High-strength fireproof sealant and preparation method thereof
Through the preparation method of high-strength fire-proof sealant, the high-strength expansion ceramic substance is formed using specific components and processes, which solves the problem of softening and collapse of existing fire-proof sealant at high temperatures, and achieves long-term fire-proof seal protection and smoke Barrier effect.
Patent Information
- Application Number
- CN202211625804.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-13
AI Technical Summary
Existing organic fire-proof sealants are prone to softening and collapse under high temperature fires, and have insufficient fire resistance and cannot provide fire-proof seal protection for a long time.
The preparation method of high-strength fire-resistant sealant, including α,ω-dihydroxypolydimethylsiloxane, composite flame retardant, composite fire-resistant filler, glass fiber and other components, is modified by vacuum water removal and dry method. An expanded ceramic material with high strength and adhesion is formed, and can be kept in a hard state at a high temperature of 1200 to 1500°C for 3 hours.
It has achieved the improvement of the fire resistance performance of high-strength fire-resistant sealant, prevents the softening and collapse of the sealing material, blocks the spread of fire and smoke, has good plasticity and adhesiveness, has a long service life, and is suitable for many occasions.
Smart Images

Figure BDA0003996087290000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fireproof materials, in particular to a high-strength fireproof sealant and a preparation method thereof. Background Art
[0002] The 2015 version of the "Code for Fire Protection Design of Buildings" clearly states that the fire resistance level of the building, the combustion performance and fire resistance limit of the component materials should be clearly defined in the design, and the fire protection zones should be reasonably divided, and appropriate fire and smoke prevention measures should be taken. Since July 1, 2020, GB514410-2020 "Technical Standard for Application of Fire Protection Sealing in Buildings" has been officially implemented, and the importance of fireproof sealing materials has been further enhanced. Fireproof sealing materials refer to materials used to seal or fill the through holes and gaps of various facilities such as buildings and pipelines, and have fireproof, smokeproof and other related properties. They can prevent the spread of fire from the gaps when a fire occurs, so as to achieve the purpose of protecting the safety of personnel and equipment. The basic principle of fireproof sealing is that the sealing material expands under heat or fire to absorb heat and insulate, which can reduce the temperature on the back of the penetration and prevent the back from catching fire. At the same time, the expansion material produced can fill the gaps produced by combustion and reduce the spread of toxic smoke produced in the fire.
[0003] Organic fireproof sealant is the most widely used fireproof sealing material. It is made of polymer resin as adhesive, mixed with various fire retardants and fillers. It has good thixotropy, plasticity and sealing properties, suitable for sealing various scenes and gaps, and can also prevent fire and block water. However, most organic fireproof sealants currently do not have sufficient fire resistance. They are easy to soften and collapse under high temperature fire conditions. The material after burning is a brittle solid, which loses strength and sealing properties and cannot provide long-term fireproof sealing protection for the seal.
[0004] Therefore, it is very necessary to develop a green and environmentally friendly fireproof sealing glue and a preparation method thereof, which has good weather resistance, good fireproof sealing performance and simple process implementation. Summary of the invention
[0005] The purpose of the present invention is to provide a high-strength fireproof sealant and a method for preparing the high-strength fireproof sealant, which has excellent fire resistance, can withstand high temperatures of 1200 to 1500°C for up to 3 hours and form a hard, intumescent ceramic material. The high-strength fireproof sealant of the present method has a structure similar to "reinforced concrete" inside, has excellent structural strength, can effectively ensure the progress of the ceramicization process, blocks the spread of fire and the diffusion of smoke, and solves the shortcomings of traditional fireproof sealants such as easy collapse, softening, and insufficient fire resistance. The fireproof sealant prepared by the present method has good plasticity and adhesion, is simple to construct, is easy to construct a second time, has a long service life, and has good prospects.
[0006] The present invention is achieved in that:
[0007] In a first aspect, the present invention provides a high-strength fireproof sealant, comprising the following components in parts by weight:
[0008] α,ω-dihydroxypolydimethylsiloxane: 350-600 parts;
[0009] 201 silicone oil: 50-200 parts;
[0010] Composite flame retardant: 300-600 parts;
[0011] Composite fireproof filler: 300-600 parts;
[0012] Composite inorganic filler: 100-300 parts;
[0013] Glass fiber: 10-15 parts;
[0014] Composite cross-linking agent: 10-40 parts;
[0015] The first coupling agent: 10-20 parts;
[0016] Second coupling agent: 10-20 parts;
[0017] First gas generating agent: 5-10 parts;
[0018] Second gas generating agent: 5-10 parts;
[0019] Catalyst: 0.5 to 2 parts.
