A method for improving the slip line of silicon epitaxial wafer
Through the two-step heating program and temperature compensation technology, the problem of slip lines in silicon epitaxial wafers is solved, and the surface quality of the epitaxial layer is effectively controlled and the production capacity is improved. It is suitable for silicon epitaxial wafers and equipment of different specifications.
Patent Information
- Application Number
- CN202310184893.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-02-17
AI Technical Summary
Existing technologies are difficult to effectively reduce or eliminate silicon epitaxial wafer slip lines, resulting in increased device noise, increased leakage current, soft breakdown and other problems. Moreover, existing methods have a long optimization design cycle or low production capacity, making it difficult to promote in industrial production.
Using a two-step heating program, the resistivity test of the silicon wafer is performed, the temperature difference is calculated and temperature compensation is performed to reduce the temperature gradient between the center and edge of the silicon wafer, release thermal stress, control the surface quality of the epitaxial layer, and improve process quality and productivity.
It effectively controls the generation of slip lines, improves the surface quality of the epitaxial layer, and enhances the yield. It is efficient, universal and simple, and is suitable for silicon epitaxial wafers and epitaxial equipment of different specifications.
Smart Images

Figure CN116072524B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicon epitaxial control methods, and in particular relates to a method for improving a slip line of a silicon epitaxial wafer. Background Art
[0002] Since the doping process of silicon epitaxial wafers is flexible, parameters such as thickness and resistivity are easy to adjust, and can significantly change the reverse durability, cutoff frequency and other characteristics of the device, they are widely used in power devices (MOSFET, transistors, etc.), analog devices (CIS, PMIC) and other semiconductor devices with high requirements for stability, defect density, high voltage and current tolerance.
[0003] With the urgent demand for high-quality devices, the quality requirements for the epitaxial layer as the substrate are becoming more and more stringent. Once the epitaxial layer has defects such as stacking faults, dislocations, slip lines and fog defects, it will cause problems such as increased device noise, increased leakage current, soft breakdown, low breakdown, etc., which will lead to device failure and reduced yield. Among them, slip lines are generated under process conditions where the superimposed stress value of its mechanical stress and thermal stress exceeds the critical stress value of lattice slip caused by the growth temperature. Therefore, the thermal stress generated by the radial temperature difference in the wafer during the epitaxial growth and temperature rise and fall process becomes the main factor in the generation of slip lines. With the improvement of edge polishing process technology, the existence of slip lines significantly reduces the mechanical stress of the substrate.
[0004] Therefore, there is an urgent need to develop a simple, efficient, and universal process that can improve the production efficiency of epitaxial wafers while reducing or eliminating slip lines. Summary of the invention
[0005] The present invention is based on the inventor's discovery and understanding of the following facts and problems:
[0006] There are several methods to reduce the temperature gradient within the chip, reduce thermal stress, and thus reduce or eliminate slip lines. From the perspective of hardware design, methods such as concave spherical bearing grooves and designed groove depth are used to reduce the gap between the substrate edge and the base caused by warping, reduce the temperature gradient between the center and the edge of the silicon wafer, and thus reduce thermal stress within the chip and improve the surface quality of the epitaxial layer. However, this method has a long optimization design cycle. From the perspective of process design, methods such as compensating the edge temperature of the substrate and controlling the heating and cooling rate are used to achieve uniform temperature control at each point in the chip, thereby effectively controlling the generation of slip lines. However, although too low a heating and cooling rate can effectively improve the surface quality of the epitaxial layer, it is accompanied by the problem of low production capacity and is difficult to promote and apply in industrial production.
[0007] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, an embodiment of the present invention proposes a method for improving the slip line of a silicon epitaxial wafer, which can reduce the temperature gradient between the center and the edge of the silicon wafer through a two-step heating procedure, release potential thermal stress, achieve the regulation of the surface quality of the epitaxial layer, and improve the process quality and production capacity.
[0008] A method for improving a slip line of a silicon epitaxial wafer according to an embodiment of the present invention comprises the following steps:
[0009] (1) placing the temperature control sheet into a cleaned epitaxial furnace reaction chamber for constant temperature baking, performing a resistivity test on the temperature control sheet obtained after constant temperature baking, obtaining the temperature distribution of each area of the temperature control sheet, and calculating the temperature difference between the front, rear, side and center areas of the temperature control sheet;
[0010] (2) Loading the silicon wafer into the reaction chamber of the epitaxial furnace after cleaning, raising the temperature to the growth temperature by a two-step heating program and simultaneously performing temperature compensation according to the temperature difference described in step (1), then introducing silicon source, hydrogen and dopant, epitaxially growing to the target thickness and target resistivity, and cooling the obtained silicon epitaxial wafer and taking it out.
