Black weather-resistant layer, photovoltaic module and colored photovoltaic module

By using black weathering layer and reinforced film layer in photovoltaic modules, the insufficient safety performance of photovoltaic modules under high temperature conditions and the diversity of appearance of color photovoltaic modules is solved, and efficient, safe and beautiful photovoltaic modules are achieved.

CN116082777BActive Publication Date: 2024-12-03LONGI SOLAR TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310076621.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-02-10
Filing Date
2023-01-19
Publication Date
2024-12-03
Estimated Expiration
2043-01-19

AI Technical Summary

Technical Problem

Existing photovoltaic modules lack safety performance under high temperature conditions, and color photovoltaic modules are difficult to meet the diverse appearance needs of buildings, and photovoltaic cells are low in efficiency.

Method used

A black weathering layer is adopted, including a weathering resin substrate, a black color material, a filler and a curing agent, with low visible light reflectivity and high infrared light reflectivity, and a reinforced adhesive layer is provided in the photovoltaic module to improve the elastic mode of the adhesive layer. , and the amount and intensity are achieved through colored glaze and transparent film layers.

Benefits of technology

It improves the safety and aesthetics of photovoltaic modules under high temperature conditions, while improving power generation efficiency, ensuring the safety performance and appearance diversity of components in building applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004067084830000211
    Figure BDA0004067084830000211
  • Figure BDA0004067084830000221
    Figure BDA0004067084830000221
  • Figure BDA0004067084830000222
    Figure BDA0004067084830000222
Patent Text Reader

Abstract

The present application discloses a black weather-resistant layer, comprising the following components: 80-100 parts of a weather-resistant resin substrate, 40-120 parts of a solvent, 10-50 parts of a black colorant, 5-20 parts of a filler, 1-20 parts of a silane coupling agent, 3-30 parts of a curing agent, and 1-5 parts of an auxiliary agent. The present application also provides a photovoltaic module and a color photovoltaic module. The photovoltaic module provided in the present application, due to the effect of the strengthening film layer, the internal film layer of the photovoltaic module still has a high elastic modulus and strength under normal working high temperature conditions, so that the photovoltaic module has a higher safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular to a black weather-resistant layer, a photovoltaic module and a color photovoltaic module. Background Art

[0002] As a tool for receiving and converting light energy, photovoltaic modules have become highly efficient after long-term technological updates and iterations, and have been widely used in large-scale ground power stations. With the increase in the number of photovoltaic installations, the use of ground resources has tended to be saturated, and a large amount of building area as the receiving surface of sunlight is the best choice for installing photovoltaics. Installing photovoltaics on buildings can increase energy income on the one hand, and reduce building energy consumption on the other hand. At the same time, buildings can generate electricity for their own use, reducing the loss of long-distance power transmission. However, photovoltaic cells are usually dark blue or black in color, which is relatively monotonous and cannot meet the diverse appearance requirements of buildings. Among the photovoltaic cell technologies, there are thin-film battery technologies, such as cadmium telluride, copper indium gallium selenide, etc., which are generally less efficient. As a mature photovoltaic power generation technology, crystalline silicon has now reached an efficiency of more than 24% in mass production, so it is the preferred technology for building photovoltaic integration. Methods to achieve the diversified color requirements of photovoltaic modules include adding inorganic or organic pigments to the film, such as colored film. On the one hand, this method will greatly reduce the efficiency of photovoltaic modules due to the absorption of light by pigments, and on the other hand, there is a risk of fading, which is not a good choice for the color of photovoltaic modules. There is also a method of applying a colored coating layer on the surface of the battery cell, but this method is difficult to control the thickness of the coating layer, the color is difficult to achieve uniformity, and the appearance is ugly.

[0003] On the other hand, when photovoltaic modules are used in buildings, especially on facades, their safety performance is a very important control performance. As a kind of laminated glass, photovoltaic modules are not easy to fall from a height due to the presence of the encapsulation film after being broken, so they have certain safety properties. The strength of this safety property is directly related to the characteristics of the encapsulation film used, especially the elastic modulus. Commonly used encapsulation films include EVA, POE, PVB, etc. The physical properties of these films are that their elastic modulus gradually decreases with the increase of temperature. EVA, POE, and PVB all have a glass transition point lower than normal temperature. When the temperature is higher than 50°C, their elastic modulus will drop significantly. Its strength is so weak that it can be ignored compared with glass. However, as an electrical unit, when photovoltaic modules are exposed to the sun to generate electricity outdoors, their operating temperature will be 30 to 40 degrees Celsius higher than the ambient temperature. For example, in summer, the temperature can reach 80°C or even higher. At this temperature, the strength of the EVA, POE, PVB and other encapsulation films inside the photovoltaic modules will be very low. If the modules are damaged by external forces at this time, the damaged modules may fall and injure people under their own weight. In summer, there is a high incidence of extreme weather such as hail and strong winds, so the risk is very high. Summary of the invention

[0004] In view of the above problems, the present application proposes a black weather-resistant layer that can absorb visible light and has a high reflectivity for infrared light, a photovoltaic module, and a color photovoltaic module having the black weather-resistant layer.

[0005] The present application provides a black weather-resistant layer, comprising the following components:

[0006] The weather-resistant resin base material is 80-100 parts, the solvent is 40-120 parts, the black colorant is 10-50 parts, the filler is 5-20 parts, the silane coupling agent is 1-20 parts, the curing agent is 3-30 parts, and the auxiliary agent is 1-5 parts.

[0007] Further, the weather-resistant resin substrate is selected from at least one of acrylic resin, polyester resin, fluorocarbon resin, epoxy resin, vinylidene fluoride, trifluoroethylene-vinyl ether copolymer, trifluoroethylene-vinyl ester copolymer, tetrafluoroethylene-vinyl ether copolymer and isocyanate, preferably acrylic resin or fluorocarbon resin;

[0008] The solvent is selected from at least one of toluene, xylene, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone and N-methyl pyrrolidone, preferably butyl acetate;

[0009] The black colorant is at least one selected from iron chrome black, iron chrome black, copper chrome black, iron manganese black, aniline black, and perylene black, preferably iron chrome black;

[0010] The filler is selected from at least one of glass powder, ceramic powder, white carbon black and alumina, preferably white carbon black;

[0011] The curing agent is at least one of an isocyanate curing agent, an imidazole curing agent, an amine curing agent and a dicyandiamide curing agent, preferably an isocyanate curing agent;

[0012] The silane coupling agent is selected from at least one of γ-aminopropyl triethoxysilane, γ-glycidyl ether aminopropyl trimethoxysilane, and γ-methacryloxy-propyl trimethoxysilane, preferably γ-aminopropyl triethoxysilane;

[0013] The auxiliary agent is selected from one of emulsified silicone oil, high carbon alcohol fatty acid ester complex, polyoxyethylene polyoxypropylene pentaerythritol ether, polyoxyethylene polyoxypropanolamine ether, polyoxypropylene glycerol ether, polyoxypropylene polyoxyethylene glycerol ether or polydimethylsiloxane; preferably polydimethylsiloxane.

[0014] Furthermore, the particle size of the black colorant is 5-50 μm; and the particle size of the filler is 1-5 μm.

[0015] Furthermore, the black weather-resistant layer is a grid-shaped film layer.

[0016] Furthermore, the black weather-resistant layer has a reflectivity lower than 10% for visible light and a reflectivity higher than 30% for infrared light with a wavelength of more than 750 nm.

[0017] The present application provides a photovoltaic module, comprising a back plate, a first lower flexible film layer, a strengthening film layer, a second lower flexible film layer, a battery sheet layer and a front plate which are stacked in sequence.

[0018] Furthermore, the first lower flexible adhesive film layer and the second lower flexible adhesive film layer are both selected from one of an EVA film layer, a POE film layer, a PVB film layer or an SGP film layer;

[0019] The thickness of the first lower flexible film layer is 0.1-2 mm;

[0020] The thickness of the second lower flexible adhesive film layer is 0.1-2 mm.

[0021] Furthermore, the reinforcing film layer is one of a PET film layer, a PU film layer, a nylon layer or a metal mesh layer;

[0022] The thickness of the strengthening film layer is 0.1-1 mm.

[0023] Furthermore, a black weather-resistant layer is provided at any position on the surface of the backplane facing away from the first lower flexible film layer, between the backplane and the first lower flexible film layer, between the first lower flexible film layer and the strengthening film layer, between the strengthening film layer and the second lower flexible film layer, and between the second lower flexible film layer and the battery cell.

