Method for refining primary silicon and reducing the area fraction of primary silicon in Al-18Si alloy by antimony alloying and phosphorus modification

Through antimony alloying and phosphorus deterioration treatment technology, the form of primary silicon in Al-18Si alloy is refined and improved, which solves the problem of insufficient strength and toughness in high temperature and high pressure environments, and achieves higher mechanical properties and wider application field.

CN116065047BActive Publication Date: 2024-11-19CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310010859.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-05
Publication Date
2024-11-19
Estimated Expiration
2043-01-05

AI Technical Summary

Technical Problem

The prior art is difficult to effectively refine and improve the form of primary silicon in Al-18Si alloys, resulting in insufficient strength and wear resistance in high temperature and high pressure environments, limiting the application field of aluminum-silicon alloys.

Method used

Using antimony alloying and phosphorus deterioration treatment technology, by adding an appropriate amount of antimony and Al-3P intermediate alloy to the Al-18Si alloy, the AlP phase is formed as the nucleation particle of primary silicon, thereby increasing the supercooling degree of the alloy and reducing primary silicon. The critical size of the nucleation inhibits its growth, thereby refining the primary silicon.

Benefits of technology

The average size of primary silicon was successfully refined from 44.6μm to 19.5μm, reducing its area share from 10.1% to 8.4%, improving the strength and mechanical properties of the alloy and expanding the application field of aluminum-silicon alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004038328600000041
    Figure BDA0004038328600000041
  • Figure HDA0004038328610000011
    Figure HDA0004038328610000011
  • Figure HDA0004038328610000012
    Figure HDA0004038328610000012
Patent Text Reader

Abstract

The present invention belongs to the technical field of nonferrous alloy processing and forming, and discloses a method for refining primary silicon in Al-18Si alloy by antimony alloying and phosphorus modification, and reducing the area fraction of primary silicon. The present invention melts Al-18Si hypereutectic aluminum-silicon alloy, adds pure antimony to the alloy liquid after the alloy is completely melted and keeps warm, then adds Al-3P master alloy for modification, and then pours the alloy liquid into a room temperature metal mold for molding after keeping warm. Antimony element can increase the supercooling of Al-18Si alloy melt and reduce the area fraction of primary silicon; and AlP phase in aluminum-phosphorus master alloy can be used as nucleation particle of primary silicon to refine primary silicon. When the two act synergistically, the increase of supercooling of Al-18Si alloy can reduce the critical size of nucleation of primary silicon, so that more AlP particles become the nucleation core of primary silicon, and at the same time inhibit the growth of primary silicon, refine the primary silicon in the alloy, and make the area fraction of primary silicon smaller.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonferrous alloy processing and forming, and specifically relates to a method for refining primary silicon in Al-18Si alloy and reducing the area fraction of primary silicon by utilizing the composite action of antimony alloying and phosphorus modifier. Background Art

[0002] Automobile engine pistons work under high temperature, high pressure and high-intensity alternating loads, so their materials need to have good high-temperature strength, wear resistance, low thermal expansion coefficient and other characteristics. Hypereutectic aluminum silicon alloys meet the above conditions and have excellent casting properties, especially with the increase of silicon content, the linear expansion coefficient decreases and the wear resistance increases. However, the increase of silicon content will also increase the content of primary silicon. The primary silicon in the cast hypereutectic aluminum silicon alloy will seriously split the alloy matrix, reduce the strength and toughness of the alloy, and cause matrix cracking, which seriously limits the application of hypereutectic aluminum silicon alloys. Cast aluminum alloys cannot improve the mechanical properties of the alloy through plastic deformation. Therefore, people have been looking for ways to improve the morphology of primary silicon in the structure of cast hypereutectic aluminum silicon alloys, and explore in the fields of modification, trace element alloying, spray deposition, etc., to promote the development and application of hypereutectic aluminum silicon alloys.