[0011] The advantages and technical effects brought by the method for improving the slip line of silicon epitaxial wafers according to the embodiment of the present invention are as follows: 1. The method according to the embodiment of the present invention can clearly obtain the actual temperature of the silicon wafer surface during the epitaxial process by testing the resistivity of the temperature control sheet that has been baked at a constant temperature to obtain the temperature distribution of each area, and can perform temperature compensation for each temperature zone of the epitaxial furnace reaction chamber, effectively control the temperature distribution of the silicon wafer surface during the epitaxial process, thereby better controlling the generation of slip lines and realizing the regulation of the surface quality of the epitaxial layer; 2. The method according to the embodiment of the present invention adopts a two-step heating program for heating, reduces the temperature gradient between the center and the edge of the silicon wafer, and then gradually releases the thermal stress generated, suppresses the probability of defect generation in the epitaxial layer, and improves the yield; 3. The method according to the embodiment of the present invention adopts a controllable two-step heating program for heating, and has better production capacity while ensuring the surface quality of the epitaxial layer; 4. The method according to the embodiment of the present invention has high universality, high efficiency, and simplicity, and is suitable for improving the slip lines of silicon epitaxial wafers of different specifications and epitaxial equipment of different types.
[0012] In some embodiments, in step (1) and / or step (2), the cleaning process is to heat the epitaxial furnace reaction chamber to the etching temperature, use hydrogen chloride and hydrogen to etch and clean the graphite components of the reaction chamber, close the hydrogen chloride pipeline, increase the hydrogen flow rate for purging, and then cool the epitaxial furnace reaction chamber to the wafer feeding temperature.
[0013] In some embodiments, in step (1), the flow rate of hydrogen chloride is 15-25 SLM, and the flow rate of hydrogen is 10-100 SLM; and / or, in step (1), the etching temperature is 1100-1200°C, and the wafer feeding temperature is 400-800°C.
[0014] In some embodiments, in step (1), the thickness of the temperature control sheet is 600-650 μm, and the resistivity is 8-20 Ω·cm; the temperature control sheet is boron-doped <100> Ion implantation into silicon wafers.
[0015] In some embodiments, in step (1), the baking temperature is 1100-1200° C., and the constant temperature baking time is 20-180 seconds.
[0016] In some embodiments, in step (1), the resistivity test is performed using a four-probe resistance tester.
[0017] In some embodiments, in step (2), the two-step heating program is to first increase the temperature to 900-1050°C at a heating rate of 10-15°C / s, and the heating time is 7-65s, and then increase the temperature to 1150°C at a heating rate of 2°C / s, and the heating time is 50-125s.
[0018] In some embodiments, in step (2), the silicon source is trichlorosilane, and the dopant includes at least one of BH3, PH3, and AsH3.
[0019] In some embodiments, in step (2), the flow rate of hydrogen is 60-90 SLM, and the rate of epitaxial growth is 1-5 μm / min.
[0020] In some embodiments, in step (2), the cooling temperature is 890° C. and the cooling rate is 2 to 15° C. / s. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is the resistance mapping diagram of the temperature control sheet 4PP after temperature compensation in Example 1;
[0022] Figure 2 is the slip line distribution diagram of the epitaxial layer obtained by the two-step heating procedure in Example 1;
[0023] Figure 3 is the slip line distribution diagram of the epitaxial layer obtained by the two-step heating procedure in Example 2;
[0024] Figure 4 is the distribution diagram of the slip lines of the epitaxial layer obtained by the two-step heating procedure in Example 3;
[0025] Figure 5 This is the slip line distribution diagram of the epitaxial layer obtained by the one-step heating procedure in Comparative Example 1;
[0026] Figure 6 This is the slip line distribution diagram of the epitaxial layer obtained by non-gradient heating in Comparative Example 2;
[0027] Figure 7 This is the slip line distribution diagram of the epitaxial layer obtained by two-step programmed heating in Example 3. DETAILED DESCRIPTION
[0028] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.