[0024] Furthermore, the backplane is one of a glass backplane, a metal backplane, an organic backplane, an inorganic backplane or a composite material backplane.

[0025] Furthermore, the front plate is an upper colored glass layer or an upper transparent layer.

[0026] Furthermore, the photovoltaic module comprises a back glass layer, a first lower flexible adhesive film layer, a strengthening adhesive film layer, a second lower flexible adhesive film layer, a battery layer and an upper colored glass layer which are stacked in sequence.

[0027] Furthermore, the black weather-resistant layer is the black weather-resistant layer described above.

[0028] The present application provides a color photovoltaic module, comprising a back glass layer, a film layer, a cell layer and an upper color glass layer stacked in sequence;

[0029] A black weather-resistant layer is provided on a surface of the back glass layer facing away from the adhesive film layer, between the back glass layer and the adhesive film layer, between the adhesive film layer and the battery cell, or in the adhesive film layer;

[0030] The reflectivity of the black weather-resistant layer to visible light is lower than 10%, and the reflectivity to infrared light with a wavelength of more than 750nm is higher than 30%.

[0031] Furthermore, the adhesive film layer is composed of an adhesive film, and the adhesive film is selected from any one of a single-layer adhesive film, a two-layer adhesive film, a three-layer adhesive film, or the above.

[0032] Furthermore, the adhesive film is a flexible adhesive film or a reinforced adhesive film or a laminated adhesive film of a flexible adhesive film and a reinforced adhesive film;

[0033] The reinforced adhesive film layer is one of a PET film layer, a PU film layer, a nylon layer or a metal mesh layer;

[0034] The thickness of the strengthening film layer is 0.1-1 mm.

[0035] Furthermore, the adhesive film layer is a first lower flexible adhesive film layer, a strengthening adhesive film and a second lower flexible adhesive film layer which are stacked in sequence.

[0036] Furthermore, the adhesive film layer is a first lower flexible adhesive film layer, a strengthening adhesive film, a black weather-resistant layer and a second lower flexible adhesive film layer which are stacked in sequence.

[0037] Furthermore, the upper colored glass layer includes an upper film layer, a colored glaze layer and a front glass layer arranged in sequence from bottom to top, and a surface of the upper film layer facing away from the colored glaze layer is connected to the battery cell layer.

[0038] Furthermore, the upper adhesive film layer is a colorless and transparent adhesive film layer, and its thickness is 0.1-2 mm.

[0039] Furthermore, the upper colored glass layer includes an upper adhesive film layer and a front glass layer which are arranged in sequence, and a surface of the upper adhesive film layer which faces away from the front glass layer is connected to the battery cell layer.

[0040] Furthermore, the upper adhesive film layer is a colored transparent adhesive film layer, and its thickness is 0.1-2 mm.

[0041] Furthermore, the front glass layer is transparent glass with a thickness of 1-16 mm.

[0042] Furthermore, an anti-reflection layer is provided on one side surface of the front glass layer.

[0043] Furthermore, the black weather-resistant layer is the black weather-resistant layer according to any one of claims 1 to 5.

[0044] The present application also provides a method for preparing a color photovoltaic device, comprising the following steps:

[0045] Provides a back glass layer,

[0046] Providing a three-layer composite film, the three-layer composite film comprising a first lower flexible adhesive film layer, a strengthening adhesive film layer and a second lower flexible adhesive film layer stacked together in sequence;

[0047] Laying the first lower flexible adhesive film layer and the back glass layer together;

[0048] Arranging a battery sheet layer on a surface of the second lower flexible adhesive film layer facing away from the strengthening adhesive film layer;

[0049] The upper material glass layer is disposed on a surface of the battery layer on a side away from the second lower flexible adhesive film layer.

[0050] Furthermore, after the two surfaces of the strengthening film layer are subjected to corona treatment, they are respectively pressed with the first lower flexible film layer and the second lower flexible film layer to form the three-layer composite film.

[0051] The black weather-resistant layer provided in the present application can absorb visible light and has a high reflectivity for infrared light.

[0052] The photovoltaic module provided in the present application has the effect of the reinforced film layer, so that the internal film layer of the photovoltaic module still has a high elastic modulus and strength under high temperature conditions of normal operation, thereby making the photovoltaic module have higher safety.

[0053] In the color photovoltaic module described in the present application, after the two surfaces of the strengthening film layer are corona treated, they are pressed together with the first lower flexible film layer and the second lower flexible film layer respectively, so as to ensure high interlayer bonding ability.

[0054] The colored photovoltaic module described in the present application can absorb visible light through the black weather-resistant layer, thereby avoiding the different reflection of incident light between the cell area and the cell gap area, which leads to uneven color rendering of the overall photovoltaic module, color difference or inability to render color, thereby affecting the overall aesthetics. The addition of the black weather-resistant layer absorbs visible light, thereby ensuring the overall color rendering and aesthetics of the photovoltaic module. At the same time, the black weather-resistant layer has a high reflectivity for infrared light, and the infrared light reflected by the black weather-resistant layer can be absorbed by the cell layer. Therefore, the photovoltaic module described in the present application further improves the power generation efficiency of the photovoltaic module when realizing color. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] The accompanying drawings are used to better understand the present application and do not constitute an improper limitation on the present application.

[0056] Figure 1 Schematic diagram of the structure of the color photovoltaic module provided for this application.

[0057] Figure 2 Schematic diagram of the structure of the color photovoltaic module provided for this application.

[0058] Figure 3 This is a curve diagram of the transmittance and monochromatic reflectivity of the color photovoltaic module of Example 1 of the present application.

[0059] Figure 4 Schematic diagram of the structure of the color photovoltaic module provided for this application.

[0060] Figure 5 Schematic diagram of the structure of the color photovoltaic module provided for this application.

[0061] Figure 6 Schematic diagram of the structure of the color photovoltaic module provided for this application.

[0062] Description of Reference Numerals

[0063] 1-front glass layer, 2-colored glaze layer, 3-upper film layer, 4-cell layer, 5-second lower flexible film layer, 6-strengthening film layer, 7-first lower flexible film layer, 8-back glass layer, 9-black weather-resistant layer. DETAILED DESCRIPTION

[0064] The following is a description of exemplary embodiments of the present application, including various details of the embodiments of the present application to facilitate understanding, which should be considered as merely exemplary. Therefore, it should be recognized by those of ordinary skill in the art that various changes and modifications can be made to the embodiments described herein without departing from the scope and spirit of the present application. Similarly, for clarity and conciseness, the description of well-known functions and structures is omitted in the following description. In the present application, the upper and lower positions are determined according to the incident direction of the light, and the place where the light is incident is the upper part.

[0065] The present application provides a black weather-resistant layer, comprising the following components: 80-100 parts of a weather-resistant resin substrate, 40-120 parts of a solvent, 10-50 parts of a black colorant, 5-20 parts of a filler, 1-20 parts of a silane coupling agent, 3-30 parts of a curing agent, and 1-5 parts of an auxiliary agent.

[0066] In the present application, the raw materials of the black weather-resistant layer 9 are composed of 80-100 parts of weather-resistant resin base material, 40-120 parts of solvent, 10-50 parts of black colorant, 5-20 parts of filler, 1-20 parts of silane coupling agent, 3-30 parts of curing agent, and 1-5 parts of auxiliary agent.

[0067] The black weather-resistant layer 9 is formed by mixing 80-100 parts of a weather-resistant resin substrate, 40-120 parts of a solvent, 10-50 parts of a black colorant, 5-20 parts of a filler, 1-20 parts of a silane coupling agent, 3-30 parts of a curing agent, and 1-5 parts of an auxiliary agent, and then heating and curing.

[0068] Specifically, the mass ratio of the weather-resistant resin substrate, solvent, black colorant, filler, silane coupling agent, curing agent and auxiliary agent is (80-100): (40-120): (10-50): (5-20): (1-20): (3-30): (1-5).

[0069] More specifically, the mass ratio of the weather-resistant resin substrate, the solvent and the black colorant can be 80:40:10, 80:50:10, 80:60:10, 80:70:10, 80:80:10, 80:90:10, 80:100:10, 80:110:10, 80:120:10, 80:40:20, 80:40:30, 80:40:40, 80:40:50, 90:40:10, 90:40:10, 90:40:10, 90:50:20, 90:50:30, 90:50:40, 90:50:50, 90:60:20, 90:60:30, 90:60:40. 0, 90:60:50, 90:70:20, 90:70:30, 90:70:40, 90:70:50, 90:80:20, 90:80:30, 90:80:40, 90:80:50, 90:90:20, 90:90:30, 90:90:40, 90:90:50, 90:100:20, 90:100:30, 90:100:40, 90:100:50, 90:110:20, 90:110:30, 90:110:40, 90:110:50, 90:120:20, 90:120:30, 90:120:40, 90:120:50.