[0020] In an optional embodiment, the composite flame retardant is at least two of ammonium polyphosphate, piperazine pyrophosphate, aluminum hypophosphite, diethyl aluminum hypophosphite, melamine polyphosphate, melamine cyanurate, aluminum hydroxide, magnesium hydroxide, zinc borate, silicon dioxide, titanium dioxide, and expandable graphite.
[0021] In an optional embodiment, the composite fireproof filler is at least two of glass fiber powder, sodium silicate, aluminum silicate, calcium silicate, silicon carbide, wollastonite powder, kaolin, and montmorillonite.
[0022] In an optional embodiment, the composite inorganic filler is at least two of calcium carbonate, talc, hydrotalcite, kaolin, white carbon black, carbon black, and red iron.
[0023] In an optional embodiment, the viscosity of the α,ω-dihydroxy polydimethylsiloxane is at least one of the following three viscosity ranges: 1000 to 10000 viscous, 10000 to 100000 viscous, and 100000 to 500000 viscous.
[0024] In an optional embodiment, the viscosity of the 201 silicone oil is 50-200 viscous.
[0025] In an optional embodiment, the glass fiber is chopped glass fiber of 3 to 6 μm or glass fiber cloth of 1 to 4 μm.
[0026] In an optional embodiment, the composite crosslinking agent is at least two of methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, phenyltriacetylsilane, vinyltributylacetoximinesilane or tetrabutylketoximesilane.
[0027] In an optional embodiment, the first coupling agent is a long-chain or cycloalkyl silane such as hexadecyltrimethoxysilane and dodecyltrimethoxysilane; the second coupling agent is at least one of KH-540, KH-550 or KH-570.
[0028] In an optional embodiment, the first gas generating agent and the second gas generating agent are at least one of ammonium carbonate, azobisisobutyronitrile, azodicarbonamide, and N,N"-dinitrosopentamethylenetetramine.
[0029] In an optional embodiment, the catalyst is at least one of stannous chloride, dibutyltin dilaurate, dibutyltin diacetate or stannous octoate.
[0030] In a second aspect, the present invention provides a method for preparing a high-strength fireproof sealant, comprising the following steps:
[0031] The composite flame retardant, the composite fireproof filler and the composite inorganic filler are mixed uniformly in a certain proportion to obtain a mixed material, and then the mixed material and the glass fiber are respectively placed in a vacuum oven to perform vacuum dehydration at a temperature of 120 to 160° C.;
[0032] The mixed material after vacuum dehydration is placed in a stirring device, and dry-modified using a first coupling agent at 80-90° C.;
[0033] Add α, ω-dihydroxy polydimethylsiloxane and 201 silicone oil into the mixed material, stir well, then heat and maintain at 90-95° C. and stir well, then remove water in vacuo to obtain a mixture;
[0034] The mixture is cooled to 20-40°C, and then glass fiber is added and mixed evenly;
[0035] The composite cross-linking agent, the second coupling agent, the first gas generating agent, the second gas generating agent and the catalyst are respectively added into the mixture in measured amounts, and after being mixed evenly, the mixture is discharged to obtain a high-strength fireproof sealant.
[0036] In an optional embodiment, the ratio of the composite flame retardant, the composite fireproof filler and the composite inorganic filler is (1-2): (1-2): (0.5-1), and the mixture is vacuum dehydrated at 120-160° C. and maintained for 4-6 hours.
