A method for preparing a large-size pressure vessel head

By carrying out tailor welding, hot press forming, quenching and tempering treatment on the large-sized heads, the chemical composition of the steel plate and welding wire is adjusted to form a stable organizational structure, which solves the problem of insufficient mechanical properties of the heads and improves the strength and toughness. Meets the standards of high-end container manufacturing.

CN116079352BActive Publication Date: 2024-10-29CHINA RAILWAY CONSTR HEAVY IND
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310162269.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-24
Publication Date
2024-10-29
Estimated Expiration
2043-02-24

AI Technical Summary

Technical Problem

The mechanical properties of the large-sized head cannot meet the standard requirements. The welding process causes the heat-affected zone of the weld joint to soften and reduce the strength, making it unable to meet the mechanical properties required by the design.

Method used

After the Q690D steel plate is used for tailor welding and hot press forming, it is quenched and tempered to adjust the chemical composition of the steel plate and welding wire, improve the hardenability of the steel plate and the tensile strength of the weld, and form martensite and tempered soxhlet. body tissue and improve the comprehensive mechanical properties of the head.

Benefits of technology

Through quenching and tempering treatment, the strength and toughness of large-sized heads are improved, meeting the mechanical performance requirements of high-end container manufacturing, reducing product scrap rates, and saving production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116079352B_ABST
    Figure CN116079352B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a large-size pressure vessel head, comprising the following steps: S1: welding a plurality of Q690D steel plates together by welding wire to obtain a large-size welded head. S2: hot pressing the welded head to obtain a hot pressing formed head. S3: heating the hot pressing formed head from room temperature to 900-920°C at a heating rate of ≤100°C / h, keeping the temperature for 1.5-2.5min / mm, and obtaining a quenched head after cooling. S4: heating the quenched head from room temperature to 600-630°C at a heating rate of ≤100°C / h, keeping the temperature for 130-170min, and air cooling to obtain the head. The present invention optimizes the head preparation process so that the large-size head base material maintains the Q690D tempered state, and the tensile strength at the weld position also exceeds the tensile strength of the Q690D material, thereby realizing batch manufacturing of large-diameter and high-strength heads.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of end cap processing, and in particular relates to a method for preparing an end cap of a large-size pressure vessel. Background Art

[0002] The head is the main pressure-bearing component of the pressure vessel. Heads of different plate thicknesses and materials have different manufacturing processes. According to the forming temperature, they are generally divided into cold forming and hot forming. According to the manufacturing process, they are generally divided into spinning and molding. The final acceptance criteria for the head include: dimensional accuracy, shape and position tolerances, and the performance of the final head base material.

[0003] Thin plate heads with a thickness of ≤20mm generally adopt cold forming technology. After cold forming, the hardness and strength of the head increase, the plastic toughness decreases, and work hardening occurs. There is some internal stress inside the material. The dimensional accuracy after forming is worse than that of hot forming. However, cold forming has little effect on the mechanical properties of quenched and tempered steel. The mechanical properties of the head after forming can still meet the requirements of relevant standards.

[0004] With the continuous enlargement of ultra-high pressure equipment, the wall thickness and size of the heads used in ultra-high pressure equipment are also increasing, and the strength level of the raw materials is also greatly improved, so the deformation resistance is greater. Therefore, the forming method of large-size ultra-thick plate high-strength heads is generally hot forming. Hot forming is a process in which the head is formed by hot forming. C3 The above 30-50℃ austenite temperature range forming has low requirements on the pressing capacity of the pressing equipment. Compared with cold forming, its process thinning is smaller, the precision is higher, and it can better meet the size requirements. When the unfolded long diameter of the head is greater than 3000mm, it is generally necessary to weld. The precision of the overall welding forming is much higher than the precision of the piece forming and then welding into a head, so the process of blanking-groove processing-welding-hot pressing-tempering-overall processing is generally adopted. However, the preparation of large-size, high-strength and ultra-thick plate heads still has the following problems:

[0005] On the one hand, the large-size head welding has a large filling volume, and the weld and surrounding tissues have large residual internal stresses, which leads to a high risk of defects in the welding, hot pressing, and tempering processes. On the other hand, the welding process will cause the heat-affected zone of the weld joint to soften and reduce its strength. The subsequent hot processing process will further reduce the strength of the weld joint and fail to meet the mechanical properties required by the design.