[0070] The weather-resistant resin substrate is selected from at least one of acrylic resin, polyester resin, fluorocarbon resin, epoxy resin, polyvinylidene fluoride (PVDF), trifluoroethylene-vinyl ether copolymer, trifluoroethylene-vinyl ester copolymer, tetrafluoroethylene-vinyl ether copolymer and isocyanate, preferably acrylic resin or fluorocarbon resin.

[0071] The solvent is at least one of toluene, xylene, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone and N-methyl pyrrolidone; preferably butyl acetate.

[0072] The black pigment is at least one of iron chrome black, copper chrome black, iron manganese black, aniline black and perylene black, preferably iron chrome black, more preferably a precursor with a Fe / Cr molar ratio of 0.5, formed by calcining at 900°C to form a high-crystallinity Cr 1.3 Fe 0.7 Iron chrome black with O3 as the main crystal phase.

[0073] The particle size of the black colorant is 5-50 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm or 50 μm.

[0074] The filler is at least one of glass powder, ceramic powder, white carbon black and alumina, preferably white carbon black. The particle size of the filler is 1-5 μm, for example, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm.

[0075] The curing agent is at least one of an isocyanate curing agent, an imidazole curing agent, an amine curing agent and a dicyandiamide curing agent, preferably an isocyanate curing agent;

[0076] The silane coupling agent is selected from one or more of γ-aminopropyltriethoxysilane, γ-glycidyl ether aminopropyltrimethoxysilane, and γ-methacryloxy-propyltrimethoxysilane, preferably γ-aminopropyltriethoxysilane.

[0077] The auxiliary agent is selected from one or more of emulsified silicone oil, high carbon alcohol fatty acid ester complex, polyoxyethylene polyoxypropylene pentaerythritol ether, polyoxyethylene polyoxypropanolamine ether, polyoxypropylene glycerol ether, polyoxypropylene polyoxyethylene glycerol ether, and polydimethylsiloxane; preferably polydimethylsiloxane.

[0078] In the present application, the black weather-resistant layer 9 is any film layer having a grid shape.

[0079] In the present application, the reflectivity of the black weather-resistant layer 9 to visible light is lower than 10%, preferably lower than 5%. For example, the reflectivity of the black weather-resistant layer 9 to visible light can be 10%, 8%, 5%, 4%, 3%, 2%, 1%, etc.

[0080] Specifically, the reflectivity of the black weather-resistant layer 9 to infrared light with a wavelength of more than 750 nm is higher than 30%. For example, the reflectivity of the black weather-resistant layer 9 to infrared light with a wavelength of more than 750 nm can be 30%, 40%, 50%, 60%, 70%, 80%, etc.

[0081] Since the black weather-resistant layer 9 can reflect infrared light, when it is applied to a photovoltaic module, the absorption of infrared light by the photovoltaic module can be further reduced, thereby reducing the operating temperature of the photovoltaic module. Moreover, the infrared light with a wavelength of 800-1100 reflected by the black weather-resistant layer 9 can be absorbed by the cell layer 4 in the photovoltaic module. Since the cell layer 4 is a solar cell layer, the energy conversion efficiency of the solar cell layer can be improved.

[0082] Existing photovoltaic modules mainly use EVA or POE as packaging materials. This packaging structure can meet the reliability requirements of photovoltaics. However, due to the low elastic modulus and tensile strength of EVA and POE, they cannot meet the requirements of anti-flexural deformation and safety performance of photovoltaic laminated glass in building application scenarios such as curtain walls and skylights. Among them, safety performance is the key performance requirement of buildings for laminated glass. Laminated glass in buildings is usually encapsulated with PVB, so the packaging material of curtain wall photovoltaic modules is also required to be encapsulated with PVB. However, since the actual operation of photovoltaic modules is due to the internal current, and most of the sunlight entering the photovoltaic modules cannot be converted into electrical energy, but into thermal energy, a large amount of heat will be generated, and the heat dissipation speed will not be very fast. Therefore, the temperature of the module in actual operation will be much higher than the ambient temperature. At an ambient temperature of 25°C, the temperature inside the module may reach above 50°C. When the ambient temperature rises and the amount of sunlight radiation is large, it can reach up to above 80°C. As elastic-plastic polymer materials, EVA, POE and PVB have a significantly lower elastic modulus when the temperature is above 25°C. When the temperature is above 50°C, the elastic modulus of EVA, POE and PVB all drop below 2MPa, which is much lower than the elastic modulus of glass (70GPa). In this normalized high-temperature environment, the bending modulus of photovoltaic laminated glass also drops significantly, and the safety properties of safety glass also lose their meaning due to the significant drop in film modulus and strength at high temperatures. (In this application, photovoltaic modules are also referred to as photovoltaic devices.)

[0083] Based on this, the present application provides a photovoltaic module, which includes a backplane, a first lower flexible film layer 7, a strengthening film layer 6, a second lower flexible film layer 5, a battery layer 4 and a front panel stacked in sequence.

[0084] Specifically, the backplane is one of a glass backplane, a metal backplane, an organic backplane, an inorganic backplane or a composite material backplane.

[0085] Specifically, the front plate is an upper colored glass layer or an upper transparent layer.

[0086] When the front plate is the upper transparent layer, the photovoltaic module is a conventional colorless or black photovoltaic module, and can also be called a photovoltaic device. That is, the transparent photovoltaic module includes a back plate, a first lower flexible film layer 7, a strengthening film layer 6, a second lower flexible film layer 5, a cell layer 4 and an upper transparent layer stacked in sequence.

[0087] When the front plate is an upper colored glass layer, the photovoltaic module is a colored photovoltaic module, which can also be called a colored photovoltaic device. That is, the colored photovoltaic module includes a back plate, a first lower flexible adhesive film layer 7, a strengthening adhesive film layer 6, a second lower flexible adhesive film layer 5, a cell layer 4 and an upper colored glass layer stacked in sequence.

[0088] A black weather-resistant layer is provided at any one position of the surface of the backplane facing away from the first lower flexible film layer, between the backplane and the first lower flexible film layer, between the first lower flexible film layer and the strengthening film layer, between the strengthening film layer and the second lower flexible film layer, and between the second lower flexible film layer and the battery cell. (The black weather-resistant layer can refer to the description of the black weather-resistant layer above)

[0089] The first lower flexible film layer 7, the strengthening film layer 6, the second lower flexible film layer 5, and the battery cell layer 4 can refer to the description of the first lower flexible film layer 7, the strengthening film layer 6, the second lower flexible film layer 5, and the battery cell layer 4 in the following color photovoltaic module.

[0090] The present application provides a color photovoltaic module, comprising a back glass layer 8, a film layer, a cell layer 4 and an upper color glass layer stacked in sequence;

[0091] A black weather-resistant layer 9 is provided on the surface of the back glass layer 8 facing away from the adhesive film layer, between the back glass layer 8 and the adhesive film layer, between the adhesive film layer and the battery cell, or in the adhesive film layer;

[0092] The reflectivity of the black weather-resistant layer 9 to visible light is lower than 10%, and the reflectivity to infrared light with a wavelength of more than 750 nm is higher than 30%.

[0093] Specifically, the color photovoltaic module includes a black weather-resistant layer 9, a back glass layer 8, an adhesive film layer, a cell layer 4 and an upper color glass layer which are stacked in sequence.

[0094] Specifically, the color photovoltaic module includes a back glass layer 8, a black weather-resistant layer 9, a film layer, a cell layer 4 and an upper color glass layer which are stacked in sequence.

[0095] Specifically, the color photovoltaic module includes a back glass layer 8, a film layer, a black weather-resistant layer 9, a cell layer 4 and an upper color glass layer which are stacked in sequence.

[0096] Specifically, the color photovoltaic module includes a back glass layer 8, an adhesive film layer, a cell layer 4 and an upper color glass layer which are stacked in sequence, and a black weather-resistant layer 9 is arranged in the adhesive film layer.

[0097] In the present application, the adhesive film layer is composed of an adhesive film, and the adhesive film is selected from a single-layer adhesive film, a two-layer adhesive film, a three-layer adhesive film, or any one of the above.

[0098] Specifically, the adhesive film is a flexible adhesive film or a reinforced adhesive film or a laminated adhesive film of a flexible adhesive film and a reinforced adhesive film.

