A cleaning composition for sapphire substrate after polishing
By using a cleaning composition composed of inorganic alkali, Gemini polyether phosphate surfactant and penetrant, combined with ultrasonic conditions, the problem of removing various pollutants after polishing the sapphire substrate sheet is solved, and efficient cleaning and long life are achieved. Effective, reduce costs and improve environmental friendliness.
Patent Information
- Application Number
- CN202310050491.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-01
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-02-01
AI Technical Summary
The cleaning agent after polishing the existing sapphire substrate sheet cannot effectively remove contaminants such as grinding powder and wax scale, and the cleaning effect is poor when the hydration layer remains, making it difficult to remove multiple contaminants at one time, increasing the cleaning cost and difficulty.
Using a cleaning composition composed of inorganic base, Gemini type polyether phosphate surfactant, penetrant and dispersant, the cleaning solution is diluted 15-20 times under ultrasonic conditions, combining the chelation and dispersion of phosphate groups. , and the wettability of polyether chains, so as to achieve efficient removal of pollutants such as abrasive particles, wax scales and other contaminants on the surface of sapphire, and destroy hydrogen bonds of the hydrated layer to improve the cleaning effect.
It realizes the single-use removal of organic pollutants such as abrasive particles and wax scale, improves the cleaning effect and service life, reduces costs, and solves the problem of difficult cleaning caused by residual hydration layer, significantly improving the cleaning yield and environmental friendliness. .
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cleaning agents, and in particular relates to a cleaning agent composition used for polishing a sapphire substrate. Background Art
[0002] Sapphire is mainly composed of aluminum oxide, which belongs to the hexagonal crystal system and is anisotropic. It has a Mohs hardness of 9, second only to diamond, high mechanical properties such as thermal conductivity and strength, stable chemical properties, high resistivity and high dielectric properties, and is widely used in industry, national defense, scientific research and other fields. Sapphire single crystals can be used as infrared window materials, and can also be used as optical elements for experiments. For example, in the semiconductor field, sapphire single crystals have become the main substrate material for GaN-based optoelectronic devices. The cleanliness of its surface has a great influence on the life of optoelectronic devices. The particles on the surface will increase the surface roughness, increase the probability of dislocations and defects during the growth of epitaxial thin films, and charged particles such as metal ions attached to the surface will lead to a decrease in breakdown voltage, leakage, etc., causing the finished device to be scrapped. Therefore, improving the cleanliness of the sapphire surface is of great significance to improving its application value.
[0003] The surface flattening of sapphire is mainly achieved through chemical-mechanical polishing (CMP). CMP removes the surface material of sapphire wafers through the corrosion of polishing liquid and the grinding action of abrasive particles. The fresh surface after polishing is full of dangling bonds and has high surface activity. In addition, the sapphire surface is negatively charged and has stronger adsorption capacity than ordinary glass, making it difficult to remove the grinding powder, wax stains and other contaminants remaining on the surface of the processed sapphire.
[0004] In addition, under the alkaline conditions of the CMP process, A12O3 reacts with alkali to generate A1O2 - A hydration layer with a thickness of about 1 nm will continue to form on the surface of the sapphire substrate. The composition of this hydration layer is diaspore, with the chemical formula A12O3·nH2O (the chemical reaction process of diaspore formation: ), with a Mohs hardness of about 7, which is lower than that of sapphire. If the hydration layer is not removed in time after the CMP process, the hydration layer will form hydrogen bonds with the sapphire surface as the water on the surface of the sapphire substrate evaporates during the subsequent placement process, and the bonding effect is further enhanced. In addition, due to the strong adsorption of diaspore, the surface is easy to adsorb organic pollutants and particles. Its presence also blocks the wetting and cleaning of the sapphire substrate surface by the cleaning liquid, making the cleaning of the sapphire after polishing more difficult.
[0005] The various sapphire substrate cleaning agents currently on the market have the following disadvantages after polishing:
[0006] (1) The cleaning effect of grinding powder and polishing liquid is poor, and the cleaning life is short. Some particles still remain after cleaning, and multiple rewashing is required, resulting in increased machine and labor costs.
