Amorphous alloy modified magnesium-aluminum-zinc alloy and preparation method thereof
By adding rare earth elements and zirconium-based amorphous alloys to magnesium-aluminum-zinc alloys, grain refinement is achieved, which solves the problem of insufficient composite properties of magnesium alloys, significantly improves strength, plasticity and heat resistance, and improves processing performance.
Patent Information
- Application Number
- CN202211521280.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-11-30
AI Technical Summary
The composite properties of existing magnesium alloys are not excellent enough, especially in terms of yield strength and heat resistance, and the melting and dispersion effect of iron-based amorphous alloys is poor, resulting in insignificant improvements in strength and hardness.
By adding rare earth elements and zirconium-based amorphous alloy to the magnesium-aluminum-zinc alloy, adjusting its composition to achieve grain refinement and improving the composite properties of the magnesium-aluminum-zinc alloy, the amorphous alloy powder is used for modification during the melting process. , combined with the segregation effect of rare earth elements, promotes uniform grain formation and dispersion.
It significantly improves the strength, plasticity, hardness and toughness of the magnesium-aluminum-zinc alloy, improves the processing performance and corrosion resistance, enhances the heat resistance and impact toughness of the magnesium-aluminum-zinc alloy, and reduces oxidation problems during the melting process.
Smart Images

Figure CN116083766B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new materials, and more specifically to an amorphous alloy-modified magnesium-aluminum-zinc alloy and a preparation method thereof. Background Art
[0002] Magnesium alloy is an alloy composed of magnesium and other elements. Its characteristics are: low density (1.8g / cm 3 It has high strength, large elastic modulus, good heat dissipation, good shock absorption, greater impact load bearing capacity than aluminum alloy, and good resistance to organic and alkali corrosion. The main alloying elements are aluminum, zinc, manganese, cerium, thorium, and a small amount of zirconium or cadmium. The most widely used is magnesium-aluminum alloy, followed by magnesium-manganese alloy and magnesium-zinc-zirconium alloy. It is mainly used in aviation, aerospace, transportation, chemical industry, rocket and other industrial sectors.
[0003] Magnesium-aluminum-zinc alloy is the earliest and most widely used high-strength and tough magnesium alloy in industrial production. It is processed into plates, bars, profiles and forgings. The alloy grades belonging to this series include AZ31, AZ61, AZ80, AZ91, etc. The main characteristics of MgAlZn alloy are high strength, ability to be strengthened by heat treatment, and good casting performance. The disadvantages are low yield strength and poor heat resistance.
[0004] CN 113493876 B discloses a method for modifying the surface of a magnesium alloy with an iron-based amorphous material. In the composite materials of different magnesium alloy surfaces reinforced with FeCrMoBC amorphous particles prepared by this method, the FeCrMoBC amorphous particles are well dispersed in the magnesium alloy matrix, and are well combined with the magnesium alloy matrix, and have stable performance. The plasticity and processing properties of the magnesium alloy obtained by this method for modifying the surface of a magnesium alloy with an iron-based amorphous material are improved. However, because the proportion of the iron-based amorphous alloy that can be dispersed is small, and experiments have verified that the melting dispersion effect of the iron-based amorphous alloy is poor, the improvement of the mechanical properties of the magnesium alloy, such as the strength and hardness, is not significant. Summary of the invention
[0005] The present invention aims to solve the technical problem that the composite properties of common magnesium alloys in the prior art are not good enough. By studying the addition of rare earth elements of different components and modifying by adding zirconium-based amorphous alloys, the composite properties of magnesium alloys are improved to obtain an amorphous alloy-modified magnesium-aluminum-zinc alloy.
[0006] Those skilled in the art know that grain refinement is one of the main ways to improve the composite properties of high-strength and tough magnesium alloys and improve the forming properties of magnesium alloys. Because according to the Hall-patch general formula: σy = σ0 + kd ~ 1 / 2, where σy is the yield strength of the material, σ0 is the yield strength of a single crystal, d is the grain size, and k is a constant. It can be inferred from the above formula that the finer the grains, the smaller the dendrite spacing, the higher the yield strength, and the better the hardness. In addition, grain refinement can reduce micro-shrinkage, hot cracking tendency, improve corrosion resistance and product processing performance, and uniform and fine equiaxed crystals are also the key to achieving superplasticity of magnesium alloys. At present, the more feasible way to refine the grains of magnesium alloys is grain refinement during the casting process. Grain refinement during the casting process is to refine the grains by adding an appropriate amount of modifiers or metal elements to the magnesium alloy melt before casting, thereby improving and improving the processing properties of the alloy.