[0029] A method for improving a slip line of a silicon epitaxial wafer according to an embodiment of the present invention comprises the following steps:
[0030] (1) placing the temperature control sheet into a cleaned epitaxial furnace reaction chamber for constant temperature baking, performing a resistivity test on the temperature control sheet obtained after constant temperature baking, obtaining the temperature distribution of each area of the temperature control sheet, and calculating the temperature difference between the front, rear, side and center areas of the temperature control sheet;
[0031] (2) Loading the silicon wafer into the reaction chamber of the epitaxial furnace after cleaning, raising the temperature to the growth temperature by a two-step heating program and simultaneously performing temperature compensation according to the temperature difference described in step (1), then introducing silicon source, hydrogen and dopant, epitaxially growing to the target thickness and target resistivity, and cooling the obtained silicon epitaxial wafer and taking it out.
[0032] The method for releasing thermal stress and improving slip lines in the embodiment of the present invention can clearly obtain the actual temperature of the silicon wafer surface during the epitaxial process by performing resistivity testing on the temperature control sheet that has been baked at a constant temperature to obtain the temperature distribution of each area, and can perform temperature compensation on each temperature zone of the epitaxial furnace reaction chamber to effectively control the temperature distribution of the silicon wafer surface during the epitaxial process, thereby better controlling the generation of slip lines and realizing the regulation of the surface quality of the epitaxial layer; a two-step heating program is used for heating to reduce the temperature gradient between the center and the edge of the silicon wafer, thereby gradually releasing the thermal stress generated, suppressing the probability of defect generation in the epitaxial layer, and improving the yield; a controllable two-step heating program is used for heating to ensure the surface quality of the epitaxial layer while having better production capacity; it has high universality, efficiency, and simplicity, and is suitable for improving slip lines of silicon epitaxial wafers of different specifications and different types of epitaxial equipment.
[0033] In some embodiments, preferably, in step (1) and / or step (2), the cleaning treatment is to heat the epitaxial furnace reaction chamber to the etching temperature, use hydrogen chloride and hydrogen to etch and clean the graphite components of the reaction chamber, close the hydrogen chloride pipeline, increase the hydrogen flow rate for purging, and then cool the epitaxial furnace reaction chamber to the wafer feeding temperature. Further preferably, in step (1), the flow rate of hydrogen chloride is 15-25SLM, and the flow rate of hydrogen is 10-100SLM; and / or, in step (1), the etching temperature is 1100-1200°C, and the wafer feeding temperature is 400-800°C. More preferably, the etching temperature is 1170°C, and the wafer feeding temperature is 750°C.
[0034] In the embodiment of the present invention, the reaction chamber is etched, cleaned and purged by high-flow hydrogen chloride and hydrogen, so that the reaction chamber can be deeply cleaned and impurities in the equipment can be removed to ensure the quality of the epitaxial wafer and reduce the probability of defects.
[0035] In some embodiments, preferably, in step (1), the thickness of the temperature control sheet is 600-650 μm, and the resistivity is 8-20 Ω·cm; the temperature control sheet is boron-doped <100> Preferably, the temperature control chip uses an ion implantation process to implant boron ions into the silicon wafer. <100> It is prepared from silicon wafers with a certain crystal orientation.
[0036] In some embodiments, preferably, in the step (1), the baking temperature is 1100-1200°C, and the constant temperature baking time is 20-180s. Further preferably, the temperature of the reaction chamber is raised to the baking temperature at a heating rate of 10-20°C / s. More preferably, the constant temperature baking is carried out in a hydrogen atmosphere, and the flow rate of the hydrogen is 60SLM. More preferably, the heating rate is 15°C / s, and the baking temperature is 1130°C.
[0037] In some embodiments, preferably, in step (1), the resistivity test is performed using a four-probe resistance tester. Further preferably, in step (1), the specific steps of temperature compensation for each temperature zone are: testing the resistivity of the five areas of the center, front, back, left, and right of the temperature control plate respectively, calculating the average resistivity difference between the four areas of the front, back, left, and right and the center area, and obtaining the temperature difference between the four areas of the front, back, left, and right and the center area through the relationship between resistivity and temperature: Δρ = -1.8 × ΔT.
[0038] In an embodiment of the present invention, the resistivity of the temperature control sheet is tested by a four-probe resistance tester, and the temperature of each temperature zone is compensated according to the linear relationship between resistivity and temperature. The actual temperature of the silicon wafer surface during the epitaxial process can be clearly obtained, and the temperature distribution of the silicon wafer surface during the epitaxial process can be effectively controlled, thereby better controlling the generation of slip lines and achieving regulation of the surface quality of the epitaxial layer.
[0039] In some embodiments, preferably, in step (2), the two-step heating program is to first increase the temperature to 900-1050°C at a heating rate of 10-15°C / s, and the heating time is 7-65s, and then increase the temperature to 1150°C at a heating rate of 2°C / s, and the heating time is 50-125s.
