Micro-nano topological structure PLLA ultrafine fiber material, preparation method and application
PLLA ultrafine fibers with a fish scale-like micro-nano topology are formed through electrospinning and acetone solution dipping, which solves the problems of difficult operation and cell growth control in the existing technology, and achieves effective control and preparation of nerve cell growth. simplification.
Patent Information
- Application Number
- CN202211529984.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-11-30
AI Technical Summary
Existing electrospun porous fiber preparation methods are difficult to operate, costly and difficult to effectively regulate cell growth, especially the lack of effective physical signal induction for nerve cell growth.
By stirring PLLA and PEO in TFE at room temperature and then electrospinning, highly oriented fibers are obtained. After vacuum drying, they are impregnated with an acetone solution to form a PLLA ultrafine fiber material with a fish scale-like micro-nano secondary topology and control the topology. structure to regulate nerve cell growth.
It achieves effective regulation of nerve cell growth. Low topology can inhibit growth, while high topology can promote growth. It also simplifies the preparation process and is suitable for industrial production.
Smart Images

Figure CN116065256B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of biomaterial preparation, and in particular relates to a micro-nano topological structure PLLA ultrafine fiber material, a preparation method and an application thereof. Background Art
[0002] Polylactic acid is a non-toxic, biodegradable, highly plastic polymer material. Its monomer raw material L-lactic acid is an endogenous active substance in the human body. Polylactic acid products are non-toxic to the human body, are not rejected and can be absorbed by the human body. They can be made into medical tissue skeleton materials and pharmaceutical carriers and can be safely used in the human body. They have obtained US FDA certification and can be degraded into carbon dioxide and water after 6-12 months when buried in the soil.
[0003] Electrospinning is a cutting-edge technology that uses a high-voltage electric field to control the deposition of polymers on a receiver to make tissue engineering materials. Usually, the solvents used in electrospinning are highly volatile. This technology allows the polylactic acid solution to spiral in an electric field at a very high speed. During this process, the solvent evaporates rapidly, and the remaining polymer is stretched into very fine fibers, and finally collected on the receiver in the form of nano-micron-scale fibers. Electrospinning polylactic acid fiber materials are mainly used in the field of tissue regeneration scaffolds. Electrospinning can make the scaffold material have a nano-scale structure, change the physical and chemical properties of the scaffold, and promote the adhesion, proliferation and gene expression of tissue cells, thereby achieving the purpose of promoting tissue regeneration and repair. At present, many studies have achieved the goal of promoting cell adhesion, proliferation and migration by changing the surface topology of the fiber scaffold, so as to better promote tissue cell growth and tissue wound healing (Adv. Funct. Mater. 2020, 30, 2002031; Appl. Mater. Today. 2020, 18, 100468). Electrospinning with highly volatile solvents is the most commonly used method for preparing porous nanofibers. At the same time, the preparation of electrospun porous fibers is also closely related to the properties of the solution, spinning parameters and environmental conditions. The main methods currently used have the disadvantages of high technical requirements, high operating difficulty and high cost consumption. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a micro-nano topological structure oriented PLLA ultrafine fiber, a preparation method and an application. The preparation method provided by the present invention is simple, and the prepared micro-nano topological structure oriented PLLA ultrafine fiber has a secondary topological polylactic acid ultrafine fiber that combines oriented microtopology and fiber surface nanotopology, which can regulate the growth of nerve cells.
[0005] The present invention provides the following technical solutions:
[0006] A method for preparing a micro-nano topological structure PLLA ultrafine fiber material comprises the following steps:
[0007] S1. PLLA and PEO were added to TFE, stirred at room temperature until completely dissolved, and then electrospun to obtain highly oriented PLLA ultrafine fibers;
[0008] S2. The oriented PLLA ultrafine fibers are vacuum dried and then immersed in an acetone solution to obtain a PLLA ultrafine fiber material with a micro-nano topological structure, wherein the micro-nano topological structure is a fish scale-like micro-nano secondary topological structure.
[0009] Furthermore, in step S1, the usage ratio of PLLA, PEO and TFE is 0.45 g:0.05 g:10 mL.