[0037] The present invention has the following beneficial effects:
[0038] A high-strength fireproof sealant and a preparation method thereof provided by the present invention have the following beneficial effects:
[0039] (1) The high-strength fireproof sealant of the present invention is stronger than the general fireproof sealants on the market. The addition of glass fiber makes the fireproof sealant have higher strength and internal adhesion, so that the internal structure of the material has a structure similar to "reinforced concrete", and the sealing integrity can still be maintained under high stress impact during use;
[0040] (2) The high-strength fireproof sealant of the present invention innovatively uses a high-efficiency gas generating agent in the propellant as a gas source, which can quickly and effectively form a porous expandable foaming layer under fire conditions and generate a large amount of non-flammable nitrogen to block the contact of combustible gases and the spread of heat;
[0041] (3) The high-strength fireproof sealant of the present invention has good fireproof performance. When the fire is small, it can self-extinguish and release fire-retardant factors to suppress the fire in the initial stage. When the fire is large, it can produce a large amount of gas to form an intumescent ceramic structure, which provides long-term protection for the seal and inhibits the spread of flames and smoke. The unique high-strength structure can prevent the sealing material from softening and collapsing, ensure the smooth progress of the ceramicization process, and thus ensure the fireproof efficiency;
[0042] (4) In the high-strength fireproof sealant described in the present invention, the hydrophobicity of the solid powder is greatly improved after dry modification, and the modifier can produce intermolecular forces with the colloid, reducing the antagonistic effect between the solid weakly acidic powder and the silicone, so that the weather resistance, water resistance, oil resistance, acid and alkali resistance, thaw resistance, UV resistance, and aging resistance of the fireproof sealant are significantly improved. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0044] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.
[0045] In the first aspect, the present invention provides a high-strength fireproof sealant, comprising the following components in parts by weight: 350 to 600 parts of α, ω-dihydroxypolydimethylsiloxane; 50 to 200 parts of 201 silicone oil; 300 to 600 parts of composite flame retardant; 300 to 600 parts of composite fireproof filler; 100 to 300 parts of composite inorganic filler; 10 to 15 parts of glass fiber; 10 to 40 parts of composite cross-linking agent; 10 to 20 parts of first coupling agent; 10 to 20 parts of second coupling agent; 5 to 10 parts of first gas generating agent; 5 to 10 parts of second gas generating agent; and 0.5 to 2 parts of catalyst.
[0046] Furthermore, the composite flame retardant is at least two of ammonium polyphosphate, piperazine pyrophosphate, aluminum hypophosphite, diethyl aluminum hypophosphite, melamine polyphosphate, melamine cyanurate, aluminum hydroxide, magnesium hydroxide, zinc borate, silicon dioxide, titanium dioxide, and expandable graphite. The composite flame retardant needs to focus on the addition of acid source, gas source, and smoke suppressant to give full play to the synergistic flame retardant efficiency. Therefore, phosphate, melamine salt, and zinc salt are mainly selected in the flame retardant, and other flame retardants are added according to requirements; in addition to the flame retardant efficiency, the effect of the flame retardant on the inherent properties of the adhesive should also be considered. Generally, the less the amount added, the smaller the effect. Therefore, the appropriate flame retardant compound can achieve a small amount of high efficiency.
[0047] Furthermore, the composite fireproof filler is at least two of glass fiber powder, sodium silicate, aluminum silicate, calcium silicate, silicon carbide, wollastonite powder, kaolin and montmorillonite.
[0048] Furthermore, the composite inorganic filler is at least two of calcium carbonate, talc, hydrotalcite, kaolin, white carbon black, carbon black, and red iron oxide.
[0049] Further, the viscosity of the α,ω-dihydroxy polydimethylsiloxane is at least one of the three viscosity ranges of 1000-10000 viscosity, 10000-100000 viscosity and 100000-500000 viscosity. Preferably, it is one in the viscosity range of 100000-500000 viscosity. The α,ω-dihydroxy polydimethylsiloxane can be selected from one of the high viscosity 100000-500000 viscosity. The low viscosity α,ω-dihydroxy polydimethylsiloxane has a large tensile strength and low elongation after curing into a film. On the contrary, the high viscosity α,ω-dihydroxy polydimethylsiloxane has a low tensile strength and high elongation after curing into a film. Since the high-strength fireproof sealant prepared by this method has a high solid material content, the strength of the material will be increased, while the elongation will be significantly reduced. Therefore, a high-viscosity α,ω-dihydroxy polydimethylsiloxane is selected to improve the elongation.
[0050] Furthermore, the viscosity of the 201 silicone oil is 50-200 viscous.
[0051] Furthermore, the glass fiber is chopped glass fiber of 3 to 6 μm or glass fiber cloth of 1 to 4 μm.