[0007] In the process of studying the grain refinement of magnesium alloy melt, the present invention experimentally verifies that adding certain types of amorphous alloys to the magnesium alloy melt can better improve the composite properties of the magnesium alloy than metal elements. On this basis, the magnesium alloy is modified by adding amorphous alloy elements of different types and compositions to obtain an amorphous alloyed magnesium-aluminum-zinc alloy with high strength and toughness.
[0008] Accordingly, the present invention provides an amorphous alloy modified magnesium-aluminum-zinc alloy, wherein the amorphous alloy modified magnesium-aluminum-zinc alloy comprises a first component and a second component, wherein the weight percentage of the first component is 82-90%, and the weight percentage of the second component is 10%-18%; wherein the first component is magnesium-aluminum-zinc alloy, and based on 100 parts by weight of magnesium-aluminum-zinc alloy, the content of each component in the magnesium-aluminum-zinc alloy is: aluminum: 7.25-8.48 parts by weight; zinc: 1.35-1.58 parts by weight; rare earth elements: 1.80-2.50 parts by weight; the balance is magnesium; the second component is a zirconium-based amorphous alloy, and the composition of the zirconium-based amorphous alloy is shown in the following general formula: Zr a Al b Cu c Ni d M e N f , wherein M is one or more of Sc, Y, La, and Ce, N is one or more of Group VIII elements, 30≤a≤60, 10≤b≤30, 10≤c≤20, 10≤d≤20, 0≤e≤20, 0≤f≤10, and a+b+c+d+e+f=100, and a, b, c, d, e, and f are mole percentages.
[0009] In the amorphous alloy modified magnesium-aluminum-zinc alloy, preferably, the rare earth element is a lanthanide element, and the weight percentage is 2.15 to 2.50 parts by weight.
[0010] In the amorphous alloy modified magnesium-aluminum-zinc alloy, preferably, the rare earth element is one or more of La, Pr and Nd.
[0011] In the amorphous alloy modified magnesium-aluminum-zinc alloy, preferably, the composition of the zirconium-based amorphous alloy is as shown in the following general formula: Zr a Al b Cu c Ni d M e N f , wherein M is one or more of Y, La, and Ce, N is one or more of Fe and Co, 40≤a≤50, 20≤b≤30, 10≤c≤15, 10≤d≤20, 5≤e≤15, 5≤f≤10, and a+b+c+d+e+f=100, and a, b, c, d, e, and f are mole percentages.
[0012] In the amorphous alloy modified magnesium-aluminum-zinc alloy, preferably, calculated by weight percentage, the weight percentage of the first component is 82-85%, and the weight percentage of the second component is 12-15%.
[0013] The present invention also provides a method for preparing the above-mentioned amorphous alloy modified magnesium-aluminum-zinc alloy, comprising the following steps:
[0014] Step 1: melt an amorphous alloy raw material in a protective gas environment, cool it and form it to obtain an amorphous alloy powder. The amount of the amorphous alloy raw material added satisfies the composition ratio shown in the following general formula: Zr a Al b Cu c Ni d M e N f , wherein M is one or more of Sc, Y, La, and Ce, N is one or more of Group VIII elements, 30≤a≤60, 10≤b≤30, 10≤c≤20, 10≤d≤20, 0≤e≤20, 0≤f≤10, and a+b+c+d+e+f=100, and a, b, c, d, e, and f are mole percentages;
[0015] Step 2, using amorphous alloy powder as the second component, and using the raw material of cast magnesium-aluminum-zinc alloy as the first component, calculated by weight percentage, the weight percentage of the second component is 10% to 18%, and the weight percentage of the first component is 82 to 90%; based on 100 parts by weight of magnesium-aluminum-zinc alloy, the content of each component in the magnesium-aluminum-zinc alloy is: aluminum: 7.25 to 8.48 parts by weight; zinc: 1.35 to 1.58 parts by weight; rare earth elements 1.80 to 2.50 parts by weight; the balance is magnesium; the magnesium-aluminum-zinc alloy raw material is melted, the amorphous alloy powder is added during the melting process, and then refined and cast to obtain the amorphous alloy-modified magnesium-aluminum-zinc alloy.
[0016] In the preparation method of the amorphous alloy modified magnesium-aluminum-zinc alloy, preferably, the composition of the amorphous alloy powder is as shown in the following general formula: Zr a Al b Cu c Ni d M e N f , wherein M is one or more of Y, La, and Ce, N is one or more of Fe and Co, 40≤a≤50, 20≤b≤30, 10≤c≤15, 10≤d≤20, 5≤e≤15, 5≤f≤10, and a+b+c+d+e+f=100, a, b, c, d, e, and f are molar percentages; the rare earth element is one or more of La, Pr, and Nd.
