Tungsten carbide powder and its preparation method and application

The multi-stage temperature-controlled carbonization process is used to prepare tungsten carbide powder with multiple-level particle size, which solves the problem of difficult to control the grain size distribution of tungsten carbide in non-uniform cemented carbide, improves the toughness and hardness of cemented carbide, simplifies the production process and Reduced costs.

CN116081625BActive Publication Date: 2024-11-08ZHUZHOU HARD ALLOY GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310083164.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-08
Publication Date
2024-11-08
Estimated Expiration
2043-02-08

AI Technical Summary

Technical Problem

In the prior art, when preparing non-uniform structural cemented carbide, it is difficult to stabilize the distribution of tungsten carbide grain size, resulting in unstable performance, cumbersome production process and high cost.

Method used

By preparing multi-level particle size tungsten carbide powder, the multi-stage temperature-controlled carbonization process is adopted to control the uniform particle size distribution of tungsten powder, and coarse, medium and fine tungsten carbide powder is obtained, which is used to prepare non-uniform cemented carbide to improve production efficiency and performance stability.

Benefits of technology

It realizes efficient preparation of non-uniform cemented carbide, improves the toughness and hardness of cemented carbide, simplifies the production process, reduces costs, and has stable product performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116081625B_ABST
    Figure CN116081625B_ABST
Patent Text Reader

Abstract

The present invention discloses a tungsten carbide powder and a preparation method and application thereof, and relates to the technical field of powder materials; the tungsten carbide powder comprises the following components by volume percentage: 19.24% to 35.21% of coarse tungsten carbide, 25.01% to 55.25% of medium tungsten carbide, and 11.32% to 20.38% of fine tungsten carbide. The present invention first prepares tungsten powder with uniform particle size distribution, and adopts a multi-stage temperature-controlled carbonization method to perform carburization. After treatment, tungsten carbide powders of different particle sizes can be obtained at one time. When the tungsten carbide powder is used to prepare cemented carbide, it is not necessary to add tungsten carbide powders of various particle sizes, and a non-uniform structure of cemented carbide can be obtained. The prepared cemented carbide has the characteristics of good toughness and excellent strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder materials, and in particular relates to tungsten carbide powder and a preparation method and application thereof. Background Art

[0002] WC-Co (tungsten carbide-cobalt) alloy is a more traditional cemented carbide material. Because the high hardness and high toughness of WC-Co alloy are contradictory, in order to prepare a "double high" alloy with both high hardness and high toughness, the use of cemented carbide with non-uniform structure is one of the effective methods to achieve the "double high" alloy.

[0003] The current method for preparing WC-Co non-uniform structure is to use WC powder of various particle size levels as combined matrix powder, and to obtain a non-uniform cemented carbide by wet grinding, drying, pressing and sintering the mixture prepared by this method.

[0004] CN101768679A discloses a method for preparing a non-uniform structure cemented carbide, which uses two or three particle sizes of WC and Co powder as raw materials, and the average grain size of the alloy obtained by conventional processes is 2.0μm to 3.0μm. The non-uniform structure cemented carbide prepared by using various particle sizes of WC raw materials has high dispersibility, so that the alloy has the plasticity and toughness of coarse particles of WC, the comprehensive performance of medium particles of WC, and the high wear resistance of fine particles of WC.

[0005] CN111349836A discloses a non-uniform structure cemented carbide roller ring. The raw materials for preparing the cemented carbide include a binder phase and a hard phase, the content of the hard phase is 80wt% to 90wt%; the hard phase is tungsten carbide, and the average grain size of the tungsten carbide ranges from 3.4μm to 4.2μm; the hard phase includes tungsten carbide with three grain sizes: coarse, medium and fine. A non-uniform structure cemented carbide roller ring is prepared by matching tungsten carbides of different grain sizes. The toughness and wear resistance of the cemented carbide roller ring are improved simultaneously.