[0052] Furthermore, the composite crosslinking agent is at least two of methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, phenyltriacetylsilane, vinyltributylanoxime silane or tetrabutylketoxime silane. Preferably, it is a combination of methyltriethoxysilane and vinyltrimethoxysilane in a ratio of 1:(1-2). Vinyltrimethoxysilane has a fast hydrolysis rate and can react to remove trace moisture in the material, so it is also used as a dehydrating agent. The hydrolysis rate of methyltrimethoxysilane is not fast. The combined use of the two crosslinking agents can remove water that may be present in the material on the one hand to avoid self-curing, and on the other hand, the curing speed of the sealing material can be regulated.
[0053] Furthermore, the first coupling agent is a long-chain or cycloalkyl silane such as hexadecyltrimethoxysilane and dodecyltrimethoxysilane, preferably dodecyltrimethoxysilane, which is easy to form silanol groups at high temperatures and can well modify the surface of solid materials. The second coupling agent is at least one of KH-540, KH-550 or KH-570, preferably KH-550, which can effectively improve the adhesion and weather resistance of fireproof sealing materials.
[0054] Furthermore, the first gas generating agent and the second gas generating agent are at least one of ammonium carbonate, azobisisobutyronitrile, azodicarbonamide (gas generating agent AC), N,N"-dinitrosopentamethylenetetramine (gas generating agent DPT), preferably gas generating agent AC and gas generating agent DPT. Gas generating agent AC and gas generating agent DPT are both high-efficiency foaming gas generating agents, which decompose under heat to produce a large amount of non-flammable nitrogen, carbon dioxide, etc., and promote the formation of an expandable porous ceramic material.
[0055] Furthermore, the catalyst is at least one of stannous chloride, dibutyltin dilaurate, dibutyltin diacetate or stannous octoate, preferably dibutyltin dilaurate.
[0056] The fireproof sealant prepared in this embodiment has excellent fire resistance, can withstand high temperatures of 1200-1500° C., has a fire resistance time of greater than or equal to 180 minutes, a combustion grade of V0, and a limiting oxygen index of greater than or equal to 40%.
[0057] In a second aspect, the present invention provides a method for preparing a high-strength fireproof sealant, comprising the following steps:
[0058] (1) mixing a composite flame retardant, a composite fireproof filler, and a composite inorganic filler in a ratio of (1-2): (1-2): (0.5-1) to obtain 700-1200 parts of a mixture, and then placing the mixture and 10-15 parts of glass fibers in a vacuum oven, respectively, and removing water at 120-160° C. in a vacuum oven for 4-6 hours;
[0059] (2) placing the mixed material after high-temperature vacuum dehydration into a stirring device, and using 10 to 20 parts of dodecyltrimethoxysilane for dry modification for 1 to 2 hours at a temperature not lower than 80 to 90° C.;
[0060] (3) adding 350 to 600 parts of α, ω-dihydroxy polydimethylsiloxane and 50 to 200 parts of 201 silicone oil into the mixture of step (2), stirring well, then heating and maintaining at 90 to 95° C. and stirring well, then removing water under vacuum for 2 to 4 hours to obtain a mixture;
[0061] (4) cooling the mixture to 20-40° C., then adding 10-15 parts of glass fiber and mixing evenly;
[0062] (5) After step (4), 10 to 40 parts of a composite crosslinking agent are added thereto respectively, and after stirring for 5 to 15 minutes, 10 to 20 parts of KH-550 are added thereto, and after stirring for 5 to 15 minutes, 5 to 10 parts of a gas generating agent AC and 5 to 10 parts of a gas generating agent DPT are added thereto, and after stirring for 5 to 15 minutes, 0.5 to 2 parts of dibutyltin dilaurate are added thereto, and after mixing and stirring for 5 to 10 minutes, the high-strength fireproof sealant is obtained.
[0063] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0064] Example 1
[0065] A high-strength fireproof sealant comprising the following raw materials in parts by weight:
[0066] 400 parts of α, ω-dihydroxy polydimethylsiloxane (100,000 viscosity), 70 parts of 201 silicone oil (100 viscosity), 400 parts of flame retardant (aluminum hydroxide: aluminum hypophosphite: melamine cyanurate: zinc borate = 1:4:5:10), 400 parts of fireproof filler (glass fiber powder: sodium silicate: kaolin = 1:3:1), 150 parts of inorganic filler (calcium carbonate: white carbon black = 6:1), 10 parts of glass fiber (6μm chopped glass fiber), 25 parts of crosslinking agent (methyltriethoxysilane: vinyltrimethoxysilane = 1:2), 10 parts of dodecyltrimethoxysilane, 10 parts of KH-550, 5 parts of gas generator AC, 5 parts of gas generator DPT, and 2 parts of dibutyltin dilaurate.