[0006] Therefore, new processes need to be developed to produce heads that meet performance requirements and conform to the development trend of high-end container manufacturing. Summary of the invention

[0007] 1. Technical issues to be resolved

[0008] In order to solve the problem in the prior art that the mechanical properties of large-sized heads cannot meet standard requirements, the present invention provides a method for preparing a large-sized pressure vessel head.

[0009] (II) Technical solution

[0010] In order to achieve the above object, the main technical solutions adopted by the present invention include:

[0011] A method for preparing a large-size pressure vessel head comprises the following steps:

[0012] S1. Welding: Welding multiple steel plates together by welding wire to obtain a welded head with a diameter of ≥3000mm; the steel plate is Q690D steel plate, and the thickness of the steel plate is ≥80mm;

[0013] S2, hot pressing forming: hot pressing the welded head to obtain a hot pressing formed head;

[0014] S3, quenching: heating the hot-pressed head from room temperature to 900-920°C at a heating rate of ≤100°C / h, keeping the temperature for 1.5-2.5min / mm, and then cooling it to room temperature to obtain a quenched head;

[0015] S4. Tempering: Heat the quenched head from room temperature to 600-630℃ at a heating rate of ≤100℃ / h, keep warm for 130-170min, and then cool to room temperature in air to obtain the head.

[0016] In the prior art, the preparation process of the large-sized head is completed after welding and hot pressing, and no quenching and tempering treatment is continued. The present invention performs quenching and tempering treatment on the head after welding and hot pressing, so that the performance of the obtained large-sized head product meets the standard requirements. The steel plate used for welding in the present invention is Q690D steel plate, and its thickness is ≥80mm. Using steel plates in this thickness range, large-sized ultra-thick heads can be obtained.

[0017] After hot pressing, the strength, hardness and wear resistance of the hot pressing head are improved, but the brittleness is large, that is, the impact performance is poor, the organization is unstable and the internal stress is large. After quenching, the organization in the steel plate is lath martensite. After tempering, the internal organization is martensite + tempered troostite organization. The tempered troostite, that is, fine-grained cementite, is dispersed in the ferrite, which improves the toughness of the steel plate. The transformation of the internal organization leads to improved performance.

[0018] The steel mill quenches and tempers the steel plate to meet the mechanical performance indicators of Q690 steel plate. The quenching and tempering process in the present invention is to restore the mechanical properties of the base material and the weld after hot pressing. The hot pressing process is to heat to the phase transition temperature and then perform hot pressing, cool in the air, and the cooling rate is slow to obtain a pearlite structure. When quenching after hot pressing, reheat to above the phase transition point and recirculate water to accelerate cooling, and high temperature tempering obtains a martensite + tempered troostite structure. Therefore, quenching and tempering in the present invention make the head have better comprehensive mechanical properties.

[0019] According to the preparation method as described above, preferably, in step S1, the chemical composition of the Q690D steel plate includes, by mass percentage: C: 0.14-0.17%, Si: 0.20-0.28%, P: 0.007-0.009%, S: 0.0020-0.0030%, Cu: 0.04-0.06%, Nb: 0.02-0.05%, Ti: 0.01-0.019%, V: 0.024-0.030%, Mn: 1.08-1.20%, Cr: 1.04-1.23%, Ni: 1.09-1.20%, Mo: 0.42-0.50%;

[0020] The rest is Fe and inevitable impurity elements.