[0006] Although the above methods can prepare non-uniform structure cemented carbide, its non-uniformity is difficult to control, because under high temperature sintering conditions, the added fine-grained WC powder is easy to dissolve and precipitate onto the surrounding coarse WC grains. Therefore, the method of adding fine WC powder may increase the average size of the WC-Co cemented carbide, but cannot make the WC grains present a non-uniform distribution. The non-uniformity of the coarse, medium and fine tungsten carbide powders themselves is difficult to stably and effectively control, resulting in unstable performance of the prepared non-uniform structure alloy. At the same time, tungsten carbide powders of different particle sizes need to be prepared separately, and the production process is cumbersome and costly.

[0007] Therefore, the present invention provides a tungsten carbide powder to solve the problems raised in the above background technology. Summary of the invention

[0008] The object of the present invention is to provide a tungsten carbide powder to solve at least one aspect of the problems and defects mentioned in the above background technology.

[0009] The invention also provides a method for preparing the tungsten carbide powder.

[0010] The invention also provides application of the tungsten carbide powder.

[0011] Specifically, the first aspect of the present invention provides a tungsten carbide powder, which comprises the following components by volume percentage: 19.24% to 35.21% of coarse tungsten carbide, 25.01% to 55.25% of medium tungsten carbide, and 11.32% to 20.38% of fine tungsten carbide;

[0012] The particle size of the coarse tungsten carbide ranges from 10.0 μm to 35.0 μm;

[0013] The particle size range of the medium tungsten carbide is 3.2 μm to 10.0 μm;

[0014] The particle size of the fine tungsten carbide ranges from 0.8 μm to 3.2 μm.

[0015] According to one technical solution of the tungsten carbide powder technical solution of the present invention, at least the following beneficial effects are achieved:

[0016] The invention provides a tungsten carbide powder with multi-level particle sizes. The tungsten carbide powder has coarse, medium and fine tungsten carbides at the same time and is used in non-uniform cemented carbide without adding tungsten carbides of different particle sizes separately, thereby improving the production efficiency of the non-uniform cemented carbide and reducing its production cost.

[0017] The coarse-grained tungsten carbide in the tungsten carbide powder of the present invention can improve the toughness of the cemented carbide, the medium-grained tungsten carbide can improve the stability of the cemented carbide structure, and the fine-grained tungsten carbide can improve the packing density of the cemented carbide, thereby improving the hardness of the cemented carbide.

[0018] The present invention can improve the applicability of tungsten carbide powder in non-uniform cemented carbide by controlling the proportion of each grade of tungsten carbide in tungsten carbide, and can also simultaneously improve the toughness and hardness of the cemented carbide.

[0019] In some specific embodiments of the present invention, the mass ratio of the coarse tungsten carbide, the medium tungsten carbide and the fine tungsten carbide is 0.4-0.8:1:0.2-0.6.

[0020] The invention can improve the toughness and hardness of cemented carbide at the same time by controlling the mass ratio of coarse tungsten carbide, medium tungsten carbide and fine tungsten carbide.

[0021] In some specific embodiments of the present invention, the particle size range of the coarse tungsten carbide includes endpoints of 10.0 μm and 35.0 μm.

[0022] In some specific embodiments of the present invention, the particle size range of the fine tungsten carbide includes endpoints of 0.8 μm and 3.2 μm.

[0023] A second aspect of the present invention provides a method for preparing the above-mentioned tungsten carbide powder, comprising the following steps:

[0024] S1. Reducing tungsten oxide to obtain tungsten powder;

[0025] S2, mixing the tungsten powder and carbon black and carbonizing them to obtain tungsten carbide;

[0026] S3, ball-milling and sieving the tungsten carbide to obtain tungsten carbide powder;

[0027] The carbonization consists of a first stage carbonization, a second stage carbonization and a third stage carbonization.

[0028] According to one technical solution of the cemented carbide technical solution of the present invention, at least the following beneficial effects are achieved:

[0029] The present invention first prepares a tungsten powder with uniform particle size distribution, uses the tungsten powder as a raw material, and carbonizes the tungsten powder through a multi-stage temperature-controlled carbonization method to obtain blocky tungsten carbide. After dry grinding and sieving, multi-level particle size tungsten carbide powder can finally be obtained at one time.