[0017] In the method for preparing the amorphous alloy modified magnesium-aluminum-zinc alloy, preferably, the rare earth element is a lanthanide element, and the weight percentage is 2.15 to 2.50 parts by weight.
[0018] In the method for preparing the amorphous alloy modified magnesium-aluminum-zinc alloy, preferably, the rare earth element is one or more of La, Pr and Nd.
[0019] In the method for preparing the amorphous alloy modified magnesium-aluminum-zinc alloy, preferably, calculated in weight percentage, the weight percentage of the first component is 82-85%, and the weight percentage of the second component is 12-15%.
[0020] The present invention adopts Zr-based amorphous alloy powder to perform modification treatment in the preparation process of MgAlZn series magnesium-aluminum-zinc alloy, the amorphous alloy powder is a modified ZrAlCuNi series amorphous alloy, the magnesium-aluminum-zinc alloy is a MgAlZn series magnesium alloy modified by adding rare earth elements, and the rare earth elements and ZrAlCuNi series amorphous alloy powder in the melting process of the magnesium-aluminum-zinc alloy can achieve the effect of refining grains and improving alloy structure; through mechanical property detection, the strength, plasticity, hardness and toughness of the magnesium-aluminum-zinc alloy modified by the amorphous alloy of the present invention are improved compared with the magnesium-aluminum-zinc alloy without adding amorphous alloy, and it is conducive to later processing and forming. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a metallographic microscope photograph of the amorphous alloy-modified magnesium-aluminum-zinc alloy of Example 1 of the present invention.
[0022] Figure 2 It is a metallographic microscope photograph of the magnesium alloy of comparative example 1 of the present invention.
[0023] Figure 3 It is a metallographic microscope photograph of the magnesium alloy of comparative example 2 of the present invention. DETAILED DESCRIPTION
[0024] The present invention is further described below in conjunction with embodiments, tables and drawings.
[0025] The present invention has found through experimental research that adding a certain amount of specific amorphous alloy powder to a specific magnesium-aluminum-zinc alloy for melting and casting can improve the composite properties of the magnesium-aluminum-zinc alloy. The present invention provides an amorphous alloy-modified magnesium-aluminum-zinc alloy, wherein the amorphous alloy-modified magnesium-aluminum-zinc alloy comprises a first component and a second component, wherein the weight percentage of the first component is 82-90%, and the weight percentage of the second component is 10%-18%; the first component is a magnesium-aluminum-zinc alloy, and the second component is a zirconium-based amorphous alloy.
[0026] Among them, the magnesium-aluminum-zinc alloy selects a magnesium-aluminum-zinc alloy containing rare earth elements. Based on 100 parts by weight of the magnesium-aluminum-zinc alloy, the content of each component in the magnesium-aluminum-zinc alloy is: aluminum: 7.25-8.48 parts by weight, zinc: 1.35-1.58 parts by weight, rare earth elements: 1.80-2.50 parts by weight, and the balance is magnesium. It is inevitable that it will contain trace amounts (less than 0.05 parts by weight) of impurities such as Si, Ni, Ca, and Mn. In a preferred case, in order to obtain a magnesium-aluminum-zinc alloy with better composite properties, the chemical composition of the amorphous alloy-modified magnesium-aluminum-zinc alloy is calculated by weight: aluminum: 8.18-8.48 parts by weight; zinc: 1.35-1.45 parts by weight; rare earth elements 2.15-2.50 parts by weight; the balance is magnesium. The present invention can improve the morphology and distribution of the second phase in the MgAlZn alloy by adding rare earth elements, so that the amorphous alloy powder is more evenly dispersed in the process of magnesium-aluminum-zinc alloying, the bonding effect is better, and the appearance of pores is avoided.
[0027] In a preferred case, the rare earth element is a lanthanide element, and the weight portion is 2.15 to 2.50 weight portions; adding a preferred content of lanthanide elements can obtain a magnesium-aluminum-zinc alloy with a better high-toughness composite component. When the lanthanide rare earth element is added as a modifier, during the solidification process, the segregation effect reduces the equilibrium liquidus temperature of the solid-liquid interface, reduces the supercooling of the components at the interface, reduces the interface energy, and inhibits the growth of crystals on the interface, promotes the formation of crystal nuclei, hinders crystal growth, and can refine the grains; and when melted, the addition of amorphous alloy powders produces a synergistic effect that can further significantly refine the grains and effectively improve the performance of the magnesium-aluminum-zinc alloy. In addition, due to the active nature of the lanthanide rare earth elements, during the melting process, they react with oxygen and active gases to generate products floating on the surface of the reaction melt, which can well solve the oxidation and burning problems of magnesium elements in the melting process of the magnesium-aluminum-zinc alloy. In a more preferred case, the rare earth element uses one or more of the light rare earth elements La, Pr, and Nd. The combination of light rare earth elements and MgAlZn alloys is better, which can significantly change the distribution of the second phase at the grain boundary in the organization, making the grain boundary less likely to be destroyed, and can improve the corrosion resistance of the magnesium-aluminum-zinc alloy to a certain extent. The best effect is achieved when the weight ratio of Pr and Nd is 1: (1.5-2). It has been verified that adding a composite ratio of Pr and Nd can reduce the gravity segregation problem in the organization, effectively improve the heat resistance of the magnesium-aluminum-zinc alloy, and thus significantly improve the processing properties including impact toughness and extrusion speed.