[0099] Specifically, the adhesive film layer is a first lower flexible adhesive film layer 7 , a strengthening adhesive film layer 6 , and a second lower flexible adhesive film layer 5 which are stacked in sequence.

[0100] Specifically, the adhesive film layer is a first lower flexible adhesive film layer 7, a strengthening adhesive film layer 6, a black weather-resistant layer 9 and a second lower flexible adhesive film layer 5 which are stacked in sequence.

[0101] Specifically, the adhesive film layer is a first lower flexible adhesive film layer 7, a black weather-resistant layer 9, a strengthening adhesive film layer 6 and a second lower flexible adhesive film layer 5 which are stacked in sequence.

[0102] In a specific embodiment, the colored photovoltaic module includes a black weather-resistant layer 9, a back glass layer 8, a first lower flexible film layer 7, a strengthening film layer 6, a second lower flexible film layer 5, a cell layer 4 and an upper colored glass layer stacked in sequence.

[0103] In a specific embodiment, the colored photovoltaic module includes a back glass layer 8, a black weather-resistant layer 9, a first lower flexible film layer 7, a strengthening film layer 6, a second lower flexible film layer 5, a cell layer 4 and an upper colored glass layer stacked in sequence.

[0104] In a specific embodiment, the colored photovoltaic module includes a back glass layer 8, a first lower flexible film layer 7, a strengthening film layer 6, a second lower flexible film layer 5, a black weather-resistant layer 9, a cell layer 4 and an upper colored glass layer stacked in sequence.

[0105] In a specific embodiment, Figure 1 As shown, the colored photovoltaic module includes a back glass layer 8, a first lower flexible film layer 7, a strengthening film layer 6, a second lower flexible film layer 5, a cell layer 4 and an upper colored glass layer stacked in sequence from bottom to top. A black weather-resistant layer 9 is coated on the surface of the strengthening film layer 6 on one side close to the second lower flexible film layer 5.

[0106] The back glass layer 8 is transparent glass, and its thickness can be 1-18 mm, for example, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, 16 mm, 17 mm, or 18 mm.

[0107] In the present application, the first lower flexible adhesive film layer 7 and the second lower flexible adhesive film layer 5 are both selected from one of an EVA film layer, a POE film layer, a PVB film layer or an SGP film layer;

[0108] Specifically, the first lower flexible adhesive film layer 7 and the second lower flexible adhesive film layer 5 may be the same film layer or different film layers.

[0109] In a specific embodiment, the first lower flexible adhesive film layer 7 is an EVA film layer, and the second lower flexible adhesive film layer 5 is an EVA film layer.

[0110] In a specific embodiment, the first lower flexible adhesive film layer 7 is an EVA film layer, and the second lower flexible adhesive film layer 5 is a POE film layer.

[0111] In a specific embodiment, the first lower flexible adhesive film layer 7 is an EVA film layer, and the second lower flexible adhesive film layer 5 is an SGP film layer.

[0112] In a specific embodiment, the first lower flexible adhesive film layer 7 is a POE film layer, and the second lower flexible adhesive film layer 5 is an EVA film layer.

[0113] In a specific embodiment, the first lower flexible adhesive film layer 7 is a POE film layer, and the second lower flexible adhesive film layer 5 is a POE film layer.

[0114] In a specific embodiment, the first lower flexible adhesive film layer 7 is a POE film layer, and the second lower flexible adhesive film layer 5 is a SGP film layer.

[0115] In a specific embodiment, the first lower flexible adhesive film layer 7 is a PVB film layer, and the second lower flexible adhesive film layer 5 is a PVB film layer.

[0116] In a specific embodiment, the first lower flexible adhesive film layer 7 is a SGP film layer, and the second lower flexible adhesive film layer 5 is a SGP film layer.

[0117] In the present application, the thickness of the first lower flexible film layer 7 and the second lower flexible film layer 5 are both 0.1-2 mm; for example, it can be 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm or 2 mm.

[0118] In the present application, the reinforced film layer 6 is one of a PET film layer, a PU film layer, a nylon layer or a metal mesh layer; the thickness of the reinforced film layer 6 is 0.1-1mm, for example, it can be 0.1mm, 0.2mm, 0.3mm, 0.4mm, 0.5mm, 0.6mm, 0.7mm, 0.8mm, 0.9mm or 1mm.

[0119] The black weather-resistant layer 9 can absorb visible light, thereby avoiding different reflections of incident light between the cell area and the cell gap area, resulting in uneven color rendering of the overall photovoltaic module, color difference or inability to render color, thereby affecting the overall aesthetics. The addition of the black weather-resistant layer will absorb visible light, thereby ensuring the overall color rendering and aesthetics of the photovoltaic module. At the same time, since the black weather-resistant layer 9 has a high reflectivity for infrared light, the infrared light reflected by the black weather-resistant layer 9 can be absorbed by the cell layer 4. Therefore, the color photovoltaic module described in the present application further improves the power generation efficiency of the photovoltaic module when realizing color.

[0120] Specifically, the reflectivity of the reinforced adhesive film layer 6 coated with the black weather-resistant layer 9 to visible light is lower than 10%, preferably lower than 5%. For example, the reflectivity of the black weather-resistant layer 9 to visible light can be 10%, 8%, 5%, 4%, 3%, 2%, 1%, etc.

[0121] Specifically, the reflectivity of the reinforced adhesive film layer 6 coated with the black weather-resistant layer 9 for infrared light with a wavelength of more than 750nm is higher than 30%. For example, the reflectivity of the reinforced adhesive film layer 6 coated with the black weather-resistant layer 9 for infrared light with a wavelength of more than 750nm can be 30%, 40%, 50%, 60%, 70%, 80%, etc.

[0122] Since the black weather-resistant layer 9 can reflect infrared light, the absorption of infrared light by the device can be further reduced, thereby reducing the operating temperature of the device, and the infrared light with a wavelength of 800-1100 reflected by the black weather-resistant layer 9 can be absorbed by the cell layer 4. Since the cell layer 4 is a solar cell layer 4, the energy conversion efficiency of the solar cell layer 4 can be improved.

[0123] In the present application, the raw materials of the black weather-resistant layer 9 include: 80-100 parts of weather-resistant resin substrate, 40-120 parts of solvent, 10-50 parts of black colorant, 5-20 parts of filler, 1-20 parts of silane coupling agent, 3-30 parts of curing agent, and 1-5 parts of auxiliary agent.

[0124] In the present application, the raw materials of the black weather-resistant layer 9 are composed of 80-100 parts of weather-resistant resin base material, 40-120 parts of solvent, 10-50 parts of black colorant, 5-20 parts of filler, 1-20 parts of silane coupling agent, 3-30 parts of curing agent, and 1-5 parts of auxiliary agent.

[0125] The black weather-resistant layer 9 is formed by mixing 80-100 parts of a weather-resistant resin substrate, 40-120 parts of a solvent, 10-50 parts of a black colorant, 5-20 parts of a filler, 1-20 parts of a silane coupling agent, 3-30 parts of a curing agent, and 1-5 parts of an auxiliary agent, and then heating and curing.

[0126] Specifically, the mass ratio of the weather-resistant resin substrate, solvent, black colorant, filler, silane coupling agent, curing agent and auxiliary agent is (80-100): (40-120): (10-50): (5-20): (1-20): (3-30): (1-5).

[0127] More specifically, the mass ratio of the weather-resistant resin substrate, the solvent and the black colorant can be 80:40:10, 80:50:10, 80:60:10, 80:70:10, 80:80:10, 80:90:10, 80:100:10, 80:110:10, 80:120:10, 80:40:20, 80:40:30, 80:40:40, 80:40:50, 90:40:10, 90:40:10, 90:40:10, 90:50:20, 90:50:30, 90:50:40, 90:50:50, 90:60:20, 90:60:30, 90:60:40. 0, 90:60:50, 90:70:20, 90:70:30, 90:70:40, 90:70:50, 90:80:20, 90:80:30, 90:80:40, 90:80:50, 90:90:20, 90:90:30, 90:90:40, 90:90:50, 90:100:20, 90:100:30, 90:100:40, 90:100:50, 90:110:20, 90:110:30, 90:110:40, 90:110:50, 90:120:20, 90:120:30, 90:120:40, 90:120:50.

[0128] The weather-resistant resin substrate is selected from at least one of acrylic resin, polyester resin, fluorocarbon resin, epoxy resin, polyvinylidene fluoride (PVDF), trifluoroethylene-vinyl ether copolymer, trifluoroethylene-vinyl ester copolymer, tetrafluoroethylene-vinyl ether copolymer and isocyanate, preferably acrylic resin or fluorocarbon resin.