[0021] The present invention improves the hardenability of the Q690D steel plate by adjusting the parent metal components of the chemical composition of the Q690D steel plate, especially adjusting the content of Cr, Ni, Mn and Mo elements. The internal structure of the Q690D steel plate is mainly martensite, and the functions of each element component in the Q690D steel plate in the present invention are as follows:

[0022] Cr: Cr can significantly improve the strength and wear resistance of the steel plate, and make the steel plate have good fatigue resistance and hardenability (the thick plate can also be completely transformed into martensite during quenching). If the Cr content is lower than 1.04%, the strength, wear resistance, fatigue resistance and hardenability of the steel plate cannot be guaranteed, and if it is higher than 1.23%, the cost will increase. Therefore, in the present invention, the Cr content is preferably 1.04-1.23%.

[0023] Mo: Mo element can reduce the transformation temperature of martensite in the steel plate, refine the martensite structure, and can transform into finer martensite even at a low cooling rate.

[0024] Ni: Ni element can improve the hardenability of steel plate, prevent the growth of grains at high temperature, so that the steel plate can still maintain fine grain structure at high temperature and improve toughness.

[0025] Mn: The combined addition of Mn, Cr and Ni can increase the hardenability of the steel plate, allowing the martensitic transformation to occur at a lower temperature, thereby obtaining a lower martensitic structure with higher strength and lower ductile-brittle transition temperature than the upper martensitic structure.

[0026] According to the preparation method described above, preferably, in step S1, the chemical composition of the welding wire includes, by mass percentage: C: 0.06-0.07%; Mn: 1.62-1.64%; Si: 0.35-0.4%; S: 0.003-0.005%; P: 0.01-0.013%; Cr: 0.35-0.39%; Ni: 2.7-3.0%; Mo: 0.5-0.6%; Cu: 0.04-0.08%;

[0027] The rest is Fe and inevitable impurity elements.

[0028] The mechanical property requirements of the Q690D steel plate in the present invention are as follows: tensile strength Rm=760-930MPa, yield strength ReH>650MPa, elongation after fracture A%≥14, and impact energy≥47J.

[0029] The present invention also makes reasonable adjustments to the element composition of the welding wire to ensure that the tensile strength of the weld position of the head after hot pressing, quenching and tempering meets the standard requirements and is greater than 760MPa. Specifically, the Ni element in the welding wire can improve the hardenability of the weld, prevent the growth of grains at high temperatures, so that the weld can still maintain a fine grain structure at high temperatures, improve toughness, improve heat resistance, and have small deformation during quenching. It can also improve welding performance together with the Cr element. The higher the Si content, the worse the welding performance, so its content should not be higher than 0.4%. The S element and the P element in the welding wire are impurity elements, and the less the content, the better.

[0030] In the preparation method as described above, preferably, in step S1, before welding, the steel plate is preheated to 100-120°C, and during welding, the welding current is 500-600A, the arc voltage is 28-32V, and the welding speed is 40-50cm / min; after welding, the welded end cap is placed at 300-350°C for dehydrogenation treatment for 2h. More preferably, before welding, the steel plate is preheated to 115°C, and during welding, the welding current is 500A, the arc voltage is 28V, and the welding speed is 40cm / min; after welding, the welded end cap is placed at 300°C for dehydrogenation treatment for 2h.

[0031] In the preparation method as described above, preferably, in step S2, the butt-welded head is subjected to two consecutive hot pressing processes to obtain a hot pressing formed head.

[0032] In the preparation method as described above, preferably, in step S2, the welded head is heated to 900-930°C at a heating rate of ≤100°C / h, kept warm for 1.5-2.5min / mm, and then molded once for preliminary forming. After the preliminary forming, it is heated for a second time. The welded head after the second heating is heated to 900-930°C at a heating rate of ≤100°C / h, kept warm for 50-70min, and air-cooled after forming.

[0033] In the preparation method as described above, preferably, in step S2, the temperature of the welded head is increased to 900°C at a heating rate of 80°C / h, and the temperature is kept at a temperature for 1.5 min / mm, and then the head is molded once for preliminary forming, and then heated for a second time after the preliminary forming. The welded head after the second heating is heated to 900°C at a heating rate of 80°C / h, and the temperature is kept at a temperature for 70 min, and then air-cooled after forming.