[0028] In the present invention, the second component is a zirconium-based amorphous alloy, and the composition of the zirconium-based amorphous alloy is shown in the following general formula: Zr a Al b Cu c Ni d M e Nf , wherein M is one or more of Sc, Y, La, Ce, N is one or more of Group VIII elements, 30≤a≤60, 10≤b≤30, 10≤c≤20, 10≤d≤20, 0≤e≤20, 0≤f≤10, and a+b+c+d+e+f=100, a, b, c, d, e, f are molar percentages. Zirconium-based amorphous alloys have high tensile strength, elastic energy, impact fracture performance, corrosion resistance, good ductility, and excellent inherent low-frequency vibration damping performance. Zirconium element Zr has super strong corrosion resistance, high temperature resistance, and nuclear radiation resistance. The amorphous alloy composed of ZrAlCuNi is a Zr-based alloy system with excellent composite performance. In the present invention, the addition of M and N elements to the amorphous alloy composed of ZrAlCuNi can correspondingly make the zirconium-based amorphous alloy have enhanced specific properties to meet the needs of various excellent properties of magnesium-aluminum-zinc alloys.
[0029] In the present invention, preferably, the composition of the zirconium-based amorphous alloy is as shown in the following general formula: Zr a Al b Cu c Ni d M e N f , wherein M is one or more of Y, La, and Ce, N is one or more of Fe and Co, 40≤a≤50, 20≤b≤30, 10≤c≤15, 10≤d≤20, 5≤e≤15, 5≤f≤10, and a+b+c+d+e+f=100, a, b, c, d, e, and f are molar percentages. The zirconium-based amorphous alloy of the preferred components of the present invention also has good dynamic compression performance, electrocatalytic activity, and positive strain rate effect, and has good electromagnetic properties after adding Fe. More preferably, when M is Y and N is Fe, and the molar percentage is (1 to 1.5): 1, the composite performance of the zirconium-based amorphous alloy is optimal. Adding amorphous alloy powder can more effectively refine the grains and purify the magnesium-aluminum-zinc alloy, and obtain a magnesium-aluminum-zinc alloy melt and finished product with more uniform composition and organization.
[0030] Although the larger the particle size of the amorphous alloy powder, the higher the proportion of the amorphous phase, the better the composite performance of the obtained amorphous alloy powder, in the present invention, the main role of the amorphous alloy is to add the amorphous alloy powder as the second component during the melting process of the magnesium-aluminum-zinc alloy for modification. Therefore, the present invention does not have high requirements on the composition and particle size of the amorphous alloy powder, and the production process adopts the conventional amorphous alloy powder production process in the field. Preferably, the volume percentage of the crystallized phase of the amorphous alloy powder is less than 40%, and the particle size is 5 to 30 microns, so as to meet the needs of modifying the composite performance of the magnesium-aluminum-zinc alloy, and to improve the hardness, toughness and wear resistance of the magnesium-aluminum-zinc alloy.
[0031] The method for preparing the amorphous alloy modified magnesium-aluminum-zinc alloy of the present invention comprises the following steps: Step 1: preparing amorphous alloy powder. In this step, the amorphous alloy raw material is melted and cooled to form under protective gas or vacuum conditions to obtain an amorphous alloy powder, and the addition amount of the amorphous alloy raw material satisfies the composition ratio shown in the following general formula: Zr a Al b Cu c Ni d M e N f , wherein M is one or more of Sc, Y, La, and Ce, N is one or more of Group VIII elements, 30≤a≤60, 10≤b≤30, 10≤c≤20, 10≤d≤20, 0≤e≤20, 0≤f≤10, and a+b+c+d+e+f=100, and a, b, c, d, e, and f are mole percentages.