[0007] (2) It is impossible to remove abrasive particles and organic matter such as wax stains at the same time, and an additional special wax removal cleaning is required, which increases the cleaning cost.
[0008] (3) When there is a residual hydration layer, the cleaning power drops sharply, which is mainly manifested in the dense number of particles in the area where the hydration layer exists, and the cleaning effect is poor. Summary of the invention
[0009] In order to solve the above technical problems, the present invention provides a cleaning composition for sapphire substrates after polishing, which has good wax removal, chelation, cleaning, wetting, dispersion and other effects, and can effectively remove surface particles, wax stains, dust and other organic pollutants remaining after grinding and polishing of sapphire substrates at one time, and can solve the difficult cleaning problem caused by the residual "hydration layer" in the industry, and has the advantages of high product concentration, good cleaning effect, high cleaning yield, long service life, and environmental friendliness.
[0010] To achieve the above object, the present invention adopts the following technical solution:
[0011] A cleaning composition for a sapphire substrate after polishing, the cleaning composition is made of the following raw materials in percentage by mass: 3-15% inorganic base, 1-10% Gemini polyether phosphate surfactant, 1-5% penetrant, 1-8% dispersant, and the balance is water, calculated by taking the sum of percentage by mass as 100%.
[0012] Furthermore, the general structural formula of the Gemini type polyether phosphate surfactant is as follows:
[0013] , wherein n is an integer of 1 to 10. The preparation thereof comprises the following steps:
[0014] (1) Synthesis of triethanolamine oleic acid soap
[0015]
[0016] Mix oleic acid and triethanolamine in a molar ratio of 1.2:1 and heat to 120°C, react for 2.5 hours under stirring, then stop heating, keep warm for 15 minutes, and then cool to below 50°C to obtain triethanolamine oleic acid soap;
[0017] (2) Synthesis of intermediate I
[0018]
[0019] In a nitrogen atmosphere, a catalyst KOH is added to triethanolamine oleic acid soap and stirred and heated. After the temperature rises to 170°C, the initial pressure is recorded, and ethylene oxide is introduced at a molar ratio of 12:1 to the triethanolamine oleic acid soap until the system pressure is 0.3-0.4 MPa, and the reaction is carried out by heat preservation. When the reaction pressure drops to the initial pressure, the heating is stopped, and when the temperature drops below 80°C, the residual ethylene oxide in the reaction system is removed by vacuum to obtain intermediate I; wherein the amount of the catalyst is 4% of the molar amount of the triethanolamine oleic acid soap;
[0020] (3) Synthesis of Gemini-type polyether phosphate surfactant A
[0021]
[0022] P2O5 was added to the intermediate I in a molar ratio of 2:1 under stirring conditions, and the reaction was carried out at 70-80°C for 4 hours. Then, an appropriate amount of distilled water was added to hydrolyze the generated phosphate ester at 80°C for 2 hours, and then the solvent was evaporated. Then, an ethanol solution containing 20wt% NaOH was added to carry out neutralization reaction until the system pH was 7-8, and then the salt was removed with anhydrous ethanol, and the solvent was evaporated to obtain a Gemini-type polyether phosphate surfactant.
[0023] Furthermore, the inorganic base is one or more of potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, anhydrous sodium metasilicate, and ammonium hydroxide.
[0024] Furthermore, the penetrant is selected from one or more of OEP-70, OEP-98, AEP, and OE-35.
[0025] Furthermore, the dispersant is selected from one or more of sodium dodecylbenzene sulfonate (LAS), polycarboxylates, sodium acrylic acid homopolymer (PAAS), dioctyl sodium sulfosuccinate, polyvinyl alcohol, and polyvinyl pyrrolidone (PVP).
[0026] Furthermore, the water is deionized water with a resistance value greater than 16 MΩ / cm.