[0034] In the preparation method as described above, preferably, in step S3, the temperature of the hot-pressed head is raised from room temperature to 900° C. at a heating rate of 80° C. / h, and the holding time is 1.5 min / mm.

[0035] In the preparation method as described above, preferably, in step S4, the quenched head is heated from room temperature to 600°C at a heating rate of 80°C / h, kept at this temperature for 170 minutes, and then cooled to room temperature in air.

[0036] According to the preparation method as described above, preferably, the mechanical properties of the head base material obtained in step S4 are: tensile strength Rm: 890-894MPa, yield strength ReH: 839-843MPa, elongation after fracture A%: 18-19, impact energy: 250-253J; the mechanical properties of the weld position of the head obtained in step S4 are: tensile strength Rm: 792-796MPa, impact energy: 110-142J, all of which meet the standard requirements.

[0037] (III) Beneficial effects

[0038] The beneficial effects of the present invention are:

[0039] The present invention optimizes the preparation process of the head, welds a plurality of Q690D steel plates together and performs hot pressing and forming treatments, and then performs quenching and tempering treatments, thereby effectively ensuring the production quality control of the Q690D large-size head, so that the large-size head mother material after the welding, hot pressing and quenching and tempering treatments maintains the Q690D tempered state, and the tensile strength at the weld position also exceeds the tensile strength of the Q690D material, thereby realizing the batch manufacturing of large-diameter and high-strength heads, improving the strength of the heads, reducing the scrap rate of large-size head products, saving production costs, and increasing economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1The present invention is a flow chart of the preparation process of a large-size pressure vessel head. DETAILED DESCRIPTION

[0041] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.

[0042] Example 1

[0043] This embodiment provides a method for preparing a large-size pressure vessel head, comprising the following steps:

[0044] S1. Welding: Use submerged arc welding to preheat multiple pieces of 80mm thick Q690D steel plates to 110℃. Then use DC reverse connection, keep the welding current at 500A, the welding voltage at 28V, and the welding speed at 40cm / min, and weld multiple pieces of 80mm thick Q690D steel plates together through welding wire. The diameter after welding is 6300mm. After welding, dehydrogenate the welded parts at 300℃ for 2h.

[0045] In this step, the chemical composition of the Q690D steel plate includes, by mass percentage, C: 0.14%, Si: 0.26%, P: 0.009%, S: 0.0027%, Cu: 0.04%, Nb: 0.02%, Ti: 0.012%, V: 0.03%, Mn: 1.08%, Cr: 1.04%, Ni: 1.14%, Mo: 0.42%, and the rest are Fe and unavoidable impurity elements.

[0046] In this step, the chemical composition of the welding wire includes, by mass percentage: C: 0.062%; Mn: 1.63%; Si: 0.36%; S: 0.004%; P: 0.011%; Cr: 0.39%; Ni: 2.83%; Mo: 0.55%; Cu: 0.06%, and the rest is Fe and unavoidable impurity elements. Specifically, the diameter of the welding wire is 4 mm, and the mechanical properties are: tensile strength Rm = 857 MPa, yield strength ReH = 734 MPa, elongation after fracture A% = 17, and impact energy 133 J.

[0047] S2. Hot pressing: The welded head is heated to 900°C at a heating rate of 80°C / h, and the heat preservation time is 1.5min / mm. Then, it is molded once for preliminary forming. After the preliminary forming, it is transferred to the furnace for further heating and secondary heating. The welded head after secondary heating is heated to 900°C at a heating rate of 80°C / h, and the heat preservation time is 70min. After forming, it is air-cooled to obtain a welded head with a diameter of 5000mm.

[0048] S3, quenching: put the hot-pressed head into a heat treatment furnace, heat it from room temperature to 900°C at a heating rate of 80°C / h, keep it at a temperature for 1.5min / mm, then cool it to room temperature in a circulating water pool to obtain a quenched head.

[0049] S4. Tempering: put the quenched head into a heat treatment furnace, raise the temperature from room temperature to 600°C at a heating rate of 80°C / h, keep the temperature for 170 minutes, and then cool it to room temperature in air to obtain the head.