[0003] Although there are many studies on the refinement of primary silicon in hypereutectic aluminum-silicon alloys, the refinement effect is still limited. Phosphorus is often used in industry to modify hypereutectic aluminum-silicon alloys. After phosphorus modification, the size of primary silicon is greatly reduced in the structure, but its distribution is not uniform, and the area ratio of primary silicon increases, which limits the improvement of the mechanical properties of the alloy. Studies have found that boron modification can effectively refine the silicon phase, but its effect of refining and improving the morphology of the silicon phase is closely related to the amount of addition. If a method can be found that can inhibit the precipitation of primary silicon in hypereutectic aluminum-silicon alloys (reduce the area fraction of primary silicon), refine primary silicon and improve the morphology of primary silicon, it will further increase the strength and toughness of aluminum-silicon alloys, obtain more ideal mechanical properties, and thus expand the application field of hypereutectic aluminum-silicon alloys. Summary of the invention

[0004] The object of the present invention is to promote the refinement of primary silicon in Al-18Si alloy, reduce the area fraction of primary silicon and improve its morphology.

[0005] In order to solve the above technical problems, the present invention provides a method for refining primary silicon in Al-18Si alloy and reducing the area fraction of primary silicon by antimony alloying and phosphorus modification, which is specifically:

[0006] Al-18Si hypereutectic aluminum-silicon alloy is placed in a crucible and melted at 850°C. After the alloy is completely melted, pure antimony is added to the alloy liquid and kept warm for 25 to 30 minutes. Then, Al-3P intermediate alloy is added for modification. After keeping warm for 5 minutes, the alloy liquid is poured into a room temperature metal mold for molding.

[0007] The amount of antimony added is 0.15wt.% to 0.75wt.% of the mass of the Al-18Si hypereutectic aluminum-silicon alloy; more preferably, the amount of antimony added is 0.3wt.%.

[0008] The amount of Al-3P master alloy added is 0.2wt.% to 0.6wt.% of the mass of Al-18Si hypereutectic aluminum-silicon alloy; the more preferred amount is 0.4wt.%.

[0009] Beneficial effects of the present invention:

[0010] The present invention uses antimony to alloy the Al-18Si alloy and an aluminum-phosphorus master alloy to modify the Al-18Si alloy. The AlP phase in the aluminum-phosphorus master alloy can serve as a nucleation particle of primary silicon, refine the primary silicon and improve the morphology of the primary silicon. When the aluminum-phosphorus master alloy and antimony work together, the increase in the supercooling of the Al-18Si alloy can reduce the critical size of the nucleation of primary silicon, so that more AlP particles become the nucleation cores of primary silicon, and at the same time inhibit the growth of primary silicon, refine the primary silicon in the alloy, and make the area fraction of primary silicon smaller. The Al-18Si alloy prepared by the present invention has an average size of primary silicon refined from 44.6μm of unalloyed and unmodified to 19.5μm, and the area proportion of primary silicon is reduced from 10.1% to 8.4%.

[0011] Different from other methods of refining primary silicon, the present invention is easy to operate, low-cost, environmentally friendly and pollution-free, and has important reference value in preparing hypereutectic aluminum-silicon alloys with fine primary silicon and expanding the application fields of hypereutectic aluminum-silicon alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.

[0013] Figure 1 This is a microstructure photograph of the cross section of the Al-18Si alloy sample in Comparative Example 1;

[0014] Figure 2 This is the microstructure photo of the cross section of the Al-18Si-xSb alloy sample;

[0015] Figure 3 This is a microstructure photograph of the cross section of the Al-18Si-0.2%Al-3P alloy sample in Comparative Example 3;

[0016] Figure 4 This is a microstructure photograph of the cross section of the Al-18Si-0.4%Al-3P alloy sample in Comparative Example 4;

[0017] Figure 5 This is a microstructure photograph of the cross section of the Al-18Si-0.6%Al-3P alloy sample in Comparative Example 5;

[0018] Figure 6 This is a microstructure photograph of the cross section of the Al-18Si-0.3Sb-0.2%Al-3P alloy sample in Example 1;

[0019] Figure 7 This is a microstructure photograph of the cross section of the Al-18Si-0.3Sb-0.4%Al-3P alloy sample in Example 2;

[0020] Figure 8 This is a microstructure photograph of the cross section of the Al-18Si-0.3Sb-0.6%Al-3P alloy sample in Example 3. DETAILED DESCRIPTION

[0021] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with specific embodiments.