[0027] Furthermore, the preparation method of the cleaning composition is:
[0028] 1) Add water, inorganic base and dispersant in proportion, and stir at 200 rpm under normal pressure until the particles are completely dissolved;
[0029] 2) When the solution temperature drops below 60°C, continue to add the penetrant and Gemini polyether phosphate surfactant, and stir at normal pressure until the solution becomes a homogeneous system;
[0030] 3) Stop stirring and let the mixture stand until it reaches room temperature to obtain a transparent, clear and uniform composition.
[0031] The method of using the cleaning composition of the present invention is to dilute the cleaning composition with water by 15-20 times, then heat it to 80±5°C, use it to clean the polished sapphire substrate under 40khz ultrasonic conditions for 240s-480s, then spray rinse with room temperature water and then spin dry the sapphire substrate at room temperature.
[0032] Furthermore, the size of the sapphire substrate sheet is 4 inches.
[0033] The significant advantages of the present invention are:
[0034] (1) The structure of the Gemini polyether phosphate surfactant used in the present invention introduces phosphate hydrophilic groups and polyether chains. According to the principle of like dissolves like, the fatty acid groups in the surfactant can combine with organic pollutants such as wax stains on the surface of the substrate, and then soften and disperse into the cleaning liquid with the help of the hydrophilic groups, thereby achieving the effect of wax removal and decontamination. At the same time, the phosphate groups in its structure have chelating and dispersing effects, and can synergize with the dispersant in the system to show a strong particle removal ability. The introduction of the polyether chain further improves the wettability of the surfactant, and with the penetrant in the system, the surface tension of the composition is still less than 30mN / m after being diluted 15-20 times.
[0035] (2) After being ionized in the cleaning solution, the anionic dispersant used in the present invention has strong adsorption properties and can make the particle surface carry the same charge. Since the sapphire surface itself also carries a negative charge, the particles and the substrate surface can repel each other according to the electrostatic repulsion effect of the same charge. Therefore, under the synergistic effect of ultrasound, the particles adsorbed on the sapphire substrate sheet are washed off and suspended and dispersed in the cleaning solution, thereby achieving an excellent particle cleaning effect and preventing the occurrence of particle re-adhesion.
[0036] (3) The cleaning composition obtained by the present invention can remove organic pollution such as abrasive particles and wax stains at one time. The particle count of a 4-inch piece detected by AOI is less than 500, and there is no visible wax trace, so there is no need for an additional special wax removal cleaning.
[0037] (4) The high permeability and strong alkalinity of the cleaning composition obtained by the present invention can destroy the hydrogen bond structure formed by diaspore in the hydration layer, thereby solving the problem of stubborn stains caused by residual hydration layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 Comparison of particle adsorption on the surface of a sapphire substrate before (a) and after (b) cleaning with the cleaning composition obtained in Example 4;
[0039] Figure 2Comparative diagram of the hydrated layer adhesion on the surface of the sapphire substrate before (a) and after (b) cleaning with the cleaning composition obtained in Example 4. DETAILED DESCRIPTION
[0040] A cleaning composition for a sapphire substrate after polishing, the cleaning composition is made of the following raw materials in percentage by mass: 3-15% inorganic base, 1-10% Gemini polyether phosphate surfactant, 1-5% penetrant, 1-8% dispersant, and the balance is water, calculated by taking the sum of percentage by mass as 100%.
[0041] Wherein, the inorganic base is one or more of potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, anhydrous sodium metasilicate, and ammonium hydroxide.
[0042] The penetrant is selected from one or more of OEP-70, OEP-98, AEP, and OE-35.
[0043] The dispersant is selected from one or more of sodium dodecylbenzene sulfonate (LAS), polycarboxylates, sodium homopolymer of acrylic acid (PAAS), dioctyl sodium sulfosuccinate, polyvinyl alcohol, and polyvinyl pyrrolidone (PVP).
[0044] The water is deionized water with a resistance value greater than 16 MΩ / cm.