[0067] The method for preparing the high-strength fireproof sealant comprises the following steps:
[0068] (1) 400 parts of flame retardant, 400 parts of fireproof filler and 150 parts of inorganic filler were uniformly mixed to obtain 950 parts of a mixture, and then the mixture and 10 parts of 6 μm chopped glass fibers were placed in a vacuum oven respectively, and water was removed at 140° C. under vacuum;
[0069] (2) placing the mixture after high-temperature vacuum dehydration in a stirring device, and dry-modifying it with 10 parts of dodecyltrimethoxysilane at 80° C. for 1 hour;
[0070] (3) adding 400 parts of 100000 viscosity α, ω-dihydroxy polydimethylsiloxane and 70 parts of 100 viscosity 201 silicone oil into the mixed material of step (2), stirring thoroughly, then heating and maintaining 90° C. and stirring thoroughly, then removing water in vacuo for 2 hours to obtain a mixture;
[0071] (4) Cooling the mixture to 30° C., then adding 10 parts of glass fiber and mixing evenly;
[0072] (5) After step (4), 25 parts of a cross-linking agent were added thereto, and after stirring for 5 minutes, 10 parts of KH-550 were added thereto, and after stirring for 5 minutes, 5 parts of a gas generating agent AC and 5 parts of a gas generating agent DPT were added thereto, and after stirring for 57 minutes, 2 parts of dibutyltin dilaurate were added thereto, and after mixing and stirring for 5 minutes, the high-strength fire-retardant sealant was obtained.
[0073] Example 2
[0074] A high-strength fireproof sealant comprising the following raw materials in parts by weight:
[0075] 500 parts of α, ω-dihydroxy polydimethylsiloxane (200,000 viscosity), 80 parts of 201 silicone oil (100 viscosity), 450 parts of flame retardant (magnesium hydroxide: diethyl aluminum hypophosphite: melamine polyphosphate: zinc borate = 1:3:6:10), 500 parts of fireproof filler (glass fiber powder: silicon carbide = 1:2), 150 parts of inorganic filler (calcium carbonate: carbon black = 6:1), 10 parts of glass fiber (4μm chopped glass fiber), 25 parts of crosslinking agent (methyltriethoxysilane: vinyltrimethoxysilane = 1:2), 15 parts of dodecyltrimethoxysilane, 10 parts of KH-550, 6 parts of gas generator AC, 6 parts of gas generator DPT, and 2 parts of dibutyltin dilaurate.
[0076] The method for preparing the high-strength fireproof sealant comprises the following steps:
[0077] (1) 450 parts of flame retardant, 500 parts of fireproof filler and 150 parts of inorganic filler were uniformly mixed to obtain 1100 parts of a mixture, and then the mixture and 10 parts of 4 μm chopped glass fibers were placed in a vacuum oven and dehydrated at 140° C. for 4 hours;
[0078] (2) placing the mixture after high-temperature vacuum dehydration in a stirring device, and dry-modifying it with 15 parts of dodecyltrimethoxysilane at 80° C. for 1 hour;
[0079] (3) adding 500 parts of 200,000 viscosity α, ω-dihydroxy polydimethylsiloxane and 80 parts of 100 viscosity 201 silicone oil into the mixture of step (2), stirring thoroughly, then heating and maintaining at 90° C. while stirring thoroughly, and then removing water in vacuo for 2 hours to obtain a mixture;
[0080] (4) Cooling the mixture to 30° C., then adding 10 parts of glass fiber and mixing evenly;
[0081] (5) After step (4), 25 parts of a cross-linking agent were added thereto, and after stirring for 5 minutes, 10 parts of KH-550 were added thereto, and after stirring for 5 minutes, 6 parts of a gas generating agent AC and 6 parts of a gas generating agent DPT were added thereto, and after stirring for 5 minutes, 2 parts of dibutyltin dilaurate were added thereto, and after mixing and stirring for 5 minutes, the high-strength fire-retardant sealant was obtained.