[0022] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0023] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0024] Comparative Example 1:

[0025] Al-18Si hypereutectic aluminum-silicon alloy is melted and kept at 850℃ for 30 minutes, and then poured into a metal mold at room temperature. The specific operation steps are as follows:

[0026] Al-18Si hypereutectic aluminum-silicon alloy was melted in a pit-type resistance furnace using a graphite crucible at a melting temperature of 850°C.

[0027] After the alloy is completely melted, scrape off the surface scum, use hexachloroethane to refine, and keep warm for another 30 minutes. During the warming process, use a graphite rod to fully stir the melt to prevent uneven composition.

[0028] After the insulation is completed, the Al-18Si hypereutectic aluminum-silicon alloy melt is poured into a room temperature metal mold with an inner cavity size of φ12x120mm;

[0029] The sample was cut at a distance of 10 mm from the bottom, and the metallographic structure was prepared. The metallographic microscope was used to observe the microstructure of the alloy. The metallographic structure photo is shown in Figure 1 As shown. Figure 1 It can be seen that there are about 97 coarse primary silicon in the structure, most of which are in the form of flakes, regular polygons and elongated strips, and a small amount is in complex shapes; a large amount of α-Al phase is generated. The average size of primary silicon is 44.6μm, and the area of ​​primary silicon accounts for 10.1%.

[0030] Comparative Example 2:

[0031] 0.3wt.% Sb is added to the Al-18Si hypereutectic aluminum-silicon alloy, melted and kept at 850℃ for 30 minutes, and then poured into a metal mold at room temperature. The specific operation is as follows:

[0032] Al-18Si hypereutectic aluminum-silicon alloy was melted in a pit-type resistance furnace using a graphite crucible at a melting temperature of 850°C.

[0033] After the alloy is completely melted, 0.3wt.% Sb is added for microalloying treatment. After being fully fused, it is kept at 850℃ for 30 minutes.

[0034] After the heat preservation is completed, the antimony-containing Al-18Si hypereutectic aluminum-silicon alloy is poured into a room temperature metal mold with an inner cavity size of φ12x120mm;

[0035] The sample was cut at a distance of 10 mm from the bottom, and the metallographic structure was prepared. The metallographic microscope was used to observe the microstructure of the alloy. The metallographic structure photo is shown in Figure 2 As shown. Figure 1 Compared with the original structure, the number of primary silicon particles is reduced to 57, and the morphology is mostly regular polygons, with a few complex shapes, which is improved compared with the original structure. The average size of primary silicon in the alloy increases from 44.6μm to 50.6μm, but the area ratio of primary silicon decreases from 10.1% to 8.0%; the α-Al phase transformation is small but dense; the eutectic structure decreases.

[0036] Figure 2Microstructure photographs of the cross section of the Al-18Si-xSb alloy sample; (a) x=0; (b) x=0.15; (c) x=0.3; (d) x=0.45; (e) x=0.6; (f) x=0.75.

[0037] Table 1 Quantitative analysis results of primary silicon in the solidification structure of Al-18Si-xSb alloy

[0038]

[0039] The amount of Sb element added was 0.15wt.% as a gradient, and the Al-18Si hypereutectic aluminum-silicon alloy was modified by adding Sb element from 0.15wt.% to 0.75wt.%. The results in Table 1 were obtained. The area share and average size of primary silicon showed a trend of first decreasing and then increasing with the increase of Sb element content, and according to the solidification structure diagram, it can be seen that when the Sb content is too high (0.6wt.%, 0.75wt.%), the morphology of primary silicon changes to a complex radial shape. When the Sb element content is 0.3wt.%, both are the smallest, and the amount of antimony element added is selected to be 0.3wt.% of the total mass of the Al-18Si alloy.

[0040] Comparative Example 3:

[0041] 0.2wt.% Al-3P is added to the Al-18Si hypereutectic aluminum-silicon alloy, melted and kept at 850℃ for 30 minutes, and then poured into a metal mold at room temperature. The specific operation is as follows:

[0042] Al-18Si hypereutectic aluminum-silicon alloy was melted in a pit-type resistance furnace using a graphite crucible at a melting temperature of 850°C.