[0032] In the present invention, the melting method is a melting method used in the open literature or by technicians in the field. As long as the amorphous alloy raw material is fully melted, for example, it is melted in a melting device. The melting temperature and melting time will vary with the different amorphous alloy raw materials. In the present invention, the melting temperature is preferably 900 to 2500 degrees Celsius, more preferably 1000 to 2000 degrees Celsius; the melting time is preferably 1 to 5 minutes, more preferably 1 to 3 minutes. The melting device is a conventional melting device, such as a vacuum arc melting furnace, a vacuum induction melting furnace or a vacuum resistance furnace, and the vacuum degree of the vacuum condition is 5×10 -5 Pa to 10 2 Pa, the protective gas is nitrogen or inert gas.
[0033] The cooling molding can adopt various conventional cooling molding methods in the art, for example, casting the molten alloy melt into a mold and then cooling it. The raw material of the amorphous alloy used in the present invention has a high amorphous forming ability and can be cooled at a low cooling rate, for example: 10 to 10 2 K / s, forming amorphous alloy powder with a particle size of 1 to 10 microns. The temperature of the mold temperature device is controlled below the glass transition temperature (Tg) of the amorphous alloy.
[0034] Step 2, prepare a magnesium-aluminum-zinc alloy, and modify the magnesium-aluminum-zinc alloy with the amorphous alloy powder obtained in step 1. The preparation method of the magnesium-aluminum-zinc alloy adopts the preparation method of magnesium alloy commonly used in the art, and adopts the melting process of material preparation → melting alloying → refining → casting to smelt the magnesium alloy to prepare the magnesium alloy. The difference is that in the process of melting alloying, amorphous alloy powder is added for melting and refining, and then cast to obtain the amorphous alloy modified magnesium alloy. The specific details are as follows:
[0035] Step 2.1, material preparation: 1) Raw materials: prepare the formula amount of pure magnesium ingots (purity ≥ 99.9 parts by weight), pure aluminum ingots (purity ≥ 99.9 parts by weight), pure zinc ingots (purity ≥ 99.9 parts by weight), and the corresponding rare earth element ingots; 2) Auxiliary agents: covering agents RJ-2, RJ-6, RJ-JL flux and refining agent RJ-5, preferably composite flux RG-FH flux; 3) Protective atmosphere: SF6 protective gas. Under the protection of SF6 gas and with the use of covering agent protection, the alloy is melted to avoid the active elements in the raw materials in the molten state from burning violently in an oxygen environment and oxidizing and burning. Melting equipment: Use a pit-type resistance crucible furnace.
[0036] Step 2.2, drying: drying the prepared raw materials, wherein magnesium, aluminum, and zinc are dried at 100 degrees Celsius ± 10 degrees Celsius, and rare earth element ingots are dried at 150 degrees Celsius ± 5 degrees Celsius, and the amorphous alloy powder is preheated at 120 ± 20 degrees Celsius; the purpose of drying is to remove moisture from the raw materials to prevent explosions caused by the reaction of water and magnesium during the melting process; the purpose of preheating is to avoid rapid temperature increase that causes crystallization of the amorphous alloy.
[0037] Step 2.3, melt alloying: preheat the crucible to 300-350 degrees Celsius, put in weighed magnesium ingots, aluminum ingots, zinc ingots, and rare earth element ingots under protective gas or vacuum conditions, continue heating to 720-750 degrees Celsius, and after all the above ingots are melted, cool down to 650-700 degrees Celsius, add amorphous alloy powder, and then heat to 750-780 degrees Celsius, stir evenly, and keep warm for 5-10 minutes to obtain a magnesium alloy melt.
[0038] Step 2.4, refining: evenly sprinkle a refining agent on the surface of the magnesium alloy melt, for example, refining agent RJ~5 or RG~FHflux for refining. During the refining process, the amount of refining agent added is 8% to 12% of the charge amount. After adding, fully stir and let stand for 5 to 15 minutes; then heat to 770 to 800 degrees Celsius and keep warm for 6 to 8 minutes to allow the added metal to be better alloyed at a higher temperature; then cool to 650 to 700 degrees Celsius and let stand for 4 to 6 minutes to make the alloy more uniform at a lower temperature to obtain a magnesium alloy melt.
[0039] Step 2.5, casting: casting the refined magnesium alloy melt into a mold preheated at a temperature of 280 to 320 degrees Celsius. After the casting is completed, the mold and the magnesium alloy melt therein are placed in the air for cooling and then demolded to obtain the amorphous alloy-modified magnesium alloy.
[0040] The preparation method of the present invention modifies the MgAlZn magnesium alloy by adding rare earth elements, and simultaneously adds amorphous alloys for grain refinement, which can reduce the surface defects of the magnesium alloy during processing, such as die casting, extrusion, etc., greatly improve the processing speed, and significantly improve the composite performance and production efficiency of the magnesium alloy products.