[0129] The solvent is at least one of toluene, xylene, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone and N-methyl pyrrolidone; preferably butyl acetate.

[0130] The black pigment is at least one of iron chrome black, copper chrome black, iron manganese black, aniline black and perylene black, preferably iron chrome black, more preferably a precursor with a Fe / Cr molar ratio of 0.5, formed by calcining at 900°C to form a high-crystallinity Cr 1.3 Fe 0.7 Iron chrome black with O3 as the main crystal phase.

[0131] The particle size of the black colorant is 5-50 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm or 50 μm.

[0132] The filler is at least one of glass powder, ceramic powder, white carbon black and alumina, preferably white carbon black. The particle size of the filler is 1-5 μm, for example, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm.

[0133] The curing agent is at least one of an isocyanate curing agent, an imidazole curing agent, an amine curing agent and a dicyandiamide curing agent, preferably an isocyanate curing agent;

[0134] The silane coupling agent is selected from one or more of γ-aminopropyltriethoxysilane, γ-glycidyl ether aminopropyltrimethoxysilane, and γ-methacryloxy-propyltrimethoxysilane, preferably γ-aminopropyltriethoxysilane.

[0135] The auxiliary agent is selected from one or more of emulsified silicone oil, high carbon alcohol fatty acid ester complex, polyoxyethylene polyoxypropylene pentaerythritol ether, polyoxyethylene polyoxypropanolamine ether, polyoxypropylene glycerol ether, polyoxypropylene polyoxyethylene glycerol ether, and polydimethylsiloxane; preferably polydimethylsiloxane.

[0136] In the present application, the black weather-resistant layer 9 is any film layer having a grid shape.

[0137] Specifically, the black weather-resistant layer 9 can be entirely coated on the surface of one side of the back glass layer 8 close to the first lower flexible film layer 7 / the surface of either side of the first lower flexible film layer 7 / the surface of either side of the strengthened film layer 6 / the surface of either side of the second lower flexible film layer 5 / the surface of the battery layer 4 close to the second lower flexible film layer 5, or can be printed on the surface of one side of the back glass layer 8 close to the first lower flexible film layer 7 / the surface of either side of the first lower flexible film layer 7 / the surface of either side of the strengthened film layer 6 / the surface of either side of the second lower flexible film layer 5 / the surface of the battery layer 4 close to the second lower flexible film layer 5 by screen printing, presenting a grid form, such as Figure 2As shown. The use of a grid structure will reduce the amount of black paint used, and allow the second lower flexible film layer 5 on the back of the battery layer 4 to be light-transmissive, so that the back side can generate electricity when a double-sided battery layer 4 is used. At the same time, infrared rays passing through the battery layer 4 can pass through the second lower flexible film layer 5 on the back side of the battery layer 4, reducing the amount of infrared rays absorbed by the device and lowering the operating temperature of the device.

[0138] In the present application, the number of the battery cell layers 4 is multiple, and the multiple battery cell layers 4 are arranged in an array at equal intervals. The battery cell layer 4 can be a common single crystal or polycrystalline battery cell layer 4, and the number of grid lines of the battery cell layer 4 can be any number between 2 and 30. It can also be a back contact battery cell layer 4, a battery cell layer 4 with a shingled structure, or a metal perforated structure battery cell layer 4 and a corresponding connection structure.

[0139] When the black weather-resistant layer 9 is in a grid shape, the black weather-resistant layer 9 is located in the gap between adjacent battery cell layers 4 , on the orthographic projection of the strengthening adhesive film layer 6 and on the edge of the strengthening adhesive film layer 6 .

[0140] In this application, the upper colored glass layer has two structures, as follows:

[0141] The first structure is: the upper colored glass layer includes an upper film layer 3, a colored glaze layer 2 and a front glass layer 1 which are arranged in sequence, and the surface of the upper film layer 3 facing away from the colored glaze layer 2 is connected to the battery layer 4.

[0142] Specifically, the upper film layer 3 is a colorless transparent film layer, which may be an EVA layer, a POE layer, a PVB layer or an SGP layer, including but not limited to these. Its thickness is 0.1-2 mm, for example, 0.1 mm, 0.5 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm or 2 mm.

[0143] The colored glaze layer 2 may be a glaze layer of various colors such as a red glaze layer, an orange glaze layer, a yellow glaze layer, a green glaze layer, a blue glaze layer, a purple glaze layer, etc.

[0144] Specifically, the colored glaze layer 2 can be a high-temperature ink composed of a glass powder base material and colored inorganic toner, or a low-temperature ink composed of an organic solvent and inorganic toner.

[0145] The high-temperature ink is prepared by mixing glass powder, inorganic color powder, and organic solvent, and then adhering to the front glass layer 1 by screen printing or spraying, and then sintering at a temperature range of 500 to 800°C, and at the same time tempering the front glass layer 1, so that the colored glaze layer 2 is arranged on the front glass layer 1.

[0146] The inorganic color powder can be a multilayer oxide composed of metal oxides such as titanium, aluminum, silicon, tin, zirconium, zinc, etc., or a multilayer structure formed by TiO2 plus natural mica or synthetic mica, which produces different colors through optical interference, or a multilayer oxide with microscopic nanostructure characteristics; the glass powder base material is a mixture of silicon oxide, bismuth oxide, boron oxide, zinc oxide, potassium carbonate, titanium oxide, zirconium oxide, aluminum oxide, calcium oxide, strontium oxide, glass strengthener, glass clarifier, decolorizer, etc., which is formed by melting and then crushing.

[0147] The low temperature ink is obtained by mixing an organic solvent with an inorganic colorant, and the obtained low temperature ink is attached to the front glass layer 1 by screen printing or spraying, and then cured by heating at 100° C. to 300° C., or cured by ultraviolet light, so that the colored glaze layer 2 is set on the front glass layer 1. The inorganic colorant is added in an amount of 0.5% to 15% in the low temperature ink.

[0148] The organic solvent may be hexanediol acrylate, functional acrylate, coupling agent, photocatalyst and other resins, and the organic solvent is stirred evenly after adding the inorganic color powder.

[0149] The front glass layer 1 is transparent glass with a thickness of 1-16 mm, for example, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, 15 mm or 16 mm.

[0150] The second structure is: the upper colored glass layer includes an upper film layer 3 and a front glass layer 1 arranged in sequence from bottom to top, and the surface of the upper film layer 3 facing away from the front glass layer 1 is connected to the battery layer 4.

[0151] Specifically, the upper film layer 3 is a colored transparent film layer with a thickness of 0.1-2 mm, for example, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm or 2 mm.

[0152] The colored transparent adhesive film layer can be formed by adding inorganic color powder to a transparent adhesive film, the transparent adhesive film can be EVA, POE, PVB or SGP, the inorganic color powder can be a multilayer oxide or pearlescent powder with interference characteristics, or can be an inorganic color powder such as ferric oxide, cobalt phosphate, copper carbonate, chromium oxide, etc. with absorption characteristics.

[0153] The front glass layer 1 is transparent glass with a thickness of 1-16 mm, for example, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, 15 mm or 16 mm.

[0154] In the present application, the upper colored glass layer is an interference type colored glass layer. Due to its high transmittance and low reflectivity, when there is a material with high visible light reflectivity below the upper colored glass layer, the visible light waves reflected by the upper colored glass layer itself are mixed with the visible light waves reflected by the upper colored glass layer below. At this time, the color seen by the human eye will be different from the color presented by the upper colored glass layer itself. Therefore, it is necessary to have a completely black or nearly black material below the upper colored glass layer to absorb the visible light transmitted by the glass. At this time, the light received by the human eye above the upper colored glass layer will mainly be the reflected light generated by the interference of the inorganic color powder in the upper colored glass layer, so that the true color of the upper colored glass layer can be seen.

[0155] In the present application, the upper colored glass layer has an anti-glare structure.

[0156] Specifically, a surface of the upper colored glass layer facing away from the colored glaze layer 2 is coated with an anti-reflection layer to improve light transmittance.

[0157] In the present application, the upper transparent layer includes an upper adhesive film layer 3 and a front glass layer 1 arranged in sequence from bottom to top, and a surface of the upper adhesive film layer 3 facing away from the front glass layer 1 is connected to the cell layer 4 .

[0158] Specifically, the upper film layer 3 is a transparent film layer with a thickness of 0.1-2 mm, for example, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm or 2 mm.

[0159] The transparent adhesive film layer may be EVA, POE, PVB or SGP, etc., including but not limited to these.