[0040] In the embodiment of the present invention, the specific operation process of the two-step heating program is preferably selected, firstly the temperature is raised to below 1050°C at a relatively fast heating rate, and then the temperature is raised to 1150°C at a relatively slow heating rate. This heating step can not only fully release the thermal stress in the growth process of the epitaxial wafer, reduce the probability of epitaxial layer defect generation, and improve the yield; but also compared with the prior art of raising the temperature to a certain temperature and performing constant temperature treatment to release thermal stress, this heating method has higher production efficiency.
[0041] In some embodiments, preferably, in step (2), the silicon source is trichlorosilane (TCS), and the dopant includes at least one of BH3, PH3, and AsH3. Further preferably, in step (2), the flow rate of hydrogen is 60 to 90 SLM, and the rate of epitaxial growth is 1 to 5 μm / min. More preferably, the target thickness is 1 to 100 μm, and the target resistivity is 0.1 to 5 Ω·cm. More preferably, under the conditions of a certain growth rate and silicon source flow rate, the dopant flow rate is controlled by Iterate the calculation until the surface resistivity of the silicon epitaxial layer meets the requirements; (now) Indicates the content of dopant injected, Dop (target) Indicates the target content of implanted dopants, Res (now) Indicates the current resistivity, Res (target) Indicates the target resistivity.
[0042] In the embodiment of the present invention, by adding BH3, PH3, AsH3 gas phase dopants during the epitaxial process, the doping concentration in the epitaxial layer can be controlled, thereby changing the electrical properties of the epitaxial layer.
[0043] In some embodiments, preferably, in the step (2), the cooling temperature is 890° C., and the cooling rate is 2 to 15° C. / s.
[0044] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and drawings.
[0045] Example 1
[0046] (1) The temperature of the epitaxial furnace reaction chamber was raised to 1170°C, and the graphite components of the reaction chamber were etched and cleaned with high-flow HCl with a flow rate of 20 SLM and H2 with a flow rate of 10 SLM for 20 seconds. The flow rate of H2 was increased to 60 SLM for another 55 seconds to remove the residual reactants in the chamber, thereby ensuring the cleanliness of the internal environment of the chamber, and the temperature of the reaction chamber was cooled to 750°C;
[0047] (2) A temperature control sheet with a thickness of 620 μm and a resistivity of 15 Ω·cm was loaded into the reaction chamber, and the temperature of the reaction chamber was raised from 750°C to 1130°C at a heating rate of 15°C / s. The temperature was then baked at a constant temperature for 120 s in a 60 SLM H2 atmosphere, and the susceptor speed was 0 r / min. After the baking was completed, the reaction chamber was cooled to 890°C and the temperature control sheet was unloaded.
[0048] (3) The resistivity of the temperature control sheet is measured using the 4PP test system Napson RT-3000 to obtain the 4PP resistivity mapping diagram of the temperature control sheet (e.g. Figure 1 As shown), the resistivity of the five temperature zones of the temperature control plate center, front, back, left and right are obtained respectively; the temperature of each temperature zone of the temperature control plate is further calculated through the linear relationship between temperature and resistivity, thereby calculating the temperature difference between the edge temperature zone and the center temperature zone, and adjusting the temperature of each temperature zone to be consistent through the corresponding temperature compensation mechanism for the edge area; specifically, the relationship between resistivity and temperature is: Δρ=-1.8×ΔT, wherein Δρ is the resistivity change, and ΔT is the temperature change.
[0049] (4) The temperature of the epitaxial furnace reaction chamber was raised to 1170°C, and the graphite components of the reaction chamber were etched and cleaned with high-flow 20SLM HCl and 10SLM H2 for 20s, and then the H2 flow was increased to 60SLM for 55s to remove the residual reactants in the chamber, thereby ensuring the cleanliness of the internal environment of the chamber; the temperature of the reaction chamber was cooled to 750°C, and the heavily arsenic-doped substrate silicon wafer was loaded into the reaction chamber;
[0050] (5) At the compensation temperature determined in step (3), the temperature of the reaction chamber is increased from 750° C. to 1050° C. at a heating rate of 15° C. / s, and then from 1050° C. to 1150° C. at a heating rate of 2° C. / s, the rotation speed of the susceptor is increased to 35 r / min, and in an atmosphere of 60 SLM H2, 16 g / min of TCS and 98 sccm of PH3 are introduced for epitaxial growth, and the epitaxial growth is performed to a thickness of 10.22 μm and a resistivity of 3.11 Ω·cm, wherein the amount of dopant used is set according to the target resistivity, and the epitaxial growth time is set according to the target thickness and growth rate;
[0051] (6) After the epitaxial growth is completed, the temperature of the reaction chamber is cooled from 1150°C to 890°C at a cooling rate of 15°C / s to unload the silicon epitaxial wafer.