[0041] The present invention has the following characteristics: the present invention adopts Zr-based amorphous alloy powder to perform modification treatment in the preparation process of MgAlZn magnesium alloy, the amorphous alloy powder is a modified ZrAlCuNi amorphous alloy, the magnesium alloy is a MgAlZn magnesium alloy modified by adding rare earth elements, and the rare earth elements and ZrAlCuNi amorphous alloy powder act together in the melting process of the magnesium alloy to achieve the effect of refining grains and improving alloy structure; through mechanical property detection, the strength, plasticity, hardness and toughness of the magnesium-aluminum-zinc alloy modified by the amorphous alloy of the present invention are improved compared with the magnesium-aluminum-zinc alloy without adding the amorphous alloy, and it is conducive to later processing and forming.
[0042] The present invention is described in detail below in conjunction with specific examples 1 to 15 and comparative examples 1 to 3.
[0043] Example 1
[0044] The method for preparing the amorphous alloy-modified magnesium-aluminum-zinc alloy of Example 1 of the present invention comprises the following steps:
[0045] Step 1: Prepare amorphous alloy powder: Under vacuum conditions, mix the amorphous alloy raw materials, and the amount of the amorphous alloy raw materials added satisfies the composition ratio shown in the following general formula: Zr 40 Al 20 Cu 10 Ni 10 Ce 10 Fe 10 The proportioned raw materials were placed in a vacuum arc melting furnace and melted at 1800 degrees Celsius for 3 minutes, and then 2 K / s cooling rate at 20 degrees Celsius to obtain amorphous alloy powder Zr 40 Al 20 Cu 10 Ni 10 Ce 10 Fe 10 .
[0046] Step 2: Prepare a magnesium-aluminum-zinc alloy, and modify the magnesium-aluminum-zinc alloy using the amorphous alloy powder obtained in step 1. The process includes the following sub-steps:
[0047] (1) Drying: The prepared raw materials: magnesium ingot (purity ≥ 99.9 parts by weight), aluminum ingot (purity ≥ 99.9 parts by weight), zinc ingot (purity ≥ 99.9 parts by weight), and lanthanum ingot (purity ≥ 99.9 parts by weight) are dried at 100 degrees Celsius.
[0048] (2) Melting: During the entire melting process, SF6 gas is continuously introduced into the resistance crucible for protection. The resistance crucible is first preheated to 300 degrees Celsius, and an appropriate amount of refining agent and covering agent RG~FH flux is sprinkled on the inner wall of the crucible. Then, weighed magnesium ingots, aluminum ingots, zinc ingots, and lanthanum ingots are placed, and the temperature is continued to be heated to 750 degrees Celsius. At the same time, the covering agent RJ~6 is evenly sprinkled. After the magnesium ingots, aluminum ingots, zinc ingots, and scandium ingots are all melted, the temperature is lowered to 700 degrees Celsius, and amorphous alloy powder is added. Then the temperature is raised to 760 degrees Celsius, and the mixture is evenly stirred. At the same time, the temperature is kept for 5 to 10 minutes to obtain a magnesium-aluminum-zinc alloy melt. Based on 100 parts by weight, 85 parts by weight of magnesium-aluminum-zinc alloy raw materials and 15 parts by weight of amorphous alloy powder are added.
[0049] (3) Refining and casting: The refining agent RJ-5 is evenly sprinkled on the surface of the magnesium-aluminum-zinc alloy melt for refining. During the refining process, the amount of the refining agent added is about 10% of the amount of the charge. After adding, it is fully stirred and left to stand for 5 minutes. Then the temperature is raised to 780 degrees Celsius and kept for 8 minutes, then the temperature is lowered to 700 degrees Celsius and left to stand for 5 minutes, and then poured into a mold preheated at 280 degrees Celsius to obtain a magnesium-aluminum-zinc alloy ingot A1.
[0050] Embodiments 2 to 15
[0051] The raw materials and the preparation method are basically the same as those in Example 1, except that the composition of the magnesium-aluminum-zinc alloy or the components of the amorphous alloy powder are different. The composition of the magnesium-aluminum-zinc alloy and the composition of the amorphous alloy powder are shown in Table 1. The chemical composition is determined (the chemical composition is determined by ICP test, and the test results are shown in Table 1). The magnesium alloy ingots are subjected to chemical composition determination to obtain magnesium-aluminum-zinc alloy ingots A2 to A15.