[0030] The present invention reduces tungsten oxide and controls the reduction conditions to obtain tungsten powder with controllable particle size and uniform particle size distribution. The tungsten powder with uniform particle size distribution is beneficial to controlling the growth of tungsten carbide grains in the subsequent carburization process, and is ultimately beneficial to obtaining tungsten carbide powder with multi-level particle sizes.

[0031] The carbonization process of the tungsten powder of the present invention is to first generate a tungsten carbide shell layer on the periphery of the particle, and the surrounding carbon atoms diffuse through the tungsten carbide layer through the gap to reach the junction of the tungsten carbide and the tungsten core, and then react with the tungsten in the inner core to generate ditungsten carbide, and quickly expand to the tungsten core to make the tungsten core disappear. With the continuous diffusion of carbon atoms, they further react with ditungsten carbide to generate tungsten carbide, thus causing the inner extension of the tungsten carbide layer to thicken until the tungsten particles are completely carbonized into single-phase particles. Since the temperature required for each carbon atom to diffuse into the inner core reaction is different during this process, and the temperature also affects the speed of the carbon atoms diffusing inward, the present invention controls the growth of tungsten carbide grains by designing a three-stage carburization, and finally controls to obtain tungsten carbide powders of different particle sizes.

[0032] In some specific embodiments of the present invention, the particle size of the tungsten powder ranges from 1.0 μm to 18.0 μm.

[0033] In the present invention, tungsten powders of different particle sizes are controlled to finally obtain tungsten carbide powders of different average particle sizes. If the particle size of tungsten powder is too small, it is difficult to control tungsten carbide powders of different particle sizes during carburization. If the particle size is too large, the tungsten powder may not be completely carburized, affecting the quality of the tungsten carbide powder.

[0034] In some specific embodiments of the present invention, the reduction temperature is 650° C. to 1100° C.; and the reduction time is 5 h to 9 h.

[0035] The reduction in the present invention is a process of reducing tungsten oxide powder to tungsten powder. By controlling the temperature and time of the reduction, tungsten powders of different particle sizes can be obtained and the particle size distribution of the tungsten powder is uniform.

[0036] In some specific embodiments of the present invention, the reduction is carried out under a hydrogen atmosphere.

[0037] In some specific embodiments of the present invention, the first stage carbonization temperature is 1400°C to 1800°C;

[0038] The first stage carbonization time is 0.5h to 2h.

[0039] In the present invention, the first stage of carburization is the process of forming a tungsten carbide shell on the surface of the tungsten powder particles. By controlling the temperature and time of this stage, each tungsten powder particle can be uniformly provided with a tungsten carbide shell. If the temperature of this stage is too low and the time is too short, the tungsten carbide shell cannot be formed on the surface of most tungsten powder particles, and the subsequent carburization is difficult to control. The tungsten carbide particles finally obtained are too small, and multi-level tungsten carbide powder cannot be obtained. If the temperature of this stage is too high and the time is too long, ditungsten carbide will be formed in the inner layer of most tungsten powder particles, or the tungsten core may disappear without subsequent carburization. Finally, the tungsten carbide particles become abnormally large, and multi-level tungsten carbide powder cannot be obtained.

[0040] In some specific embodiments of the present invention, the second stage carbonization temperature is 1700°C to 2200°C;

[0041] The second stage carbonization time is 1h to 5h.

[0042] In the present invention, the second stage of carburization is that carbon atoms diffuse through the tungsten carbide layer through the gap to reach the junction of tungsten carbide and tungsten core, and then react with the tungsten in the inner core to generate ditungsten carbide. In this stage, due to the uneven diffusion rate of carbon atoms, part of ditungsten carbide will react with carbon to generate fine tungsten carbide particles. If the temperature is too low and the time is too short in this stage, the diffusion rate of carbon atoms will be slow or there will be no time for them to diffuse. Carbon atoms cannot effectively reach the junction of tungsten carbide and tungsten core, and ditungsten carbide cannot be generated, and tungsten carbide fine particles cannot be formed. Finally, multi-level tungsten carbide powder cannot be formed in subsequent carburization. If the temperature is too high and the time is too long in this stage, it will accelerate the conversion of all ditungsten carbide into tungsten carbide, and finally cause the tungsten carbide to grow abnormally large, and multi-level tungsten carbide powder cannot be obtained.