[0052] The slip line condition in the silicon epitaxial wafer prepared in this embodiment was tested using a microscope, and the results are as follows: Figure 2 As shown, there is no slip line on the surface of the epitaxial wafer. At the same time, the uniformity of the epitaxial layer thickness in the silicon epitaxial wafer is controlled within 1.0%, and the repeatability of the thickness between different epitaxial wafers is controlled within 0.5%; the uniformity of the resistivity within the silicon epitaxial wafer is controlled within 2.5%, and the repeatability of the resistivity between wafers is controlled within 1.0%, which fully meets the epitaxial requirements. The wafer output per hour (WPH) is calculated to be 4.88pcs / h.
[0053] Example 2
[0054] The method is the same as that in Example 1, except that in step (5), the two heating procedures are: heating the temperature of the reaction chamber from 750°C to 1050°C at a heating rate of 10°C / s, and then heating from 1050°C to 1150°C at a heating rate of 2°C / s.
[0055] The slip line condition in the silicon epitaxial wafer prepared in this embodiment was tested using a microscope, and the results are as follows: Figure 3 As shown, there is no slip line on the surface of the epitaxial wafer; the wafer output per hour (WPH) is calculated to be 4.45 pcs / h.
[0056] Example 3
[0057] The method is the same as that in Example 1, except that in step (5), the two heating procedures are: heating the temperature of the reaction chamber from 750°C to 1050°C at a heating rate of 15°C / s, and then heating from 1050°C to 1150°C at a heating rate of 3°C / s.
[0058] The slip line condition in the silicon epitaxial wafer prepared in this embodiment was tested using a microscope, and the results are as follows: Figure 4As shown, there are very slight slip lines at the 3, 6, and 9 o'clock directions of the epitaxial wafer; the wafer output per hour (WPH) is calculated to be 5.08 pcs / h.
[0059] Comparative Example 1
[0060] (1) The temperature of the epitaxial furnace reaction chamber was raised to 1170°C, and the graphite components of the reaction chamber were etched and cleaned with high-flow HCl of 20 SLM and H2 of 10 SLM for 20 seconds. The H2 flow rate was increased to 60 SLM for another 55 seconds to remove the residual reactants in the chamber, thereby ensuring the cleanliness of the internal environment of the chamber, and the temperature of the reaction chamber was cooled to 750°C;
[0061] (2) Loading the heavily arsenic-doped silicon wafer substrate into a reaction chamber, raising the temperature of the reaction chamber from 750° C. to 1150° C. at a heating rate of 15° C. / s at the compensation temperature determined in Example 1, increasing the rotation speed of the susceptor to 35 r / min, introducing 16 g / min of TCS and 98 sccm of PH3 in an atmosphere of 60 SLM H2 for epitaxial growth, and epitaxial growth to a thickness of 10.22 μm and a resistivity of 3.11 Ω·cm, wherein the amount of dopant used is set according to the target resistance, and the epitaxial time is set according to the target thickness and the growth rate;
[0062] (3) After the epitaxial growth is completed, the reaction chamber is cooled from 1150°C to 890°C at a rate of 15°C / s to unload the silicon epitaxial wafer.
[0063] The slip line condition in the silicon epitaxial wafer prepared in this comparative example was tested using a microscope, and the results were as follows: Figure 5 As shown, there are 4 shallow slip lines at the 3 o'clock direction of the epitaxial wafer, 1 deep and 2 shallow slip lines at the 6 o'clock direction, two shallow slip lines between the 8 o'clock and 9 o'clock directions, and n shallow and dense slip lines at the 11 o'clock direction; the wafer output per hour (WPH) is calculated to be 4.35 pcs / h.
[0064] Comparative Example 2
[0065] The processing method of this comparative example is the same as that of Example 1, except that in step (5), the temperature control program adopted is: the temperature of the reaction chamber is increased from 750°C to 1150°C at a heating rate of 15°C / s, and the temperature is kept constant for 2 minutes when the temperature is increased to 800°C and 900°C, the susceptor speed is increased to 35r / min, and 16g / min of TCS and 98sccm of PH3 are introduced in an atmosphere of 60SLM H2 for epitaxial growth, and the epitaxial growth is performed to a thickness of 10.22μm and a resistivity of 3.11Ω·cm, wherein the amount of dopant is set according to the target resistivity, and the epitaxial growth time is set according to the target thickness and growth rate.