[0052] Comparative Example 1
[0053] Comparative Example 1 is used to illustrate the performance of a magnesium-aluminum-zinc alloy without rare earth elements. The rest is the same as in Example 1, and a magnesium-aluminum-zinc alloy ingot B1 is obtained.
[0054] Comparative Example 2
[0055] Comparative Example 2 is used to illustrate the performance of a magnesium-aluminum-zinc alloy without adding amorphous alloy powder. The rest is the same as Example 1, and a magnesium-aluminum-zinc alloy ingot B2 is obtained.
[0056] Comparative Example 3
[0057] Comparative Example 2: An iron-based amorphous modified magnesium-aluminum-zinc alloy was prepared by the method disclosed in CN 113493876 B to obtain a magnesium-aluminum-zinc alloy ingot B3. This is used to illustrate the performance comparison between magnesium-aluminum-zinc alloys with iron-based amorphous alloy powders and zirconium-based amorphous alloy powders.
[0058] Performance Testing:
[0059] 1. Mechanical properties test: The magnesium-aluminum-zinc alloy ingots A1-A15 prepared in Examples 1-15 and the magnesium alloy ingots B1-B3 prepared in Comparative Examples 1-3 were respectively subjected to mechanical properties tests (tested by a universal mechanical testing machine, a micro Vickers hardness tester and an impact toughness testing machine). The mechanical properties test results of the magnesium-aluminum-zinc alloys obtained are shown in Table 2.
[0060] 2. Extrusion speed test: The magnesium-aluminum-zinc alloy ingots A1-A15 prepared in Examples 1-15 and the magnesium-aluminum-zinc alloy ingots B1-B3 prepared in Comparative Examples 1-3 were extruded in a 600-800 ton extruder. The extrusion speeds shown are shown in Table 2.
[0061] 3. Microstructure observation: The magnesium-aluminum-zinc alloy ingot A1 prepared in Example 1 and the magnesium-aluminum-zinc alloy ingot B1 prepared in Comparative Examples 1 and 2 were homogenized and annealed at 350 to 450 degrees Celsius for 10 to 14 hours and then sampled for microstructure observation. The microstructure photographs are as follows: Figure 1 to Figure 3 shown.
[0062]
[0063] Table 1
[0064]
[0065]
[0066] Table 2
[0067] According to the data of Table 1 and Table 2 above, Example 1 and Comparative Examples 1 to 3 are compared. Compared with Comparative Example 1, which does not add rare earth elements, Example 1 has better strength, hardness, toughness and elongation than Comparative Example 2, which does not add amorphous alloy powder, and also has better processing performance. Compared with Comparative Example 3, i.e., the solution of the background technology reference document, it has better strength, hardness, toughness and elongation.
[0068] Comparing the data between Examples 1 to 15, for example: Example 3 adopts the preferred zirconium-based amorphous alloy composition compared with Example 1, and has better strength, hardness, toughness, elongation and processing performance; Example 15 adopts the preferred magnesium-aluminum-zinc alloy composition compared with Example 1, and has better strength, hardness, toughness, elongation and processing performance. Example 13 adopts the most preferred components of zirconium-based amorphous alloy and magnesium-aluminum-zinc alloy, and its composite performance is the best; Example 10 adopts non-preferred components of zirconium-based amorphous alloy and magnesium-aluminum-zinc alloy, and its composite performance is slightly worse; comparing different examples, the performance of the magnesium-aluminum-zinc alloy of the example of selecting preferred components and elements is better than the performance of the magnesium-aluminum-zinc alloy of the example of non-preferred components and elements.
[0069] contrast Figure 1 and Figure 2 , Figure 3 It is obvious that the grain bonding effect of the amorphous alloy modified magnesium-aluminum-zinc alloy A1 is significantly better than that of the magnesium alloy B1 and magnesium alloy B2. The clearly discernible crystal phase indicates that the addition of amorphous alloy powder can more effectively refine the grains and purify the magnesium alloy, and obtain a magnesium alloy product with more uniform composition and organization.
[0070] In the description of the present invention, it should be understood that the terms "first", "second", etc. are used for descriptive purposes only and cannot be understood as indicating or implying relative importance. In the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0071] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. An amorphous alloy modified magnesium aluminum zinc alloy, characterized in that: The amorphous alloy modified magnesium-aluminum-zinc alloy comprises a first component and a second component, wherein the weight percentage of the first component is 82% to 90% and the weight percentage of the second component is 10% to 18% by weight; The first component is a magnesium-aluminum-zinc alloy. Based on 100 parts by weight of the magnesium-aluminum-zinc alloy, the contents of the components in the magnesium-aluminum-zinc alloy are as follows: aluminum: 7.25-8.48 parts by weight; zinc: 1.35-1.58 parts by weight; rare earth elements: 1.80-2.50 parts by weight; and the balance is magnesium. The second component is a zirconium-based amorphous alloy, and the composition of the zirconium-based amorphous alloy is shown in the general formula: Zr a Al b Cu c Ni d M e N f , wherein M is one or more of Sc, Y, La, and Ce, N is one or more of Group VIII elements, 30≤a≤60, 10≤b≤30, 10≤c≤20, 10≤d≤20, 0≤e≤20, 0≤f≤10, and a+b+c+d+e+f=100, and a, b, c, d, e, and f are mole percentages.