[0082] Example 3
[0083] A high-strength fireproof sealant comprising the following raw materials in parts by weight:
[0084] 450 parts of α, ω-dihydroxy polydimethylsiloxane (500,000 viscosity), 100 parts of 201 silicone oil (50 viscosity), 400 parts of flame retardant (ammonium polyphosphate: melamine polyphosphate: zinc borate = 2:2:5), 500 parts of fireproof filler (glass fiber powder: aluminum silicate: montmorillonite = 1:3:1), 100 parts of inorganic filler (talcum powder: iron red = 6:1), 10 parts of glass fiber (2μm2 glass fiber cloth), 30 parts of cross-linking agent (methyltriethoxysilane: vinyltrimethoxysilane = 1:1), 12 parts of dodecyltrimethoxysilane, 10 parts of KH-550, 5 parts of gas generating agent AC, 8 parts of gas generating agent DPT, and 1 part of dibutyltin dilaurate.
[0085] The method for preparing the high-strength fireproof sealant comprises the following steps:
[0086] (1) 400 parts of flame retardant, 500 parts of fireproof filler and 100 parts of inorganic filler were uniformly mixed to obtain 1000 parts of a mixture, and then the mixture and 10 parts of 2 μm2 chopped glass fibers were placed in a vacuum oven respectively, and dehydrated at 140° C. for 4 hours;
[0087] (2) placing the mixture after high-temperature vacuum dehydration in a stirring device, and dry-modifying it with 12 parts of dodecyltrimethoxysilane at 85° C. for 1 hour;
[0088] (3) adding 450 parts of 500000 viscosity α, ω-dihydroxy polydimethylsiloxane and 100 parts of 50 viscosity 201 silicone oil into the mixed material of step (2), stirring thoroughly, then heating and maintaining 90° C. stirring thoroughly, and then removing water in vacuo for 2 hours to obtain a mixture;
[0089] (4) Cooling the mixture to 30° C., then adding 10 parts of glass fiber and mixing evenly;
[0090] (5) After step (4), 30 parts of a cross-linking agent were added thereto, and after stirring for 10 minutes, 10 parts of KH-550 were added thereto, and after stirring for 10 minutes, 5 parts of a gas generating agent AC and 8 parts of a gas generating agent DPT were added thereto, and after stirring for 10 minutes, 1 part of dibutyltin dilaurate was added thereto, and after mixing and stirring for 10 minutes, the high-strength fire-retardant sealant was obtained.
[0091] In order to have a clearer intuitive understanding of the quality of the products prepared by the present invention, the fire resistance and weather resistance of the products prepared in Examples 1-3 were analyzed and compared with a certain product on the market. The test standards followed GB / T23864-2009, GB / T2408-2008, GB / T2406.2-2009 and GB / T1040-2018. The test results are shown in the following table:
[0092] Comparison Table
[0093]
[0094] As can be seen from the above table, the basic configuration of the fireproof sealant prepared by this method can be maintained for more than 3 hours under high temperature fire, and can keep the temperature of the protected object below 180°C for up to 3 hours, and is much better than the control sample in terms of fire resistance time at 1200°C; from the perspective of flame retardancy and limiting oxygen index, the fireproof sealant belongs to the non-flammable grade, and the limiting oxygen index is much higher than the control sample; from the perspective of weather resistance test results, the fireproof sealant has good weather resistance, meets the use conditions of many occasions, and is better than the control sample; the fireproof sealant prepared by this method has good tensile strength and can cope with a certain degree of stress impact while maintaining integrity.
[0095] From the above, it can be seen that the fireproof sealant prepared by this method has fireproof performance, weather resistance and mechanical properties that meet the standards, is better than similar products on the market, meets the needs of use in various occasions, and is suitable for continuous industrial production.