[0160] The front glass layer 1 is transparent glass with a thickness of 1-16 mm, for example, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, 15 mm or 16 mm.

[0161] Furthermore, the upper transparent layer has an anti-glare structure.

[0162] The present application provides a method for preparing a colored photovoltaic module, comprising the following steps:

[0163] Step 1: Provide a back glass layer 8,

[0164] Step 2: providing a three-layer composite film, wherein the three-layer composite film comprises a first lower flexible adhesive film layer 7, a strengthening adhesive film layer 6 and a second lower flexible adhesive film layer 5 which are sequentially stacked together;

[0165] Step 3: stacking the first lower flexible adhesive film layer 7 and the back glass layer 8 together;

[0166] Step 4: Arranging a battery cell layer 4 on a surface of the second lower flexible adhesive film layer 5 which is away from the strengthening adhesive film layer 6;

[0167] Step 5: Arrange the upper glass layer on the surface of the battery cell layer 4 which faces away from the second lower flexible adhesive film layer 5 .

[0168] In step 2, after the two surfaces of the strengthening film layer 6 are subjected to corona treatment, they are respectively pressed with the first lower flexible film layer 7 and the second lower flexible film layer 5 to form a three-layer composite film.

[0169] The three-layer composite film exists in the color photovoltaic module. When the strengthening film layer 6 is a PET film layer, the surface activity of the PET film and the surface coating of the PET film is usually low, and the adhesion to the flexible film is low. In order to enhance the adhesion, the surface of the PET film is usually treated with plasma corona treatment when leaving the factory, so as to form abundant hanging bonds on the surface of the PET film, so that the PET film and the flexible film form chemical bonds and produce strong adhesion. Therefore, the PET film after corona treatment can be directly laminated with the flexible film in a laminator to form a three-layer composite film. PET, as a thermosetting material, has an elastic modulus of about 1 to 2GPa at room temperature, and the fracture strength can reach more than 120MPa, which is higher than the strength of tempered glass. Even if the temperature rises to 75°C, its elastic modulus still exceeds 1GPa, and the strength is not much lost. In this way, the device works normally when the ambient temperature is high. When the component temperature reaches 60 to 80°C, the presence of the PET film layer makes the three-layer composite film still have high modulus and high strength. In this way, even at a high temperature of 80°C, when the device is subjected to abnormal external force and the back glass layer 8 or the front glass layer is broken, the high-strength and tough PET film layer can adhere to the flexible film such as the first lower flexible film layer 7 and the second lower flexible film layer 5, so as to adhere to the broken glass fragments and prevent them from falling in pieces and injuring pedestrians under the high-rise building. If there is no high-temperature rigid material such as PET film, when the device is broken, the dead weight of the glass fragments will be fully loaded on the flexible film such as the first lower flexible film layer 7, the second lower flexible film layer 5 and the upper flexible film layer with lower high-temperature strength, causing the film to stretch and deform until it cracks, causing large pieces of glass fragments to fall off the component, which will cause safety hazards. Therefore, a high-strength PET layer at high temperature can allow the component to maintain high flexural deformation resistance and high impact resistance, that is, it has high safety performance. This high-strength PET film material can also be replaced by PU, nylon or metal mesh materials. These materials have higher strength and can have stronger anti-falling ability when the component is broken, and have higher safety performance.

[0170] Example

[0171] The experimental methods used in the following examples are all conventional methods unless otherwise specified.

[0172] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0173] Example 1

[0174] The method for preparing the colored photovoltaic module of this embodiment comprises the following steps:

[0175] Step 1: Provide the back glass layer,

[0176] The back glass layer is transparent glass, and its thickness can be 3.2 mm.

[0177] Step 2: providing a three-layer composite film, wherein the three-layer composite film comprises a first lower flexible adhesive film layer, a strengthening adhesive film layer and a second lower flexible adhesive film layer stacked together in sequence;

[0178] Before the reinforcing film layer is composited, a black weather-resistant layer is printed on one surface of the reinforcing film layer. Then, after the two surfaces of the reinforcing film layer are corona treated, they are respectively pressed with the first lower flexible film layer and the second lower flexible film layer, so as to be stacked together to form a three-layer composite film.

[0179] The first lower flexible film layer is an EVA film layer, and its thickness is 0.5 mm.

[0180] The strengthening film layer is a PET film layer, and its thickness is 0.2 mm.

[0181] The second lower flexible film layer is a POE film layer, and its thickness is 0.5 mm.

[0182] The black weather-resistant layer is in a grid shape. The formula of the black weather-resistant layer is acrylic resin, butyl acetate, iron chrome black, white carbon black, γ-aminopropyl triethoxysilane, isocyanate curing agent and polydimethylsiloxane in a mass ratio of 80:40:10:5:10:10:1. The black weather-resistant layer is formed by mixing the above compounds, heating and curing.

[0183] Step 3: stacking the first lower flexible adhesive film layer and the back glass layer together;

[0184] Step 4: a battery cell layer is arranged on the surface of the second lower flexible adhesive film layer which is away from the strengthening adhesive film layer; the battery cell layer is a crystalline silicon battery cell layer.

[0185] Step 5: Arranging an upper flexible adhesive film layer on a surface of the battery layer on a side away from the second lower flexible adhesive film layer;

[0186] A front glass layer is provided, and a blue glaze layer is formed on one side surface of the front glass layer, and the side surface of the front glass layer having the blue glaze layer is laminated with the upper flexible adhesive film.

[0187] The upper flexible adhesive film layer is an EVA film layer, and its thickness is 0.5 mm.

[0188] The front glass layer is transparent glass with a thickness of 3.2 mm.

[0189] The colored photovoltaic modules were tested as follows:

[0190] Strength test: In terms of strength, the test was conducted according to the drop ball test standard, using steel balls of different weights to impact the color photovoltaic module from different heights. In the case where the back glass layer and the front glass layer are damaged, the glass fragments in the color photovoltaic module of this embodiment can adhere to the strengthening film layer without scattering, and the safety is relatively high.

[0191] Flexural deformation test: The device with both the back glass layer and the front glass layer broken after impact by a steel ball was placed sideways in a high temperature box at 80°C for 1 hour (simulating the high temperature state of the component during actual operation), and the device of this embodiment was taken out and remained intact.

[0192] Color test: Use a spectrophotometer to test the color of the finished components. After testing, the Musell index L, C, and H that characterize the color characteristics are 32, 23, and -86 respectively. Among them, L is lightness, C is saturation, and H is hue. Saturation 23 is already a relatively high saturation, and the color characteristics are very obvious. Glass of this color has a high transmittance and a low reflectivity.

[0193] The performance of the colored photovoltaic module is shown in Table 1 and Table 2. Its color characteristics are as follows Figure 3 , from Table 2 and Figure 3 It can be seen that the color photovoltaic module of Example 1 has high color saturation while still maintaining high device efficiency and high safety features.

[0194] Example 2

[0195] The difference between Example 2 and Example 1 is that the black weather-resistant layer in Example 2 covers the entire surface of the strengthening film layer. The performance of the color photovoltaic module is shown in Table 1 and Table 2.

[0196] Example 3

[0197] The difference between Example 3 and Example 1 is that there is no black weather-resistant layer. The performance of the color photovoltaic module is shown in Table 1 and Table 2.

[0198] Example 4

[0199] The difference between Example 3 and Example 1 is that the strengthening film layer is a PU film layer. The performance of the color photovoltaic module is shown in Table 1 and Table 2.

[0200] Example 5

[0201] The difference between Example 5 and Example 1 is that the strengthening film layer is a nylon layer. The performance of the color photovoltaic module is shown in Table 1 and Table 2.

[0202] Example 6

[0203] The difference between Example 6 and Example 1 is that the strengthening film layer is a metal mesh layer. The performance of the color photovoltaic module is shown in Table 1 and Table 2.

[0204] Example 7

[0205] The difference between Example 7 and Example 1 is that the formula of the black weather-resistant layer is different. The formula of the black weather-resistant layer in Example 7 is: the mass ratio of acrylic resin, butyl acetate, iron chrome black, white carbon black, γ-aminopropyltriethoxysilane, isocyanate curing agent and polydimethylsiloxane is 90:60:15:5:10:10:1. The performance of the color photovoltaic module is shown in Table 1 and Table 2.

[0206] Example 8

[0207] The difference between Example 8 and Example 1 is that the formula of the black weather-resistant layer is different. The formula of the black weather-resistant layer in Example 8 is: the mass ratio of polyvinylidene fluoride, butyl acetate, iron chrome black, white carbon black, γ-aminopropyltriethoxysilane, isocyanate curing agent and polydimethylsiloxane is 80:60:20:5:10:10:1. The performance of the color photovoltaic module is shown in Table 1 and Table 2.