[0043] After the alloy is completely melted, scrape off the surface scum, use hexachloroethane to refine, and keep warm for 25 minutes; after the end of the heat preservation, add 0.2wt.% Al-3P, after fully fusion, keep warm for 5 minutes;

[0044] After the insulation is completed, the phosphorus modified Al-18Si hypereutectic aluminum-silicon alloy is poured into a room temperature metal mold with an inner cavity size of φ12x120mm;

[0045] The sample was cut at a distance of 10 mm from the bottom, and the metallographic structure was prepared. The metallographic microscope was used to observe the microstructure of the alloy. The metallographic structure photo is shown in Figure 3 As shown. Figure 3It can be seen that in the solidification structure of the alloy after 0.2% Al-3P modification, the average size of primary silicon decreases slightly, with an average size of 40.1μm, and the number of particles increases to 119, and the overall proportion increases to 12.2%; the morphology is mainly composed of a large number of thin strips and polygons, with a small amount of petal-shaped; the amount of α-Al phase decreases and becomes short rod-shaped; the eutectic structure increases and is fine and fibrous.

[0046] Comparative Example 4:

[0047] 0.4wt.% Al-3P is added to the Al-18Si hypereutectic aluminum-silicon alloy, melted and kept at 850℃ for 30 minutes, and then poured into a metal mold at room temperature. The specific operation is as follows:

[0048] Al-18Si hypereutectic aluminum-silicon alloy was melted in a pit-type resistance furnace using a graphite crucible at a melting temperature of 850°C.

[0049] After the alloy is completely melted, scrape off the surface scum, refine with hexachloroethane, and keep warm for 25 minutes; after the heat preservation, add 0.4wt.% Al-3P, and keep warm for 5 minutes after it is fully fused;

[0050] After the insulation is completed, the phosphorus modified Al-18Si hypereutectic aluminum-silicon alloy is poured into a room temperature metal mold with an inner cavity size of φ12x120mm;

[0051] The sample was cut at a distance of 10 mm from the bottom, and the metallographic structure was prepared. The metallographic microscope was used to observe the microstructure of the alloy. The metallographic structure photo is shown in Figure 4 shown. Figure 4 and Figure 1 , Figure 2 and Figure 3 In comparison, the primary silicon is refined and increased to 230 particles, with an average size of 29.2μm, an area share of 11.6%, and a morphology dominated by regular polygons; the α-Al phase is concentrated near the primary silicon and precipitates in the form of short rod particles; the eutectic structure is fine.

[0052] Comparative Example 5:

[0053] 0.6wt.% Al-3P is added to the Al-18Si hypereutectic aluminum-silicon alloy, melted and kept at 850℃ for 30 minutes, and then poured into a metal mold at room temperature. The specific operation is as follows:

[0054] Al-18Si hypereutectic aluminum-silicon alloy was melted in a pit-type resistance furnace using a graphite crucible at a melting temperature of 850°C.

[0055] After the alloy is completely melted, scrape off the surface scum, refine with hexachloroethane, and keep warm for 25 minutes; after the heat preservation, add 0.6wt.% Al-3P, and keep warm for 5 minutes after it is fully fused;

[0056] After the insulation is completed, the phosphorus modified Al-18Si hypereutectic aluminum-silicon alloy is poured into a room temperature metal mold with an inner cavity size of φ12x120mm;

[0057] The sample was cut at a distance of 10 mm from the bottom, and the metallographic structure was prepared. The metallographic microscope was used to observe the microstructure of the alloy. The metallographic structure photo is shown in Figure 5 shown.

[0058] and Figure 3 Compared with 0.4% Al-3P, the modification effect of adding 0.6% Al-3P is worse, but Figure 1 , Figure 2 , Figure 3 Compared with the original, the modification effect is still better. The primary silicon begins to grow larger, with 142 primary silicon particles, with an average size of 32.2μm and an area share of 10.8%; the α-Al phase changes to short-rod dendrites; and the eutectic structure is fine.

[0059] Embodiment 1:

[0060] The Al-18Si hypereutectic aluminum-silicon alloy was treated by adding trace element antimony and modifier phosphorus alloy. After the Al-18Si hypereutectic aluminum-silicon alloy was kept at 850°C for 30 minutes, it was poured into a room temperature metal mold. The specific operation steps are as follows:

[0061] Al-18Si hypereutectic aluminum-silicon alloy was melted in a pit-type resistance furnace using a graphite crucible at a melting temperature of 850°C.