[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high-strength fireproof sealant, characterized in that: The composition comprises the following components in parts by weight: α,ω-dihydroxypolydimethylsiloxane: 350-600 parts; 201 silicone oil: 50~200 parts; Composite flame retardant: 300~600 parts; Composite fireproof filler: 300~600 parts; Composite inorganic filler: 100~300 parts; Glass fiber: 10~15 parts; Composite cross-linking agent: 10~40 parts; The first coupling agent: 10-20 parts; Second coupling agent: 10-20 parts; First gas generating agent: 5~10 parts; Second gas generating agent: 5~10 parts; Catalyst: 0.5~2 parts; The composite flame retardant is at least two of ammonium polyphosphate, piperazine pyrophosphate, aluminum hypophosphite, diethyl aluminum hypophosphite, melamine polyphosphate, melamine cyanurate, aluminum hydroxide, magnesium hydroxide, zinc borate, silicon dioxide, titanium dioxide and expandable graphite; The composite fireproof filler is at least two of glass fiber powder, sodium silicate, aluminum silicate, calcium silicate, silicon carbide, wollastonite powder, kaolin and montmorillonite; The composite inorganic filler is at least two of calcium carbonate, talc, hydrotalcite, clay, white carbon black, carbon black and iron red; The viscosity of the α,ω-dihydroxy polydimethylsiloxane is at least one of the following three viscosity ranges: 1000-10000 viscous, 10000-100000 viscous, and 100000-500000 viscous; The viscosity of the 201 silicone oil is 50-200 viscous; The glass fiber is 3-6 μm chopped glass fiber or 1-4 μm glass fiber cloth; The composite crosslinking agent is at least two of methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, phenyltriacetylsilane, vinyltributylacetoximate silane and tetrabutylketoxime silane; The first coupling agent is hexadecyltrimethoxysilane, dodecyltrimethoxysilane or cycloalkylsilane; the second coupling agent is at least one of KH-540, KH-550 and KH-570; The first gas generating agent and the second gas generating agent are at least one of ammonium carbonate, azobisisobutyronitrile, azodicarbonamide and N,N'-dinitrosopentamethylenetetramine; the first gas generating agent and the second gas generating agent are used for thermal decomposition to generate nitrogen or carbon dioxide; The catalyst is at least one of stannous chloride, dibutyltin dilaurate, dibutyltin diacetate and stannous octoate; Wherein, the high-strength fireproof sealant is prepared by the following steps: The composite flame retardant, the composite fireproof filler and the composite inorganic filler are uniformly mixed in a preset ratio to obtain a mixed material, and then the mixed material and the glass fiber are respectively placed in a vacuum oven to perform vacuum dehydration at a temperature of 120 to 160° C.; The mixed material after vacuum dehydration is placed in a stirring device, and dry-modified using a first coupling agent at 80-90° C.; Add α, ω-dihydroxy polydimethylsiloxane and 201 silicone oil into the mixed material, stir well, then heat and maintain at 90-95° C. and stir well, then remove water in vacuo to obtain a mixture; The mixture is cooled to 20-40°C, and then glass fiber is added and mixed evenly; The composite cross-linking agent, the second coupling agent, the first gas generating agent, the second gas generating agent and the catalyst are respectively added into the mixture in measured amounts, and after being mixed evenly, the mixture is discharged to obtain a high-strength fireproof sealant.
2. A method for preparing a high-strength fireproof sealant, used for preparing the high-strength fireproof sealant as claimed in claim 1, characterized in that: The steps include: The composite flame retardant, the composite fireproof filler and the composite inorganic filler are uniformly mixed in a preset ratio to obtain a mixed material, and then the mixed material and the glass fiber are respectively placed in a vacuum oven to perform vacuum dehydration at a temperature of 120 to 160° C.; The mixed material after vacuum dehydration is placed in a stirring device, and dry-modified using a first coupling agent at 80-90° C.; Add α, ω-dihydroxy polydimethylsiloxane and 201 silicone oil into the mixed material, stir well, then heat and maintain at 90-95° C. and stir well, then remove water in vacuo to obtain a mixture; The mixture is cooled to 20-40°C, and then glass fiber is added and mixed evenly; The composite cross-linking agent, the second coupling agent, the first gas generating agent, the second gas generating agent and the catalyst are respectively added into the mixture in measured amounts, and after being mixed evenly, the mixture is discharged to obtain a high-strength fireproof sealant.
3. The method for preparing the high-strength fireproof sealant according to claim 2, characterized in that: The ratio of the composite flame retardant, the composite fireproof filler and the composite inorganic filler is (1-2): (1-2): (0.5-1), and the mixture is vacuum dehydrated at 120-160° C. and maintained for 4-6 hours.