[0208] Example 9

[0209] The difference between Example 9 and Example 1 is that the formula of the black weather-resistant layer is different. The formula of the black weather-resistant layer in Example 9 is: the mass ratio of acrylic resin, propylene glycol methyl ether acetate, iron chrome black, white carbon black, γ-aminopropyl triethoxy silane, isocyanate curing agent and polydimethylsiloxane is 100:70:25:5:10:10:2. The performance of the color photovoltaic module is shown in Tables 1 and 2.

[0210] Example 10

[0211] The difference between Example 10 and Example 1 is that the formula of the black weather-resistant layer is different. The formula of the black weather-resistant layer in Example 10 is: the mass ratio of perfluoroethyl ether, butyl acetate, iron chrome black, white carbon black, γ-aminopropyltriethoxysilane, isocyanate curing agent and polydimethylsiloxane is 100:70:30:5:10:10:2. The performance of the color photovoltaic module is shown in Tables 1 and 2.

[0212] Embodiment 11

[0213] The difference between Example 11 and Example 1 is that the formula of the black weather-resistant layer is different. The formula of the black weather-resistant layer in Example 11 is: the mass ratio of acrylic resin, butyl acetate, carbon black, white carbon black, γ-aminopropyltriethoxysilane, isocyanate curing agent and polydimethylsiloxane is 80:60:20:5:10:10:1. The performance of the color photovoltaic module is shown in Tables 1 and 2.

[0214] Example 12

[0215] like Figure 6 As shown, the difference between Example 12 and Example 1 is that the position of the black weather-resistant layer is different. In this embodiment, the black weather-resistant layer is arranged between the back glass layer and the first lower flexible adhesive film layer.

[0216] The performance of the photovoltaic module is shown in Table 1.

[0217] Example 13

[0218] like Figure 5 As shown, the difference between Example 13 and Example 1 is that the position of the black weather-resistant layer is different. In this embodiment, the black weather-resistant layer is arranged between the first lower flexible adhesive film layer and the strengthening adhesive film layer.

[0219] The performance of the photovoltaic module is shown in Table 1.

[0220] Embodiment 14

[0221] like Figure 4 As shown, the difference between Example 14 and Example 1 is that the position of the black weather-resistant layer is different. In this embodiment, the black weather-resistant layer is arranged between the second lower flexible film layer and the battery cell layer.

[0222] The performance of the photovoltaic module is shown in Table 1.

[0223] Embodiment 15

[0224] The difference between Example 15 and Example 1 is that the position of the black weather-resistant layer is different. In this embodiment, the black weather-resistant layer is arranged on the surface of the back glass layer away from the first lower flexible adhesive film layer.

[0225] The performance of the photovoltaic module is shown in Table 1.

[0226] Comparative Example 1

[0227] The difference between Comparative Example 1 and Example 1 is that there is no strengthening film layer. The performance of the color photovoltaic module is shown in Table 1 and Table 2.

[0228] Table 1 shows the formula and reflectivity of the black weather-resistant layer of each embodiment and comparative example

[0229]

[0230]

[0231] Table 2 Flexural deformation resistance and high impact resistance

[0232]

[0233] Summary: As can be seen from Tables 1 and 2, the colored photovoltaic modules described in this application use colored ink printed glass to achieve the color of the front glass. The use of pearlescent powder or multi-layer oxide nano-color powder ensures that the glass is colored while maintaining a high light transmittance, thereby ensuring the high efficiency of the photovoltaic module. This ensures that the photovoltaic module not only meets the appearance requirements when used in the construction field, but also maintains the core power generation properties of the photovoltaic module to the highest extent. In terms of packaging materials, a unique flexible film plus a rigid film plus a flexible film is used. The use of a rigid material layer ensures the high strength of the photovoltaic module, especially the post-destruction strength, that is, after the module is damaged, it will not fall due to insufficient film strength, especially after the strength of the flexible film decreases under high temperature conditions. The core property of the safety of the photovoltaic module used on the building curtain wall is guaranteed. The black weather-resistant layer of the rigid film layer is a necessary component for the color development of pearlescent powder and multi-layer oxide nano-color powder. The ordinary black weather-resistant layer has a low reflectivity and strong absorption in the visible and near-infrared light bands. After verification using the different formulas shown in Table 1, it was found that the change in the material has improved the reflectivity of near-infrared light above 750nm to varying degrees. The light reflected by the back material of the photovoltaic module can pass through the gap and be reflected by the glass interface to the surface of the cell, where it is absorbed by the cell, generating power gain. The highly reflective coating structure will generate power gain, further improving the efficiency of the photovoltaic module and bringing additional benefits.

[0234] Although the embodiments of the present application are described above, the present application is not limited to the above specific embodiments and application fields, and the above specific embodiments are merely illustrative and instructive, rather than restrictive. A person of ordinary skill in the art can make many forms under the guidance of this specification and without departing from the scope of protection of the claims of the present application, all of which belong to the protection of the present application.

Claims

1. A colored photovoltaic module, It is characterized in that It includes a back glass layer, a film layer, a battery layer and an upper colored glass layer which are stacked in sequence; A black weather-resistant layer is provided on a surface of the back glass layer facing away from the adhesive film layer, between the back glass layer and the adhesive film layer, between the adhesive film layer and the battery cell, or in the adhesive film layer; The black weather-resistant layer has a reflectivity of less than 10% for visible light and a reflectivity of more than 30% for infrared light with a wavelength of more than 750 nm.

2. The color photovoltaic module according to claim 1, It is characterized in that The adhesive film layer is composed of an adhesive film, and the adhesive film is selected from any one of a single-layer adhesive film, a double-layer adhesive film, a triple-layer adhesive film, or the like.

3. The color photovoltaic module according to claim 2, It is characterized in that The adhesive film is a flexible adhesive film or a reinforced adhesive film or a laminated adhesive film of a flexible adhesive film and a reinforced adhesive film; The reinforced adhesive film layer is one of a PET film layer, a PU film layer, a nylon layer or a metal mesh layer; The thickness of the strengthening film layer is 0.1-1 mm.

4. The colored photovoltaic module according to claim 1, It is characterized in that The adhesive film layer comprises a first lower flexible adhesive film layer, a strengthening adhesive film and a second lower flexible adhesive film layer which are stacked in sequence.

5. The colored photovoltaic module according to claim 1, It is characterized in that The adhesive film layer comprises a first lower flexible adhesive film layer, a strengthening adhesive film, a black weather-resistant layer and a second lower flexible adhesive film layer which are stacked in sequence.

6. The colored photovoltaic module according to claim 1, It is characterized in that The upper colored glass layer includes an upper adhesive film layer, a colored glaze layer and a front glass layer which are sequentially arranged from bottom to top, and a surface of the upper adhesive film layer on a side away from the colored glaze layer is connected to the battery sheet layer.

7. The colored photovoltaic module according to claim 6, It is characterized in that The upper adhesive film layer is a colorless and transparent adhesive film layer, and its thickness is 0.1-2 mm.

8. The colored photovoltaic module according to claim 1, It is characterized in that The upper colored glass layer comprises an upper adhesive film layer and a front glass layer which are arranged in sequence, and a surface of the upper adhesive film layer on a side facing away from the front glass layer is connected to the battery sheet layer.

9. The colored photovoltaic module according to claim 8, It is characterized in that The upper adhesive film layer is a colored transparent adhesive film layer, and its thickness is 0.1-2 mm.

10. The colored photovoltaic module according to claim 6, It is characterized in that The front glass layer is transparent glass with a thickness of 1-16 mm.

11. The colored photovoltaic module according to claim 6, It is characterized in that An anti-reflection layer is disposed on one side surface of the front glass layer.

12. The colored photovoltaic module according to any one of claims 1 to 11, It is characterized in that The black weather-resistant layer comprises the following components: The weather-resistant resin base material is 80-100 parts, the solvent is 40-120 parts, the black colorant is 10-50 parts, the filler is 5-20 parts, the silane coupling agent is 1-20 parts, the curing agent is 3-30 parts, and the additive is 1-5 parts; The black colorant is iron chrome black or perylene black.