[0045] The general structural formula of the Gemini type polyether phosphate surfactant is as follows:
[0046] , wherein n is an integer of 1 to 10. The preparation thereof comprises the following steps:
[0047] (1) Synthesis of triethanolamine oleic acid soap: oleic acid and triethanolamine were added into a three-necked flask at a molar ratio of 1.2:1, heated to 120°C, reacted for 2.5 hours under stirring, then stopped heating, kept warm for 15 minutes, and then cooled to below 50°C to obtain triethanolamine oleic acid soap;
[0048] (2) Synthesis of intermediate I: Inhale triethanolamine oleic acid soap and catalyst KOH into a reactor filled with nitrogen, stir and heat to 170 °C, record the initial pressure, and introduce ethylene oxide at a molar ratio of 12:1 to triethanolamine oleic acid soap to start the induction reaction. When the system pressure reaches 0.3-0.4 MPa, keep the temperature to react. When the reaction pressure drops to the initial pressure, stop heating. When the temperature drops below 80 °C, evacuate the reaction system to remove the residual ethylene oxide, fill with nitrogen and discharge to obtain intermediate I; the amount of catalyst used is 4% of the molar amount of triethanolamine oleic acid soap;
[0049] (3) Synthesis of Gemini polyether phosphate surfactant A: P2O5 was added to the intermediate I in a molar ratio of 2:1 under stirring conditions. After reacting at 70-80°C for 4 h, an appropriate amount of distilled water was added to hydrolyze the generated phosphate ester at 80°C for 2 h. After that, the solvent was evaporated. An ethanol solution containing 20 wt% NaOH was added to carry out neutralization reaction until the system pH was 7-8. Then, the salt was removed with anhydrous ethanol and the solvent was evaporated to obtain a Gemini polyether phosphate surfactant.
[0050] The preparation method of the cleaning composition is:
[0051] 1) Add water, inorganic base and dispersant in proportion, and stir at 200 rpm under normal pressure until the particles are completely dissolved;
[0052] 2) When the solution temperature drops below 60°C, continue to add the penetrant and Gemini polyether phosphate surfactant, and stir at normal pressure until the solution becomes a homogeneous system;
[0053] 3) Stop stirring and let the mixture stand until it reaches room temperature to obtain a transparent, clear and uniform composition.
[0054] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.
[0055] Example:
[0056] A cleaning composition for a sapphire substrate after polishing, the preparation method of which is as follows:
[0057] (1) Prepare inorganic base, Gemini polyether phosphate surfactant, penetrant, dispersant and water according to the proportions in Table 1;
[0058] (2) Add water, inorganic base and dispersant to a stirring kettle in sequence, and stir at a speed of 200 rpm under normal pressure until the particles are completely dissolved;
[0059] (3) When the solution temperature drops below 60°C, continue to add the penetrant and Gemini polyether phosphate surfactant, and stir at normal pressure until the solution becomes a homogeneous system;
[0060] (4) Stop stirring and let the mixture stand until it reaches room temperature to obtain a transparent, clear and uniform composition.