2. The amorphous alloy modified magnesium-aluminum-zinc alloy according to claim 1, characterized in that: The rare earth element is a lanthanide element, and the weight percentage is 2.15-2.50 parts by weight.
3. The amorphous alloy modified magnesium-aluminum-zinc alloy according to claim 1 or 2, characterized in that: The rare earth element is one or more of La, Pr and Nd.
4. The amorphous alloy modified magnesium-aluminum-zinc alloy according to claim 1, characterized in that: The composition of the zirconium-based amorphous alloy is shown in the following general formula: Zr a Al b Cu c Ni d M e N f , wherein M is one or more of Y, La, and Ce, N is one or more of Fe and Co, 40≤a≤50, 20≤b≤30, 10≤c≤15, 10≤d≤20, 5≤e≤15, 5≤f≤10, and a+b+c+d+e+f=100, and a, b, c, d, e, and f are mole percentages.
5. The amorphous alloy modified magnesium-aluminum-zinc alloy according to claim 1, characterized in that: Calculated in weight percentage, the weight percentage of the first component is 82-85%, and the weight percentage of the second component is 12-15%.
6. A method for preparing an amorphous alloy-modified magnesium-aluminum-zinc alloy, characterized in that: The following steps are involved: Step 1: melt an amorphous alloy raw material in a protective gas environment, cool it and form it to obtain an amorphous alloy powder. The amount of the amorphous alloy raw material added satisfies the composition ratio shown in the following general formula: Zr a Al b Cu c Ni d M e N f , wherein M is one or more of Sc, Y, La, and Ce, N is one or more of Group VIII elements, 30≤a≤60, 10≤b≤30, 10≤c≤20, 10≤d≤20, 0≤e≤20, 0≤f≤10, and a+b+c+d+e+f=100, and a, b, c, d, e, and f are mole percentages; Step 2, using amorphous alloy powder as the second component, and using the raw material of cast magnesium-aluminum-zinc alloy as the first component, calculated by weight percentage, the weight percentage of the second component is 10% to 18%, and the weight percentage of the first component is 82 to 90%; based on 100 parts by weight of magnesium-aluminum-zinc alloy, the content of each component in the magnesium-aluminum-zinc alloy is: aluminum: 7.25 to 8.48 parts by weight; zinc: 1.35 to 1.58 parts by weight; rare earth elements 1.80 to 2.50 parts by weight; the balance is magnesium; the magnesium-aluminum-zinc alloy raw material is melted, the amorphous alloy powder is added during the melting process, and then refined and cast to obtain the amorphous alloy-modified magnesium-aluminum-zinc alloy.
7. The method for preparing the amorphous alloy-modified magnesium-aluminum-zinc alloy according to claim 6, characterized in that: The composition of the amorphous alloy powder is shown in the following general formula: Zr a Al b Cu c Ni d M e N f , wherein M is one or more of Y, La, and Ce, N is one or more of Fe and Co, 40≤a≤50, 20≤b≤30, 10≤c≤15, 10≤d≤20, 5≤e≤15, 5≤f≤10, and a+b+c+d+e+f=100, and a, b, c, d, e, and f are mole percentages; The rare earth element is one or more of La, Pr and Nd.
8. The method for preparing the amorphous alloy-modified magnesium-aluminum-zinc alloy according to claim 6, characterized in that: The rare earth element is a lanthanide element, and the weight percentage is 2.15-2.50 parts by weight.
9. The method for preparing the amorphous alloy-modified magnesium-aluminum-zinc alloy according to claim 6, characterized in that: The rare earth element is one or more of La, Pr and Nd.
10. The method for preparing the amorphous alloy modified magnesium-aluminum-zinc alloy according to claim 6, characterized in that: Calculated in weight percentage, the weight percentage of the first component is 82-85%, and the weight percentage of the second component is 12-15%.
Citation Information
Patent Citations
A method for modifying the surface of iron-based amorphous magnesium alloys
CN113493876B
Wrought magnesium alloy and preparation method thereof
CN102330006A
Magnesium alloy and preparation method thereof
CN102534327A