[0066] The slip line condition in the silicon epitaxial wafer prepared in this comparative example was tested using a microscope, and the results were as follows: Figure 6 As shown, there is no slip line on the surface of the epitaxial wafer; the wafer output per hour (WPH) is calculated to be 3.68 pcs / h.
[0067] Comparative Example 3
[0068] The method is the same as that in Example 1, except that in step (5), the two heating procedures are: heating the temperature of the reaction chamber from 750°C to 1050°C at a heating rate of 3°C / s, and then heating from 1050°C to 1150°C at a heating rate of 2°C / s.
[0069] The slip line condition in the silicon epitaxial wafer prepared in this comparative example was tested using a microscope, and the results were as follows: Figure 7 As shown, there is no slip line on the surface of the epitaxial wafer; the wafer output per hour (WPH) is calculated to be 4.04 pcs / h.
[0070] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0071] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.
Claims
1. A method for improving the slip line of a silicon epitaxial wafer, characterized in that: The following steps are involved: (1) placing the temperature control sheet into a cleaned epitaxial furnace reaction chamber for constant temperature baking, performing a resistivity test on the temperature control sheet obtained after constant temperature baking, obtaining the temperature distribution of each area of the temperature control sheet, and calculating the temperature difference between the front, rear, side and center areas of the temperature control sheet; (2) loading the silicon wafer into a cleaned epitaxial furnace reaction chamber, raising the temperature to the growth temperature using a two-step heating program and simultaneously performing temperature compensation according to the temperature difference described in step (1), then introducing a silicon source, hydrogen and a dopant, epitaxially growing to a target thickness and a target resistivity, cooling the obtained silicon epitaxial wafer and then taking it out, wherein the two-step heating program is to first raise the temperature to 900 to 1050° C. at a heating rate of 10 to 15° C. / s for a heating time of 7 to 65 s, and then raise the temperature to 1150° C. at a heating rate of 2° C. / s for a heating time of 50 to 125 s; Wherein, in step (1) and / or step (2), the reaction chamber of the epitaxial furnace that has been cleaned is lowered to a wafer loading temperature, and the wafer loading temperature is 400-800°C.
2. The method for improving the slip line of a silicon epitaxial wafer according to claim 1, characterized in that: In step (1) and / or step (2), the cleaning treatment is to heat the epitaxial furnace reaction chamber to the etching temperature, use hydrogen chloride and hydrogen to etch and clean the graphite components in the reaction chamber, close the hydrogen chloride pipeline, increase the hydrogen flow rate for purging, and then cool the epitaxial furnace reaction chamber to the wafer feeding temperature.
3. The method for improving the slip line of a silicon epitaxial wafer according to claim 2, characterized in that: In the step (1), the flow rate of the hydrogen chloride is 15 to 25 SLM, and the flow rate of the hydrogen is 10 to 100 SLM; and / or, in the step (1), the etching temperature is 1100 to 1200°C.
4. The method for improving the slip line of a silicon epitaxial wafer according to claim 1, characterized in that: In the step (1), the thickness of the temperature control sheet is 600-650 μm, and the resistivity is 8-20 Ω·cm; the temperature control sheet is boron-doped <100> Ion implantation into silicon wafers.
5. The method for improving the slip line of a silicon epitaxial wafer according to claim 1, characterized in that: In the step (1), the baking temperature is 1100-1200° C., and the constant temperature baking time is 20-180 seconds.
6. The method for improving the slip line of a silicon epitaxial wafer according to claim 1, characterized in that: In the step (1), the resistivity test is performed using a four-probe resistance tester.
7. The method for improving the slip line of a silicon epitaxial wafer according to claim 1, characterized in that: In the step (2), the silicon source is trichlorosilane, and the dopant includes at least one of BH3, PH3, and AsH3.
8. The method for improving the slip line of a silicon epitaxial wafer according to claim 7, characterized in that: In the step (2), the flow rate of the hydrogen is 60 to 90 SLM, and the rate of the epitaxial growth is 1 to 5 μm / min.
9. The method for improving the slip line of a silicon epitaxial wafer according to claim 1, characterized in that: In the step (2), the cooling temperature is 890° C., and the cooling rate is 2 to 15° C. / s.