[0050] The mechanical properties of the head base material prepared in this embodiment are as follows:

[0051] Tensile strength Rm = 894MPa, yield strength ReH = 843MPa, elongation after fracture A% = 19, impact energy 253J.

[0052] The tensile strength and impact work of the weld position of the head prepared in this embodiment are as follows:

[0053] Tensile strength Rm=794MPa, impact energy 142J.

[0054] The mechanical properties of the above-mentioned head base material and weld position can meet the standard requirements of "GBT 16270-2009 High Strength Structure Quenched and Tempered Steel Plate".

[0055] Example 2

[0056] This embodiment provides a method for preparing a large-size pressure vessel head, comprising the following steps:

[0057] S1. Welding: Use submerged arc welding to preheat multiple pieces of 85mm thick Q690D steel plates to 115℃. Then use DC reverse connection, keep the welding current at 550A, the welding voltage at 30V, and the welding speed at 45cm / min, and weld multiple pieces of 85mm thick Q690D steel plates together through welding wire. The diameter after welding is 6300mm. After welding, dehydrogenate the welded parts at 325℃ for 2h.

[0058] In this step, the chemical composition of the Q690D steel plate includes, by mass percentage, C: 0.15%, Si: 0.26%, P: 0.007%, S: 0.0020%, Cu: 0.06%, Nb: 0.05%, Ti: 0.019%, V: 0.024%, Mn: 1.18%, Cr: 1.23%, Ni: 1.20%, Mo: 0.44%, and the rest are Fe and unavoidable impurity elements.

[0059] In this step, the chemical composition of the welding wire includes by mass percentage: C: 0.06%; Mn: 1.62%; Si: 0.35%; S: 0.003%; P: 0.01%; Cr: 0.35%; Ni: 2.7%; Mo: 0.5%; Cu: 0.04%, and the rest is Fe and inevitable impurity elements. The diameter of the welding wire is 4mm, and the mechanical properties are: tensile strength Rm = 852MPa, yield strength ReH = 730MPa, elongation after fracture A% = 17, and impact energy 131J.

[0060] S2. Hot pressing: The welded head is heated to 905°C at a heating rate of 90°C / h, and the heat preservation time is 2.0min / mm. Then, it is molded once for preliminary forming. After the preliminary forming, it is transferred to the furnace for further heating and secondary heating. The welded head after secondary heating is heated to 905°C at a heating rate of 90°C / h, and the heat preservation time is 60min. After forming, it is air-cooled to obtain a welded head with a diameter of 5000mm.

[0061] S3, quenching: put the hot-pressed head into a heat treatment furnace, heat it from room temperature to 910°C at a heating rate of 90°C / h, keep it at a temperature for 2.0min / mm, then cool it to room temperature in a circulating water pool to obtain a quenched head.

[0062] S4. Tempering: put the quenched head into a heat treatment furnace, raise the temperature from room temperature to 610°C at a heating rate of 90°C / h, keep the temperature for 150 minutes, and then cool it to room temperature in air to obtain the head.

[0063] The mechanical properties of the head base material prepared in this embodiment are as follows:

[0064] Tensile strength Rm = 894MPa, yield strength ReH = 840MPa, elongation after fracture A% = 19, impact energy 250J.

[0065] The tensile strength and impact work of the weld position of the head prepared in this embodiment are as follows:

[0066] Tensile strength Rm=792MPa, impact energy 132J.

[0067] The mechanical properties of the above-mentioned head base material and weld position can meet the standard requirements of "GBT 16270-2009 High Strength Structure Quenched and Tempered Steel Plate".

[0068] Example 3

[0069] This embodiment provides a method for preparing a large-size pressure vessel head, comprising the following steps:

[0070] S1. Welding: Use submerged arc welding to preheat multiple pieces of 90mm thick Q690D steel plates to 120℃. Then use DC reverse connection, keep the welding current at 600A, the welding voltage at 32V, and the welding speed at 50cm / min, and weld multiple pieces of 90mm thick Q690D steel plates together through welding wire. The diameter after welding is 6300mm. After welding, dehydrogenate the welded parts at 350℃ for 2h.