[0043] In some specific embodiments of the present invention, the third stage carbonization temperature is 2000°C to 2400°C;

[0044] The carbonization time of the third stage is 0.5h to 2h.

[0045] In the present invention, the third stage is the process of producing tungsten carbide from ditungsten carbide, and at the same time, the tungsten carbide grows larger. If the temperature is too low and the time is too short in this stage, part of the ditungsten carbide will not react to form tungsten carbide, and the final tungsten carbide powder will be mixed with ditungsten carbide particles, which will affect the powder performance. If the temperature is too high and the time is too long in this stage, the tungsten carbide particles will become too large, and finally, multi-level tungsten carbide powder cannot be obtained.

[0046] In some specific embodiments of the present invention, the mixing time is 3 h to 6 h.

[0047] In some specific embodiments of the present invention, the mixing time is 3 h to 5 h.

[0048] In the present invention, the mixing time is controlled so that the carbon black can be fully coated on the surface of the tungsten powder particles, which is beneficial to the carbonization process. If the time is too short, the carbon black cannot fully coat the tungsten powder particles, and if the time is too long, the production cycle will be increased.

[0049] In some specific embodiments of the present invention, the ball-to-material ratio of the ball milling is 1 to 2:1;

[0050] The ball milling time is 1h-4h.

[0051] A third aspect of the present invention provides an application of tungsten carbide powder in preparing a cemented carbide with a non-uniform structure.

[0052] Compared with the prior art, the present invention has the following beneficial effects:

[0053] 1. The present invention provides a tungsten carbide powder with multiple levels of particle sizes, which can be used to prepare non-uniform structure cemented carbide. During the preparation process, there is no need to add tungsten carbide powder with different levels of particle sizes, which can avoid the need for purchasing raw materials of multiple particle sizes for non-uniform structure cemented carbide, and at the same time, quality accidents caused by possible mistakes in the batching process.

[0054] 2. The present invention prepares tungsten powder with uniform particle size distribution and controls the temperature and time of multi-stage carbonization, and finally can obtain tungsten carbide powder with multi-level particle sizes at one time, with excellent production process control and product performance stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] In order to facilitate understanding by those skilled in the art, the present invention is further described below with reference to the accompanying drawings.

[0056] Figure 1 This is the particle size distribution diagram of the tungsten powder prepared in Example 1.

[0057] Figure 2 This is the SEM image of tungsten powder prepared in Example 1.

[0058] Figure 3 This is the particle size distribution diagram of the tungsten carbide powder prepared in Example 1.

[0059] Figure 4 This is the SEM image of the tungsten carbide powder prepared in Example 1.

[0060] Figure 5 Metallographic image of the non-uniform cemented carbide prepared for the application example. DETAILED DESCRIPTION

[0061] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0062] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0063] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0064] Specific embodiments of the present invention are described in detail below.

[0065] The proportions in Table 1 and Table 2 of the embodiments of the present invention are volume proportions.

[0066] In the embodiments or comparative examples, the carbon black grade is TYJ-P1.

[0067] Specific embodiments of the present invention are described in detail below.

[0068] Example 1

[0069] This embodiment is a tungsten carbide powder, which includes the following components by volume percentage: 29.20% coarse tungsten carbide, 49.24% medium tungsten carbide, and 18.06% fine tungsten carbide;

[0070] The average particle size of the tungsten carbide powder in this embodiment is 6.2.

[0071] The method for preparing tungsten carbide powder in this embodiment comprises the following steps:

[0072] S1. Send tungsten oxide into a reduction furnace for hydrogen reduction at a reduction temperature of 650°C for 5 hours, and obtain a tungsten powder with an average particle size of 1.0 μm;

[0073] S2, mix tungsten powder and carbon black, the mass ratio of the mixture is 16:1, the mixing time is 5h, put the evenly mixed tungsten powder and carbon black into a multi-stage temperature-controlled carbonization furnace for three-stage carbonization, the first stage carbonization temperature is 1400℃, the time is 0.5h, the second stage carbonization temperature is 1700℃, the time is 1h, and the third stage carbonization temperature is 2000℃, the time is 0.5h. Obtain block tungsten carbide;

[0074] S3. Ball-mill the tungsten carbide with a ball-to-material mass ratio of 2:1 for 2 hours, and sieve out the blocky tungsten carbide that is not broken by the ball milling to obtain tungsten carbide powder.