[0010] Furthermore, the electrospinning conditions are: injection speed of 0.5 ml / h, voltage of 6-7 kV, and receiving drum speed of 2000 r / min.
[0011] Furthermore, in step S2, the vacuum drying treatment is specifically: vacuum drying in a vacuum drying oven for 48 to 72 hours.
[0012] Furthermore, in step S2, the immersion in the acetone solution is performed for 10-30 minutes.
[0013] Furthermore, the immersion time in the acetone solution is 10 minutes, and the obtained micro-nano topological structure PLLA ultrafine fiber material has a low-degree micro-nano topological structure.
[0014] Furthermore, in step S2, the immersion in the acetone solution is treated for 20-30 minutes, and the obtained micro-nano topological structure PLLA ultrafine fiber material has a high degree of micro-nano topological structure.
[0015] The present invention also provides a PLLA ultrafine fiber material with a micro-nano topological structure prepared by the above-mentioned preparation method.
[0016] The present invention also provides a medical material for regulating the growth of nerve cells. The medical material is a PLLA ultrafine fiber material with a micro-nano topological structure. The micro-nano topological structure is a fish scale-like micro-nano secondary topological structure. The micro-nano topological structure is used to regulate the growth of nerve cells.
[0017] Furthermore, the regulation of nerve cell growth is inhibition of nerve cell growth, and the PLLA ultrafine fiber material with micro-nano topological structure orientation is a low-degree micro-nano topological structure prepared by the above preparation method.
[0018] Furthermore, the regulation of nerve cell growth is to promote nerve cell growth, and the PLLA ultrafine fiber material with micro-nano topological structure orientation is a high-degree micro-nano topological structure prepared by the above preparation method.
[0019] Compared with the prior art, the present invention has the following technical effects:
[0020] (1) The present invention controls the viscosity of the PLLA solution, the injection speed and the receiver rotation speed to obtain highly oriented PLLA ultrafine fibers, and then uses an acetone solution for immersion treatment to obtain a PLLA ultrafine fiber material with a fish scale-like secondary topological structure. The PLLA ultrafine fiber material has a physical signal inducing effect on the growth of nerve cells. When the topological degree of the micro-nano topological structure is low, the growth of nerve cells can be inhibited. When the topological degree of the micro-nano topological structure is high, the growth of nerve cells can be promoted.
[0021] (2) The preparation method provided by the present invention is simple, convenient and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The scanning electron microscope images are of the highly oriented PLLA ultrafine fiber A obtained in Example 1 of the present invention and the micro-nano topological structure PLLA ultrafine fiber material BD obtained in Example 2;
[0023] Figure 2 Immunofluorescence images of neurofilaments in dorsal root ganglia after three days of culture on the material;
[0024] Figure 3 This is a statistical chart obtained by quantitatively analyzing the extension distance of dorsal root ganglion neurofilaments on different materials. DETAILED DESCRIPTION
[0025] The present invention will be further explained below in conjunction with the embodiments and drawings. The following embodiments are only used to illustrate the present invention but are not intended to limit the scope of implementation of the present invention.
[0026] Example 1
[0027] S1. At room temperature, add 0.45 g PLLA (poly(L-lactic acid)) and 0.05 g PEO (polyethylene oxide Mr = 5000 kDa) into 10 ml TFE (trifluoroethanol), and stir to dissolve at room temperature overnight to obtain a PLLA solution.
[0028] S2. Using a high-voltage electrospinning device, the pushing rate of the PLLA solution was controlled to be 0.5 ml / h, the voltage was 7 Kv, the drum speed was 2000 r / min, and the fiber membrane was received by a high-speed rotating drum wrapped with aluminum foil. The collected fiber membrane was placed in a vacuum drying oven and dried for 48 hours to obtain highly oriented PLLA ultrafine fibers A. The electron microscope image is shown in FIG. Figure 1As shown in A, it can be seen that the surface of highly oriented PLLA ultrafine fiber A is smooth.