[0062] After the alloy is completely melted, 0.3wt.% Sb is added for microalloying treatment. After being fully fused, the alloy is kept at 850°C for 25 minutes. After the heat preservation, 0.2wt.% Al-3P is added. After being fully fused, the alloy is kept at 850°C for 25 minutes.

[0063] After the heat preservation is completed, the antimony-containing Al-18Si hypereutectic aluminum-silicon alloy is poured into a room temperature metal mold with an inner cavity size of φ12x120mm;

[0064] The sample was cut at a distance of 10 mm from the bottom, and the metallographic structure was prepared. The metallographic microscope was used to observe the microstructure of the alloy. The metallographic structure photo is shown in Figure 6 As shown. Figure 3 In contrast, adding 0.3% Sb Figure 6 The number of primary silicon particles in the alloy increases to 126. Compared with the alloy with phosphorus added alone, the number of primary silicon particles increases slightly, and the size decreases slightly, with an average size of 36.9 μm, but the area share decreases significantly to 7.7%. The morphology of primary silicon is mainly regular plates, without complex shapes, but with extremely small particles. The α-Al phase precipitates around the primary silicon phase in the form of short rod dendrites. The eutectic structure is fine.

[0065] Embodiment 2:

[0066] The Al-18Si hypereutectic aluminum-silicon alloy is treated by adding trace element antimony and modifier phosphorus alloy. After the Al-18Si hypereutectic aluminum-silicon alloy is kept at 850℃ for 30 minutes, it is poured into a room temperature metal mold. The specific operation steps are as follows:

[0067] Al-18Si hypereutectic aluminum-silicon alloy was melted in a pit-type resistance furnace using a graphite crucible at a melting temperature of 850°C.

[0068] After the alloy is completely melted, 0.3wt.% Sb is added for microalloying treatment. After being fully fused, the alloy is kept at 850°C for 25 minutes. After the heat preservation, 0.4wt.% Al-3P is added. After being fully fused, the alloy is kept at 850°C for 25 minutes.

[0069] After the heat preservation is completed, the antimony-containing Al-18Si hypereutectic aluminum-silicon alloy is poured into a room temperature metal mold with an inner cavity size of φ12x120mm;

[0070] The sample was cut at a distance of 10 mm from the bottom, and the metallographic structure was prepared. The metallographic microscope was used to observe the microstructure of the alloy. The metallographic structure photo is shown in Figure 7 shown.

[0071] When Al-3P alloy was not added to Comparative Example 2, the Sb element eliminated the non-spontaneous nucleation base in the hypereutectic aluminum-silicon alloy, and the phenomenon of "reduced number of nuclei and increased average size" occurred; after the Al-3P alloy was added to Example 2, a large amount of AlP was generated in the melt, and AlP was the core of heterogeneous nucleation. The addition of the Sb element increased the supercooling and reduced the critical size of nucleation, resulting in more particles meeting the nucleation conditions. An obvious silicon-poor phenomenon appeared around, thereby inhibiting the growth of primary silicon. Sb and Al-3P played a synergistic role. After the Sb element was added, the morphology, quantity and proportion of primary silicon were improved.

[0072] and Figure 4 Compared with the addition of 0.3% Sb Figure 7 The primary silicon is smaller and more uniform, with an average size of 19.5μm. The number of particles increases to 370, but the area share decreases to 8.4%; the primary silicon is mostly regular polygonal in shape, and some are pentagonal in shape; the α-Al phase is distributed near the primary silicon and the number increases; the eutectic structure is finer.

[0073] When Al-3P is used for modification, AlP is generated. During the solidification process, AlP becomes the nucleation base of primary silicon, refining the primary silicon; and the morphology of primary silicon is relatively uniform, which is a regular polyhedron with smooth edges and corners and an increased number, but the size is small, averaging about 30μm, but the distribution is not uniform. After adding Sb, the Sb element increases the supercooling of Al-18Si and reduces the critical size of the nucleation particles. Therefore, more particles meet the nucleation conditions, the number of primary silicon increases, and the silicon concentration in the surrounding matrix decreases. Therefore, the growth of primary silicon is restricted and the size becomes smaller; the reduction in silicon concentration promotes the growth of α-Al phase, thereby increasing the α-Al phase.