[0075] Figure 1 This is the particle size distribution diagram of the tungsten powder obtained in this embodiment. Figure 2 The SEM image of the tungsten powder prepared in this embodiment is Figure 1 and Figure 2 It can be seen that the prepared tungsten powder has a narrow particle size distribution, uniform particle size, and an average particle size of 1.0 μm.

[0076] Figure 3 This is the particle size distribution diagram of tungsten carbide obtained in this embodiment. Figure 4Table 2 is a SEM image of the tungsten carbide prepared in this embodiment, and Table 3 is a result table of the particle size ratio of the tungsten carbide prepared in this embodiment. Figure 3 and Figure 4 It can be seen that the prepared tungsten carbide has different particle sizes and a wide particle size distribution. There are tungsten carbide grains of coarse, medium and fine multi-level particle sizes. Table 2 shows the volume proportion of tungsten carbide of each level of particle size.

[0077] Example 2

[0078] This embodiment is a tungsten carbide powder, which includes the following components by volume percentage: 32.10% coarse tungsten carbide, 50.08% medium tungsten carbide, and 15.32% fine tungsten carbide;

[0079] The average particle size of the tungsten carbide powder in this embodiment is 12.0 μm.

[0080] The method for preparing tungsten carbide powder in this embodiment comprises the following steps:

[0081] S1. Send tungsten oxide into a reduction furnace for hydrogen reduction at a reduction temperature of 950°C for 6 hours, and obtain a tungsten powder with an average particle size of 10.0 μm;

[0082] S2, mix tungsten powder and carbon black, the mass ratio of the mixture is 16:1, the mixing time is 4h, put the evenly mixed tungsten powder and carbon black into a multi-stage temperature-controlled carbonization furnace for three-stage carbonization, the first stage carbonization temperature is 1600℃, the time is 1h, the second stage carbonization temperature is 1900℃, the time is 2h, and the third stage carbonization temperature is 2200℃, the time is 1h. Obtain block tungsten carbide;

[0083] S3. Ball-mill the tungsten carbide with a ball-to-material mass ratio of 2:1 for 2 hours, and sieve out the blocky tungsten carbide that is not broken by the ball milling to obtain tungsten carbide powder.

[0084] Example 3

[0085] This embodiment is a tungsten carbide powder, which includes the following components by volume percentage: 34.83% coarse tungsten carbide, 49.80% medium tungsten carbide, and 11.87% fine tungsten carbide;

[0086] The average particle size of the tungsten carbide powder in this embodiment is 17.2 μm.

[0087] The method for preparing tungsten carbide powder in this embodiment comprises the following steps:

[0088] S1. Put tungsten oxide into a reduction furnace for hydrogen reduction at a reduction temperature of 1100°C for 8 hours, and obtain tungsten powder with an average particle size of 16.0 μm;

[0089] S2, mix tungsten powder and carbon black, the mass ratio of the mixture is 16:1, the mixing time is 3h, put the evenly mixed tungsten powder and carbon black into a multi-stage temperature-controlled carbonization furnace for three-stage carbonization, the first stage carbonization temperature is 1800℃, the time is 1.5h, the second stage carbonization temperature is 2200℃, the time is 4h, and the third stage carbonization temperature is 2400℃, the time is 1.5h. Obtain block tungsten carbide;

[0090] S3. Ball-mill the tungsten carbide with a ball-to-material mass ratio of 2:1 for 2 hours, and sieve out the blocky tungsten carbide that is not broken by the ball milling to obtain tungsten carbide powder.

[0091] Comparative Example 1

[0092] This comparative example is a tungsten carbide powder, which includes the following components by volume percentage: 4.98% of medium tungsten carbide and 95.02% of fine tungsten carbide;

[0093] The average particle size of the tungsten carbide powder in this comparative example is 1.4 μm.