[0071] In this step, the chemical composition of the Q690D steel plate includes, by mass percentage, C: 0.17%, Si: 0.20%, P: 0.007%, S: 0.003%, Cu: 0.05%, Nb: 0.04%, Ti: 0.01%, V: 0.029%, Mn: 1.20%, Cr: 1.04%, Ni: 1.09%, Mo: 0.5%, and the rest are Fe and unavoidable impurity elements.

[0072] In this step, the chemical composition of the welding wire includes by mass percentage: C: 0.07%; Mn: 1.64%; Si: 0.4%; S: 0.005%; P: 0.013%; Cr: 0.39%; Ni: 3.0%; Mo: 0.6%; Cu: 0.08%, and the rest is Fe and inevitable impurity elements. The diameter of the welding wire is 4mm, and the mechanical properties are: tensile strength Rm = 853MPa, yield strength ReH = 730MPa, elongation after fracture A% = 17, and impact energy 129J.

[0073] S2. Hot pressing: The welded head is heated to 910°C at a heating rate of 100°C / h, and the heat preservation time is 2.5min / mm. Then, it is molded once for preliminary forming. After the preliminary forming, it is transferred to the furnace for further heating and secondary heating. The welded head after secondary heating is heated to 910°C at a heating rate of 100°C / h, and the heat preservation time is 50min. After forming, it is air-cooled to obtain a welded head with a diameter of 5000mm.

[0074] S3, quenching: put the hot-pressed head into a heat treatment furnace, heat it from room temperature to 920°C at a heating rate of 100°C / h, keep it at this temperature for 2.5min / mm, then cool it to room temperature in a circulating water pool to obtain a quenched head.

[0075] S4. Tempering: put the quenched head into a heat treatment furnace, raise the temperature from room temperature to 620°C at a heating rate of 100°C / h, keep the temperature for 130 minutes, and then cool it to room temperature in air to obtain the head.

[0076] The mechanical properties of the head base material prepared in this embodiment are as follows:

[0077] Tensile strength Rm = 890MPa, yield strength ReH = 839MPa, elongation after fracture A% = 18, impact energy 251J.

[0078] The tensile strength and impact work of the weld position of the head prepared in this embodiment are as follows:

[0079] Tensile strength Rm=796MPa, impact energy 110J.

[0080] The mechanical properties of the above-mentioned head base material and weld position meet the standard requirements of "GBT 16270-2009 High Strength Structure Quenched and Tempered Steel Plate".

[0081] Example 4

[0082] The present embodiment provides a method for preparing a large-size pressure vessel head, which is different from the embodiment 1 in that, in step S2, the temperature of the welded head is increased to 920°C at a heating rate of 90°C / h, and the temperature is kept for 2.0 min / mm, and then the head is molded once for preliminary forming. After the preliminary forming, the head is transferred to the furnace for further heating and secondary heating is performed. The welded head after secondary heating is also heated to 920°C at a heating rate of 90°C / h, and the temperature is kept for 60 min, and the head is air-cooled after forming.

[0083] The mechanical properties of the head base material prepared in this embodiment are as follows:

[0084] Tensile strength Rm = 882MPa, yield strength ReH = 841MPa, elongation after fracture A% = 18, impact energy 241J.

[0085] The tensile strength and impact work of the weld position of the head prepared in this embodiment are as follows:

[0086] Tensile strength Rm=790MPa, impact energy 124J.

[0087] The mechanical properties of the above-mentioned head base material and weld position meet the standard requirements of "GBT 16270-2009 High Strength Structure Quenched and Tempered Steel Plate".

[0088] Example 5

[0089] The present embodiment provides a method for preparing a large-size pressure vessel head, which is different from the embodiment 1 in that, in step S2, the temperature of the welded head is increased to 930°C at a heating rate of 100°C / h, and the temperature is kept at a high temperature for 2.5 min / mm, and then the head is molded once for preliminary forming. After the preliminary forming, the head is transferred to the furnace for further heating and secondary heating is performed. The welded head after secondary heating is also heated to 930°C at a heating rate of 100°C / h, and the temperature is kept at a high temperature for 50 min, and the head is air-cooled after forming.