[0061] The preparation steps of the Gemini type polyether phosphate surfactant used are as follows:
[0062] (1) Add 0.12 mol oleic acid and 0.1 mol triethanolamine into a three-necked flask, heat to 120°C, react for 2.5 hours under stirring, then stop heating, keep warm for 15 minutes, and then cool to below 50°C to obtain triethanolamine oleic acid soap;
[0063] (2) In a nitrogen-filled kettle, 0.1 mol of triethanolamine oleic acid soap and 4 mmol of catalyst KOH were sucked in, and after stirring and heating to 170°C, the initial pressure was recorded, and 1.2 mol of ethylene oxide was introduced until the system pressure reached 0.3-0.4 MPa, and the reaction was carried out by heat preservation. When the reaction pressure dropped to the initial pressure, heating was stopped, and when the temperature dropped below 80°C, the residual ethylene oxide in the reaction system was removed by vacuum, and nitrogen was introduced to discharge the product to obtain intermediate I (n=6);
[0064] (3) 0.1 mol of intermediate I and 0.05 mol of P2O5 were added under stirring conditions, reacted at 70°C for 4 h, 500 ml of distilled water was added, the generated phosphate was hydrolyzed at 80°C for 2 h, and the solvent was evaporated. Then, an ethanol solution containing 20 wt% NaOH was added to carry out neutralization reaction until the system pH was 7-8, and then the salt was removed with anhydrous ethanol, and the solvent was evaporated to obtain Gemini type polyether phosphate surfactant A (n=6), whose structural characterization data are as follows:
[0065] 1 H NMR (300Mhz, DMSO-d6), δ: 0.88 (m, 3H, CH3), 1.26 (m, 24H, CH2), 1.29 (m, 4H, CH2), 1 .30(m,2H,CH2), 1.33(m,2H,CH2), 1.66(t,2H,CH2), 2.16(m,4H,CH2), 2.32(t,2H, CH2), 2.51(t, 4H, CH2), 2.97 (t, 2H, CH2), 3.51 (m, 4H, CH2), 3.52 (m, 40H, CH2), 3.7 2(t, 2H, CH2), 4.20 (m, 4H, CH2), 4.35 (m, 2H, CH2), 4.80 (s, 2H, OH), 5.43 (m, 2H, CH);
[0066] 13 C NMR (125Mhz, DMSO-d6), δ: 14.1, 22.7, 25.0, 29.0, 29.4, 29.7, 29.9, 33.7, 33.9, 51.1, 54.8, 62.1, 64.8, 68.1, 69.7, 69.8, 70.1, 70.4, 130.6, 173.1;
[0067] HRMS calculated value C 48 H95 O 20 P2Na2(M+H) + :1099.56, measured value:1100.57.
[0068] Table 1 Components and their contents in different cleaning agent compositions
[0069]
[0070] The 4-inch sapphire substrate with polishing abrasive and residual wax on the surface after polishing was immersed in the cleaning agent composition prepared in Examples 1-6 and Comparative Examples 1-6, respectively, and ultrasonically cleaned under the set dilution multiple, temperature, and time ultrasonic conditions, and then rinsed with ultrapure water spray, and then spin dried. The cleaning effect was confirmed by observation under a metallographic microscope. The operating conditions and results are shown in Table 2.
[0071] Table 2 Cleaning effect of different cleaning agent compositions on polished sapphire substrates
[0072]
[0073] It can be seen from Tables 1-2 that within the set temperature and time, the cleaning agent composition of the present invention can effectively remove residual polishing powder, abrasives, wax and other organic pollutants on the sapphire substrate to obtain a clean surface with extremely low particle count, and the liquid is easy to rinse without residue.
[0074] Compared with Example 4, Comparative Example 1 does not contain an inorganic base, and under the same ultrasonic conditions, the number of surface particles is relatively large, which indicates that the non-alkaline conditions greatly reduce the wax removal effect of the liquid, resulting in an extremely low cleaning yield.
[0075] Compared with Example 4, Comparative Example 2 does not contain a penetrant. Under the same ultrasonic conditions, due to the decreased wettability of the liquid, its penetration and removal effect on part of the hydration layer is reduced, and the sapphire substrate sheet with residual hydration layer is difficult to clean, resulting in a reduced cleaning yield.
[0076] Compared with Example 4, Comparative Example 3 does not contain a dispersant. Under the same ultrasonic conditions, due to the decrease in the dispersing power of the liquid, its particle removal effect is greatly reduced, and a large number of particles remain attached to the surface of the sapphire substrate, resulting in a decrease in the cleaning yield.
[0077] Compared with Example 4, Comparative Example 4 does not contain a Gemini polyether phosphate surfactant. Under the same ultrasonic conditions, the wax removal and particle removal properties of the liquid are greatly affected, resulting in a very poor cleaning yield.
[0078] Compared with Example 4, Comparative Example 5 uses triethanolamine oleic acid soap as a surfactant. Under the same ultrasonic conditions, the wax removal ability of the solution is similar, but the lack of polyether groups in the structure weakens the wettability, and the lack of phosphate groups partially affects the dispersibility and particle removal ability of the solution, thereby reducing the cleaning yield.