[0029] Example 2
[0030] The highly oriented PLLA ultrafine fiber A prepared in Example 1 was cut into a 2 cm × 2 cm film, fixed with a stainless steel clip, and then immersed in an acetone solution for 10 min, 20 min and 30 min, respectively, to obtain a micro-nano topological structure PLLA ultrafine fiber material BD. The electron microscope image is shown in FIG. Figure 1 B. Figure 1 C. Figure 1 As shown in D, it can be found that after acetone treatment, fish-scale micro-nano secondary structures of varying degrees are produced on the fiber surface. This is because the non-solvent (acetone) quickly diffuses into the fiber, inducing recrystallization inside the fiber. Figure 1 AC can find that with the extension of acetone treatment time, the topological degree of the obtained micro-nano topological structure PLLA ultrafine fiber material gradually deepens with recrystallization.
[0031] Test Example 1
[0032] The dorsal root ganglion of one-day-old SD rats was inoculated into the above materials and cultured for three days. Immunofluorescence staining was performed to observe the growth of the dorsal root ganglion and to count the length of the neurofilaments. The immunofluorescence image of the dorsal root ganglion is shown in the figure. Figure 2 As shown in the figure, the statistical diagram of the extension length of dorsal root ganglion neurofilaments is shown in Figure 3 shown.
[0033] according to Figure 2 , Figure 3 It can be found that compared with the ultrafine fibers with smooth surfaces, the oriented ultrafine fibers treated with acetone for 10 minutes have an inhibitory effect on the extension of ganglia, and the oriented ultrafine fibers treated with acetone for 20 and 30 minutes can effectively promote the extension of neurofilaments. It can be seen that low-topology oriented fibers will inhibit the extension of neurofilaments compared with smooth oriented fibers, and high-topology oriented fibers will promote the extension of neurofilaments compared with smooth oriented fibers. This may be because the "contact guidance" method of this fish-scale micro-nano secondary structure affects the morphology of nerve cells, thereby changing the working mode of the genetic material in the cell, thereby regulating the growth of neurofilaments.
Claims
1. A method for preparing a micro-nano topological structure PLLA ultrafine fiber material, characterized in that: The following steps are involved: S1. Add PLLA and PEO to TFE, stir at room temperature until completely dissolved, and then electrospin to obtain highly oriented PLLA ultrafine fibers; the TFE is trifluoroethanol; S2. The highly oriented PLLA ultrafine fibers are vacuum dried and then immersed in an acetone solution to obtain a PLLA ultrafine fiber material with a micro-nano topological structure, wherein the micro-nano topological structure is a fish scale-like micro-nano secondary topological structure.
2. The preparation method according to claim 1, characterized in that: In step S1, the usage ratio of PLLA, PEO and TFE is 0.45 g:0.05 g:10 mL.
3. The preparation method according to claim 1, characterized in that: The electrospinning conditions are as follows: injection speed of 0.5 ml / h, voltage of 6-7 kV, and receiving drum speed of 2000 r / min.
4. The preparation method according to claim 1, characterized in that: In step S2, the immersion in the acetone solution is performed for 10-30 min.
5. The preparation method according to claim 1, characterized in that: In step S2, the immersion in the acetone solution is performed for 10 minutes.
6. The preparation method according to claim 1, characterized in that: In step S2, the immersion in the acetone solution is performed for 20-30 minutes.
7. The micro-nano topological structure PLLA ultrafine fiber material prepared by the preparation method according to any one of claims 1 to 6.
8. A medical material for regulating the growth of nerve cells, characterized in that: The medical material is a PLLA ultrafine fiber material with a micro-nano topological structure orientation, which is prepared by the preparation method described in claim 5. The micro-nano topological structure is a fish scale-like micro-nano secondary topological structure, and the regulation of nerve cell growth is the inhibition of nerve cell growth.
9. A medical material for regulating the growth of nerve cells, characterized in that: The medical material is a PLLA ultrafine fiber material with a micro-nano topological structure orientation, which is prepared by the preparation method described in claim 6. The micro-nano topological structure is a fish scale-like micro-nano secondary topological structure, and the regulation of nerve cell growth is to promote nerve cell growth.