13. The colored photovoltaic module according to claim 12, It is characterized in that The weather-resistant resin substrate is selected from at least one of acrylic resin, polyester resin, fluorocarbon resin, epoxy resin, trifluoroethylene-vinyl ether copolymer, trifluoroethylene-vinyl ester copolymer, and tetrafluoroethylene-vinyl ether copolymer; The solvent is selected from at least one of toluene, xylene, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone and N-methylpyrrolidone; The filler is selected from at least one of glass powder, ceramic powder, white carbon black and alumina; The curing agent is at least one of an isocyanate curing agent, an imidazole curing agent, an amine curing agent and a dicyandiamide curing agent; The silane coupling agent is selected from at least one of γ-aminopropyltriethoxysilane, γ-glycidyl ether aminopropyltrimethoxysilane, and γ-methacryloxy-propyltrimethoxysilane; The auxiliary agent is selected from one of emulsified silicone oil, high carbon alcohol fatty acid ester complex, polyoxyethylene polyoxypropylene pentaerythritol ether, polyoxyethylene polyoxypropanolamine ether, polyoxypropylene glycerol ether, polyoxypropylene polyoxyethylene glycerol ether or polydimethylsiloxane.

14. The colored photovoltaic module according to claim 13, It is characterized in that The weather-resistant resin substrate is acrylic resin or fluorocarbon resin.

15. The colored photovoltaic module according to claim 13, It is characterized in that The solvent is butyl acetate.

16. The colored photovoltaic module according to claim 13, It is characterized in that The filler is white carbon black.

17. The colored photovoltaic module according to claim 13, It is characterized in that The curing agent is an isocyanate curing agent.

18. The colored photovoltaic module according to claim 13, It is characterized in that The silane coupling agent is γ-aminopropyltriethoxysilane.

19. The colored photovoltaic module according to claim 13, It is characterized in that The auxiliary agent is polydimethylsiloxane.

20. The colored photovoltaic module according to claim 12, It is characterized in that The particle size of the black colorant is 5-50 μm; the particle size of the filler is 1-5 μm.

21. The colored photovoltaic module according to claim 12, It is characterized in that The black weather-resistant layer is a film layer having a grid shape.

22. A photovoltaic module, It is characterized in that It includes a back plate, a first lower flexible film layer, a strengthening film layer, a second lower flexible film layer, a battery sheet layer and a front plate which are stacked in sequence; A black weather-resistant layer is provided at any one position of the surface of the backplane facing away from the first lower flexible adhesive film layer, between the backplane and the first lower flexible adhesive film layer, between the first lower flexible adhesive film layer and the strengthening adhesive film layer, between the strengthening adhesive film layer and the second lower flexible adhesive film layer, and between the second lower flexible adhesive film layer and the battery cell; The back plate is a glass back plate; the front plate is an upper colored glass layer; The black weather-resistant layer includes a black pigment, and the black pigment is iron chrome black or perylene black.

23. The photovoltaic module according to claim 22, It is characterized in that The first lower flexible adhesive film layer and the second lower flexible adhesive film layer are both selected from one of an EVA film layer, a POE film layer, a PVB film layer or an SGP film layer; The thickness of the first lower flexible adhesive film layer is 0.1-2 mm; The thickness of the second lower flexible adhesive film layer is 0.1-2 mm.

24. The photovoltaic module according to claim 22, It is characterized in that The reinforced adhesive film layer is one of a PET film layer, a PU film layer, a nylon layer or a metal mesh layer; The thickness of the strengthening film layer is 0.1-1 mm.

25. The photovoltaic module according to claim 22, It is characterized in that The photovoltaic module comprises a back glass layer, a first lower flexible adhesive film layer, a strengthening adhesive film layer, a second lower flexible adhesive film layer, a battery sheet layer and an upper colored glass layer which are stacked in sequence.

26. The photovoltaic module according to claim 25, It is characterized in that The upper colored glass layer includes an upper adhesive film layer, a colored glaze layer and a front glass layer which are sequentially arranged from bottom to top, and a surface of the upper adhesive film layer on a side away from the colored glaze layer is connected to the battery sheet layer.

27. The photovoltaic module according to claim 26, It is characterized in that The upper adhesive film layer is a colorless and transparent adhesive film layer, and its thickness is 0.1-2 mm.

28. The photovoltaic module according to claim 25, It is characterized in that The upper colored glass layer comprises an upper adhesive film layer and a front glass layer which are arranged in sequence, and a surface of the upper adhesive film layer on a side facing away from the front glass layer is connected to the battery sheet layer.

29. The photovoltaic module according to claim 28, It is characterized in that The upper adhesive film layer is a colored transparent adhesive film layer, and its thickness is 0.1-2 mm.

30. The photovoltaic module according to claim 28, It is characterized in that The front glass layer is transparent glass with a thickness of 1-16 mm.

31. The photovoltaic module according to claim 28, It is characterized in that An anti-reflection layer is disposed on one side surface of the front glass layer.

32. The photovoltaic module according to any one of claims 22 to 31, It is characterized in that The black weather-resistant layer comprises the following components: The weather-resistant resin base material is 80-100 parts, the solvent is 40-120 parts, the black colorant is 10-50 parts, the filler is 5-20 parts, the silane coupling agent is 1-20 parts, the curing agent is 3-30 parts, and the auxiliary agent is 1-5 parts.

33. The photovoltaic module according to claim 32, It is characterized in that The weather-resistant resin substrate is selected from at least one of acrylic resin, polyester resin, fluorocarbon resin, epoxy resin, trifluoroethylene-vinyl ether copolymer, trifluoroethylene-vinyl ester copolymer, and tetrafluoroethylene-vinyl ether copolymer; The solvent is selected from at least one of toluene, xylene, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone and N-methylpyrrolidone; The filler is selected from at least one of glass powder, ceramic powder, white carbon black and alumina; The curing agent is at least one of an isocyanate curing agent, an imidazole curing agent, an amine curing agent and a dicyandiamide curing agent; The silane coupling agent is selected from at least one of γ-aminopropyltriethoxysilane, γ-glycidyl ether aminopropyltrimethoxysilane, and γ-methacryloxy-propyltrimethoxysilane; The auxiliary agent is selected from one of emulsified silicone oil, high carbon alcohol fatty acid ester complex, polyoxyethylene polyoxypropylene pentaerythritol ether, polyoxyethylene polyoxypropanolamine ether, polyoxypropylene glycerol ether, polyoxypropylene polyoxyethylene glycerol ether or polydimethylsiloxane.

34. The photovoltaic module according to claim 33, It is characterized in that The weather-resistant resin substrate is acrylic resin or fluorocarbon resin.

35. The photovoltaic module according to claim 33, It is characterized in that The solvent is butyl acetate.

36. The photovoltaic module according to claim 33, It is characterized in that The filler is white carbon black.

37. The photovoltaic module according to claim 33, It is characterized in that The curing agent is an isocyanate curing agent.

38. The photovoltaic module according to claim 33, It is characterized in that The silane coupling agent is γ-aminopropyltriethoxysilane.

39. The photovoltaic module according to claim 33, It is characterized in that The auxiliary agent is polydimethylsiloxane.

40. The photovoltaic module according to claim 32, It is characterized in that The particle size of the black colorant is 5-50 μm; the particle size of the filler is 1-5 μm.

41. The photovoltaic module according to claim 32, It is characterized in that The black weather-resistant layer is a film layer having a grid shape.

42. The photovoltaic assembly according to claim 32, It is characterized in that The black weather-resistant layer has a reflectivity of less than 10% for visible light and a reflectivity of more than 30% for infrared light with a wavelength of more than 750 nm.

43. A method for preparing a colored photovoltaic module according to any one of claims 1 to 21, It is characterized in that The steps include: Provides a back glass layer, Providing a three-layer composite film, the three-layer composite film comprising a first lower flexible adhesive film layer, a strengthening adhesive film layer and a second lower flexible adhesive film layer stacked together in sequence; Laying the first lower flexible adhesive film layer and the back glass layer together; Arranging a battery sheet layer on a surface of the second lower flexible adhesive film layer facing away from the strengthening adhesive film layer; Arranging the upper material glass layer on the surface of the battery layer on the side away from the second lower flexible adhesive film layer; A black weather-resistant layer is provided at any position on the surface of the back glass layer facing away from the first lower flexible adhesive film layer, between the back glass layer and the first lower flexible adhesive film layer, between the first lower flexible adhesive film layer and the strengthening adhesive film layer, between the strengthening adhesive film layer and the second lower flexible adhesive film layer, and between the second lower flexible adhesive film layer and the battery cell.

44. The method for preparing a colored photovoltaic module according to claim 43, It is characterized in that After the two surfaces of the strengthening film layer are subjected to corona treatment, they are respectively pressed with the first lower flexible film layer and the second lower flexible film layer to form the three-layer composite film.