[0079] Compared with Example 4, Comparative Example 6 uses intermediate I as a surfactant. Under the same ultrasonic conditions, although the wettability and wax removal ability of the solution are similar, due to the lack of phosphate groups, the dispersibility and particle removal ability of the solution are partially affected, thereby reducing the cleaning yield.
[0080] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A cleaning composition for a sapphire substrate after polishing, characterized in that: The composition is made of the following raw materials in percentage by weight, calculated by taking the sum of percentage by weight as 100%: 3-15% inorganic base, 1-10% Gemini polyether phosphate surfactant, 1-5% penetrant, 1-8% dispersant, and the balance water; The preparation of the Gemini type polyether phosphate surfactant comprises the following steps: (1) Synthesis of triethanolamine oleic acid soap: oleic acid and triethanolamine were mixed at a molar ratio of 1.2:1 and heated to 120°C. After stirring for 2.5 hours, the heating was stopped, the temperature was kept at 15 minutes, and the temperature was then lowered to below 50°C to obtain triethanolamine oleic acid soap. (2) Synthesis of intermediate I: Under nitrogen atmosphere, add catalyst KOH to triethanolamine oleic acid soap and stir and heat. When the temperature rises to 170°C, record the initial pressure, and introduce ethylene oxide at a molar ratio of 12:1 to triethanolamine oleic acid soap until the system pressure reaches 0.3-0.4 MPa. Keep the temperature to react. When the reaction pressure drops to the initial pressure, stop heating. When the temperature drops below 80°C, remove the residual ethylene oxide in the reaction system by vacuum to obtain intermediate I. The amount of catalyst used is 4% of the molar amount of triethanolamine oleic acid soap. (3) Synthesis of Gemini polyether phosphate surfactant A: P2O5 was added to the intermediate I in a molar ratio of 2:1 under stirring conditions, and reacted at 70-80°C for 4 h. An appropriate amount of distilled water was added to hydrolyze the generated phosphate ester at 80°C for 2 h, and then the solvent was evaporated. An ethanol solution containing 20 wt% NaOH was added to neutralize the reaction until the system pH was 7-8. The salt was then removed with anhydrous ethanol, and the solvent was evaporated to obtain a Gemini polyether phosphate surfactant. The general structural formula is as follows: , where n is an integer from 1 to 10; The inorganic base is one or more of potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, anhydrous sodium metasilicate, and ammonium hydroxide; The penetrant is selected from one or more of OEP-70, OEP-98, AEP, and OE-35; The dispersant is selected from one or more of sodium dodecylbenzene sulfonate, polycarboxylate, sodium salt of acrylic acid homopolymer, dioctyl sodium sulfosuccinate, polyvinyl alcohol, and polyvinyl pyrrolidone.
2. A cleaning composition for polishing a sapphire substrate according to claim 1, characterized in that: The water is deionized water with a resistance value greater than 16 MΩ / cm.
3. The cleaning composition for polishing a sapphire substrate according to claim 1, characterized in that: The preparation method of the cleaning composition is: 1) Add water, inorganic base and dispersant in proportion, and stir at 200 rpm under normal pressure until the particles are completely dissolved; 2) When the solution temperature drops below 60°C, continue to add the penetrant and Gemini polyether phosphate surfactant, and stir at normal pressure until the solution becomes a homogeneous system; 3) Stop stirring and let the mixture stand until it reaches room temperature to obtain a transparent, clear and uniform composition.
Citation Information
Patent Citations
Sapphire cleaning agent
CN104818142A
Preparation method and application of Gemini type polyether phosphate ester
CN106928445A
Sapphire wafer cleaning agent and preparation method thereof
CN114106934A
Method for cleaning semiconductor substrate
JP2012104671A
Surface-modified metal oxide particle material, dispersion liquid, silicone resin composition, silicone resin composite, optical semiconductor light-emitting device, lighting device, and liquid crystal imaging device