[0094] The preparation method of tungsten carbide powder in this comparative example consists of the following steps:

[0095] S1. Send tungsten oxide into a reduction furnace for hydrogen reduction at a reduction temperature of 650°C for 5 hours, and obtain a tungsten powder with an average particle size of 1.0 μm;

[0096] S2. Mix tungsten powder and carbon black at a mass ratio of 16:1 for 5 hours. Put the evenly mixed tungsten powder and carbon black into a multi-stage temperature-controlled carbonization furnace for two-stage carbonization. The first-stage carbonization temperature is 1400°C for 1 hour, and the second-stage carbonization temperature is 2000°C for 3 hours.

[0097] Obtaining bulk tungsten carbide;

[0098] S3. Ball-mill the tungsten carbide with a ball-to-material mass ratio of 2:1 for 2 hours, and sieve out the blocky tungsten carbide that is not broken by the ball milling to obtain tungsten carbide powder.

[0099] Comparative Example 2

[0100] This comparative example is a tungsten carbide powder, which includes the following components by volume percentage: 67.89% of coarse tungsten carbide, 43.51% of medium tungsten carbide, and 2.34% of fine tungsten carbide;

[0101] The average particle size of the tungsten carbide powder in this comparative example is 28.3 μm.

[0102] The preparation method of tungsten carbide powder in this comparative example consists of the following steps:

[0103] S1. Put tungsten oxide into a reduction furnace for hydrogen reduction at a reduction temperature of 1300°C for 10 hours, and obtain a tungsten powder with an average particle size of 21.0 μm;

[0104] S2, mix tungsten powder and carbon black, the mass ratio of the mixture is 16:1, the mixing time is 5h, put the evenly mixed tungsten powder and carbon black into a multi-stage temperature-controlled carbonization furnace for three-stage carbonization, the first stage carbonization temperature is 1400℃, the time is 0.5h, the second stage carbonization temperature is 1700℃, the time is 1h, and the third stage carbonization temperature is 2000℃, the time is 0.5h. Obtain block tungsten carbide;

[0105] S3. Ball-mill the tungsten carbide with a ball-to-material mass ratio of 2:1 for 2 hours, and sieve out the blocky tungsten carbide that is not broken by the ball milling to obtain tungsten carbide powder.

[0106] Comparative Example 3

[0107] This comparative example is a tungsten carbide powder, which includes the following components by volume percentage: 71.35% of coarse tungsten carbide and 25.15% of medium tungsten carbide;

[0108] The average particle size of the tungsten carbide powder in this comparative example is 30.2 μm.

[0109] The preparation method of tungsten carbide powder in this comparative example consists of the following steps:

[0110] S1. Put tungsten oxide into a reduction furnace for hydrogen reduction at a reduction temperature of 1100°C for 8 hours, and obtain a tungsten powder with an average particle size of 18.0 μm;

[0111] S2, mix tungsten powder and carbon black, the mass ratio of the mixture is 16:1, the mixing time is 5h, put the evenly mixed tungsten powder and carbon black into a multi-stage temperature-controlled carbonization furnace for three-stage carbonization, the first stage carbonization temperature is 1900℃, the time is 1.5h, the second stage carbonization temperature is 2200℃, the time is 1h, and the third stage carbonization temperature is 2500℃, the time is 4h. Obtain block tungsten carbide;

[0112] S3. Ball-mill the tungsten carbide with a ball-to-material mass ratio of 2:1 for 2 hours, and sieve out the blocky tungsten carbide that is not broken by the ball milling to obtain tungsten carbide powder.

[0113] Application Examples

[0114] This application example is a non-uniform cemented carbide, using the tungsten carbide powder obtained in Example 1 as a raw material.

[0115] The specific preparation is as follows:

[0116] S1, weigh 700kg tungsten carbide powder, 60kg cobalt powder, 18.0kg PEG1500 and 80kg ethanol, mix them, and then wet grind the mixture, the mass ratio of the grinding rod to the mixture is 1:0.6, the speed of wet grinding is 35r / min, and the time is 12h;

[0117] S2, drying the wet-milled raw material at 90° C. for 5 h, granulating, and pressing to form a green body;

[0118] S3. Sinter the green body at 1450°C for 2 hours to obtain a non-uniform cemented carbide.