[0090] The mechanical properties of the head base material prepared in this embodiment are as follows:

[0091] Tensile strength Rm = 879 MPa, yield strength ReH = 832 MPa, elongation after fracture A% = 18, impact energy 246 J.

[0092] The tensile strength and impact work of the weld position of the head prepared in this embodiment are as follows:

[0093] Tensile strength Rm=789MPa, impact energy 119J.

[0094] The mechanical properties of the above-mentioned head base material and weld position meet the standard requirements of "GBT 16270-2009 High Strength Structure Quenched and Tempered Steel Plate".

[0095] Comparative Example 1

[0096] This comparative example provides a method for preparing a large-size pressure vessel head, which is different from Example 1 in that the quenching treatment in step S3 and the tempering treatment in step S4 are not performed.

[0097] The mechanical properties of the head base material prepared in this comparative example are as follows:

[0098] Tensile strength Rm = 522 MPa, yield strength ReH = 378 MPa, elongation after break A% = 30%.

[0099] The tensile strength and impact work of the weld position of the head prepared in this comparative example are as follows:

[0100] Tensile strength Rm=597MPa.

[0101] The mechanical properties of the above-mentioned head base material and weld position do not meet the standard requirements of "GBT 16270-2009 High Strength Structure Quenched and Tempered Steel Plate".

[0102] Comparative Example 2

[0103] This comparative example provides a method for preparing a large-size pressure vessel head. The difference compared with Example 1 is that the chemical composition of the Q690D steel plate includes, by mass percentage: C: 0.14%, Si: 0.26%, P: 0.009%, S: 0.0027%, Cu: 0.04%, Nb: 0.02%, Ti: 0.012%, V: 0.03%, Mn: 0.68%, Cr: 0.83%, Ni: 0.92%, Mo: 0.25%, and the rest are Fe and unavoidable impurity elements.

[0104] The mechanical properties of the head base material prepared in this comparative example are as follows:

[0105] Tensile strength Rm = 710MPa, yield strength ReH = 612MPa, elongation after fracture A% = 12, impact energy 128J.

[0106] The tensile strength and impact work of the weld position of the head prepared in this comparative example are as follows:

[0107] Tensile strength Rm=784MPa, impact energy 129J.

[0108] The mechanical properties of the above-mentioned head base material do not meet the standard requirements of "GBT 16270-2009 High Strength Quenched and Tempered Steel Plate for Structures".

[0109] Comparative Example 3

[0110] This comparative example provides a method for preparing a large-size pressure vessel head. The difference compared with Example 1 is that the chemical composition of the welding wire includes, by mass percentage: C: 0.06%; Mn: 1.62%; Si: 0.35%; S: 0.003%; P: 0.01%; Cr: 0.24%; Ni: 1.5%; Mo: 0.5%; Cu: 0.04%, and the rest is Fe and unavoidable impurity elements.

[0111] The mechanical properties of the head base material prepared in this comparative example are as follows:

[0112] Tensile strength Rm = 855MPa, yield strength ReH = 826MPa, elongation after fracture A% = 18, impact energy 242J.

[0113] The tensile strength and impact work of the weld position of the head prepared in this comparative example are as follows:

[0114] Tensile strength Rm=583MPa, impact energy 104J.

[0115] The mechanical properties of the above-mentioned head weld position do not meet the standard requirements of "GBT 16270-2009 High Strength Structure Quenched and Tempered Steel Plate".

[0116] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "embodiment", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.