[0074] The tiny and rounded primary silicon phase greatly improves the performance of hypereutectic aluminum-silicon alloy and is of great value in expanding its application prospects.

[0075] Embodiment 3:

[0076] The Al-18Si hypereutectic aluminum-silicon alloy is treated by adding trace element antimony and modifier phosphorus alloy. After the Al-18Si hypereutectic aluminum-silicon alloy is kept at 850℃ for 30 minutes, it is poured into a room temperature metal mold. The specific operation steps are as follows:

[0077] Al-18Si hypereutectic aluminum-silicon alloy was melted in a pit-type resistance furnace using a graphite crucible at a melting temperature of 850°C.

[0078] After the alloy is completely melted, 0.3wt.% Sb is added for microalloying treatment. After being fully fused, the alloy is kept at 850°C for 25 minutes. After the heat preservation, 0.6wt.% Al-3P is added. After being fully fused, the alloy is kept at 850°C for 25 minutes.

[0079] After the heat preservation is completed, the antimony-containing Al-18Si hypereutectic aluminum-silicon alloy is poured into a room temperature metal mold with an inner cavity size of φ12x120mm;

[0080] The sample was cut at a distance of 10 mm from the bottom, and the metallographic structure was prepared. The metallographic microscope was used to observe the microstructure of the alloy. The metallographic structure photo is shown in Figure 8 Compared with Al-18Si ( Figure 5 ), in the microstructure of Al-18Si with 0.6% Al-3P and 0.3% Sb added, the primary silicon is finer and has more particles, which are 293, with an average size of 26.8μm and an area share of 8.9%; the morphology is basically regular polygonal plate-like without complex shape; the distribution is more uniform; α-Al increases to a certain extent; and the eutectic structure is fine.

[0081] As shown in the above figure, the addition of Sb and Al-3P can inhibit the growth of primary silicon in hypereutectic aluminum-silicon alloy. Under the condition of Sb addition of 0.3%, the best effect is achieved when Al-3P addition reaches 0.4%. The average size of primary silicon is refined from 44.553μm before modification to 19.519μm, and when only Al-3P is modified, although the size of primary silicon is reduced, the area share increases; when Al-3P is lower than 0.4%, although the area fraction of primary silicon is reduced, its average size changes little, and the morphology becomes more complex; when the content is higher than 0.4%, the average size and area fraction of primary silicon are greater than the modification result of 0.4% Al-3P, and the effect is reduced.

[0082] The present invention adopts trace antimony and trace phosphorus alloy to carry out composite modification treatment on Al-18Si alloy. By adding trace phosphorus alloy, the nucleation particles in the Al-18Si alloy are increased to promote heterogeneous nucleation. Then, the trace element Sb is added to increase the supercooling degree of the Al-18Si alloy, reduce the critical size of nucleation, and enable a large number of nuclei to be formed during solidification, thereby reducing the silicon concentration in the matrix, inhibiting the growth of primary silicon, and thus refining the primary silicon phase.

[0083] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for refining primary silicon in Al-18Si alloy and reducing the area fraction of primary silicon by antimony alloying and phosphorus modification, characterized in that: The Al-18Si hypereutectic aluminum-silicon alloy is melted, and pure antimony is added to the alloy liquid after the alloy is completely melted and kept warm, and then Al-3P master alloy is added for modification treatment. After keeping warm, the alloy liquid is poured into a room temperature metal mold for molding; the amount of the Al-3P master alloy added is 0.2wt.%~0.6wt.% of the mass of the Al-18Si hypereutectic aluminum-silicon alloy; the amount of antimony added is 0.3wt.% of the total mass of the Al-18Si hypereutectic aluminum-silicon alloy.

2. The method for refining primary silicon and reducing the area fraction of primary silicon in Al-18Si alloy by antimony alloying and phosphorus modification as claimed in claim 1, characterized in that: The amount of Al-3P master alloy added is 0.4 wt.% of the mass of Al-18Si hypereutectic aluminum-silicon alloy.

3. The method for refining primary silicon and reducing the area fraction of primary silicon in Al-18Si alloy by antimony alloying and phosphorus modification as claimed in claim 1, characterized in that: The melting temperature of Al-18Si hypereutectic aluminum-silicon alloy is 850℃.