlled within 20% by reducing the blast furnace air volume.
2. The method for distributing the charge of a blast furnace from center-focusing to non-center-focusing according to claim 1, characterized in that: The critical tilting angle α=arctg(E / L), E is the vertical distance between the chute hanging point and the chute bottom, and L is the chute length.
3. The method for distributing the charge of a blast furnace from center-focusing to non-center-focusing according to claim 1, characterized in that: The critical tilting angle is 12-18°.
4. The method for distributing the charge of a blast furnace from center-focusing to non-center-focusing according to claim 1, characterized in that: When the blast furnace is operated using the center coking method, the charging angles for charging to various areas from the edge to the center of the blast furnace are 43.5°, 41.5°, 39°, 36°, 32.5°, 28.5°, 22.5° and 11.5° respectively.