[0119] The Rockwell hardness of the inhomogeneous cemented carbide was measured to be 87.9HRA.

[0120] The bending strength of the inhomogeneous cemented carbide was measured to be 2250 MPa.

[0121] The obtained non-uniform cemented carbide was subjected to metallographic examination. Figure 5 .

[0122] Hardness test reference: GB / T3849.1-2015 Cemented Carbide Rockwell Hardness (A Scale) Part 1: Experimental Method.

[0123] Bending strength test reference: GB / T3851-2015 Cemented carbide transverse fracture strength determination method.

[0124] It can be seen from the test results that the tungsten carbide powder prepared by the technical solution of the present invention is used as a raw material, and a non-uniform cemented carbide can be prepared without adding tungsten carbide of various grades. The prepared non-uniform cemented carbide has good hardness and toughness.

[0125] The particle size of the tungsten carbide powders obtained in Examples 1 to 3 and Comparative Examples 1 to 3 was tested. The results are shown in Table 1.

[0126] Table 1 Results of the particle size ratios of tungsten carbides obtained in Examples 1 to 3 and Comparative Examples 1 to 3

[0127]

[0128]

[0129] Table 2 Volume percentage of each particle size of tungsten carbide obtained in Example 1

[0130]

[0131] It can be seen from Table 1 that, under the premise of reasonably controlling the reduction temperature and time, three-stage carbonization is adopted, and the carbonization temperature and carbonization time of each time are reasonably controlled, coarse, medium and fine tungsten carbide powders of multiple levels can be obtained.

[0132] Although Comparative Example 2 can also obtain tungsten carbide of three different particle sizes, the content of fine tungsten carbide is too small.

[0133] In summary, the present invention provides a tungsten carbide powder with multi-level particle sizes, which can be used to prepare non-uniform structure cemented carbide. During the preparation process, there is no need to add tungsten carbide powder with different levels of particle sizes, which can avoid the need for purchasing raw materials of various particle sizes for non-uniform alloys, and at the same time, quality accidents caused by possible mistakes in the batching process; the present invention also provides a method for preparing the tungsten carbide powder, by preparing tungsten powder with uniform particle size distribution, controlling the temperature and time of multi-stage carbonization, and finally obtaining tungsten carbide powder with multi-level particle sizes at one time, with excellent production process control and product performance stability.

[0134] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing tungsten carbide powder, characterized in that: The following steps are involved: S1. Reducing tungsten oxide to obtain tungsten powder; S2, mixing the tungsten powder and carbon black and carbonizing them to obtain tungsten carbide; S3, ball-milling and sieving the tungsten carbide to obtain tungsten carbide powder; The carbonization consists of a first stage carbonization, a second stage carbonization and a third stage carbonization; The tungsten carbide powder obtained in step S3 includes the following components by volume percentage: 19.24% to 35.21% of coarse tungsten carbide, 25.01% to 55.25% of medium tungsten carbide, and 11.32% to 20.38% of fine tungsten carbide; The particle size range of the coarse tungsten carbide is 10.0 μm to 35.0 μm; The particle size range of the medium tungsten carbide is 3.2 μm to 10.0 μm; The particle size of the fine tungsten carbide ranges from 0.8 μm to 3.2 μm; The reduction temperature is 650°C to 1100°C; The reduction time is 5h~9h; The temperature of the first stage carbonization is 1400°C to 1600°C; The first stage carbonization time is 0.5h~2h; The temperature of the second stage carbonization is 1700°C~1900°C; The second stage carbonization time is 1h~5h; The temperature of the third stage carbonization is 2000°C to 2400°C; The third stage carbonization time is 0.5h~2h.

2. The method for preparing tungsten carbide powder according to claim 1, characterized in that: The average particle size of the tungsten powder is 1.0 μm to 18.0 μm.

3. The method for preparing tungsten carbide powder according to claim 1, characterized in that: The ball-to-material ratio of the ball mill is 1-2:1; The ball milling time is 1h-4h.