[0117] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may alter, modify, replace and modify the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a large-size pressure vessel head. It is characterized in that The steps include: S1. Welding: Welding multiple steel plates together by welding wire to obtain a welded head with a diameter of ≥3000mm; the steel plate is Q690D steel plate, and the thickness of the steel plate is ≥80mm; S2, hot pressing forming: hot pressing the welded head to obtain a hot pressing formed head; S3, quenching: heating the hot-pressed head from room temperature to 900-920°C at a heating rate of ≤100°C / h, keeping the temperature for 1.5-2.5min / mm, and then cooling it to room temperature to obtain a quenched head; S4, tempering: the quenched head is heated from room temperature to 600-630℃ at a heating rate of ≤100℃ / h, kept at this temperature for 130-170min, and then cooled to room temperature in air to obtain the head; In step S1, the chemical composition of the Q690D steel plate includes, by mass percentage, C: 0.14-0.17%, Si: 0.20-0.28%, P: 0.007-0.009%, S: 0.0020-0.0030%, Cu: 0.04-0.06%, Nb: 0.02-0.05%, Ti: 0.01-0.019%, V: 0.024-0.030%, Mn: 1.08-1.20%, Cr: 1.04-1.23%, Ni: 1.09-1.20%, Mo: 0.42-0.50%; the rest are Fe and unavoidable impurity elements; The chemical composition of the welding wire includes, by mass percentage, C: 0.06-0.07%; Mn: 1.62-1.64%; Si: 0.35-0.4%; S: 0.003-0.005%; P: 0.01-0.013%; Cr: 0.35-0.39%; Ni: 2.7-3.0%; Mo: 0.5-0.6%; Cu: 0.04-0.08%; and the rest are Fe and unavoidable impurity elements.

2. The preparation method according to claim 1, It is characterized in that In step S1, before welding, the steel plate is preheated to 100-120°C. During welding, the welding current is 500-600A, the arc voltage is 28-32V, and the welding speed is 40-50cm / min. After welding, the welded head is placed at 300-350°C for dehydrogenation treatment for 2h.

3. The preparation method according to claim 1, It is characterized in that In step S2, the butt-welded head is subjected to two consecutive hot pressing processes to obtain a hot pressing formed head.

4. The preparation method according to claim 3, It is characterized in that In step S2, the welded head is heated to 900-930°C at a heating rate of ≤100°C / h, kept warm for 1.5-2.5min / mm, and then molded once for preliminary forming. After the preliminary forming, it is heated for a second time. The welded head after the second heating is heated to 900-930°C at a heating rate of ≤100°C / h, kept warm for 50-70min, and air-cooled after forming.

5. The preparation method according to claim 4, It is characterized in that In step S2, the temperature of the welded head is increased to 900°C at a heating rate of 80°C / h, and the temperature is kept for 1.5min / mm, and then it is molded once for preliminary forming. After the preliminary forming, it is heated for a second time. The welded head after the second heating is heated to 900°C at a heating rate of 80°C / h, and the temperature is kept for 70min. After forming, it is air-cooled.

6. The preparation method according to claim 1, It is characterized in that In step S3, the temperature of the hot-pressed head is raised from room temperature to 900°C at a heating rate of 80°C / h, and the holding time is 1.5 min / mm.

7. The preparation method according to claim 1, It is characterized in that In step S4, the quenched head is heated from room temperature to 600°C at a heating rate of 80°C / h, kept at this temperature for 170 minutes, and then cooled to room temperature in air.

8. The preparation method according to claim 1, It is characterized in that The mechanical properties of the head base material obtained in step S4 are as follows: tensile strength Rm: 890-894 MPa, yield strength ReH: 839-843 MPa, elongation after fracture A%: 18-19, and impact energy: 250-253 J; The mechanical properties of the weld position of the head obtained in step S4 are: tensile strength Rm: 792-796 MPa, impact energy: 110-142 J.

Citation Information

Patent Citations

  • Steel plate with super-large thickness for nuclear power engineering equipment and production method thereof

    CN102851578A

  • Submerged-arc welding method for P690QL1 and Q370R dissimilar steel

    CN103464876A

  • Integral forming method for large aluminum alloy welding plate sealing head with uniform performance

    CN108161353A

  • Punch forming method for nickel-based alloy end socket

    CN115139065A

  • Pressure vessel steel plate resistant against hydrogen-induced cracking and manufacturing method thereof

    US20180298463A1