A color-changing film and preparation method thereof
By adopting a three-layer structural design in the photochromic discoloration film, including infrared reflective layer, color discoloration layer and ultraviolet protection layer, it prevents the migration of color discoloration additives and protects them, and solves the problem that color discoloration additives are prone to migrating and precipitation in the photochromic discoloration film. Improves discoloration stability and durability, and enhances infrared reflection performance.
Patent Information
- Application Number
- CN202211397026.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-11-09
AI Technical Summary
The color discoloration additives in the photosensitive discoloration film are prone to migration and precipitation, resulting in unstable discoloration effect and affecting the durability of use.
The color discoloration film design adopts a three-layer structure, including infrared reflective layer, color discoloration layer and UV protection layer. By introducing sheet-layer structure fillers into the color discoloration layer and setting a color discoloration layer at the intermediate layer, the migration of color discoloration additives is prevented and the color discoloration additives are passed through infrared. Reflective layer and UV-proof protective color discoloration additive to prevent external factors from aging.
It effectively improves the discoloration stability and durability of the discoloration film, enhances the infrared reflection performance, and enhances its resistance to factors such as water vapor and oxygen without affecting the discoloration function.
Smart Images

Figure BDA0003933599470000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of color-changing materials, and in particular to a color-changing film and a preparation method thereof. Background Art
[0002] Color-changing film is a type of polymer film that changes color in response to changes in the external environment. Depending on the type of external environmental change conditions it responds to, it can be divided into photochromic film, temperature-sensitive color-changing film, and electrochromic film.
[0003] Among them, photochromic film is a relatively common color-changing film, which is composed of a main film layer composed of a polymer resin and a color-changing agent distributed therein. The color-changing principle of the photochromic film is that the molecular structure of the color-changing agent will change under the action of light of a certain wavelength and intensity, resulting in a corresponding change in its light absorption peak, that is, the color, and this change is generally reversible. The color-changing agent is generally a small molecule compound, which generally has poor compatibility with the matrix polymer resin and is prone to migration and precipitation. In addition, the color-changing agent is easily affected by external environmental factors such as water vapor, oxygen, and heat energy, resulting in aging of the structure after migration and precipitation, affecting the color-changing effect, which is not conducive to improving the color-changing stability and durability of the photochromic film. Summary of the invention
[0004] In view of this, the present invention provides a color-changing film and a preparation method thereof. The color-changing auxiliary agent in the color-changing film provided by the present invention is not easy to migrate and precipitate, and has good color-changing stability.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] A color-changing film, comprising an infrared reflection layer, a color-changing layer and an ultraviolet protection layer which are stacked in sequence;
[0007] The infrared reflective layer comprises infrared reflective particles and a matrix resin;
[0008] The color-changing layer includes a color-changing auxiliary agent, a lamellar structure filler and a base resin;
[0009] The anti-ultraviolet layer comprises an inorganic filler and a base resin;
[0010] The infrared reflective particles include one or more of titanium dioxide, aluminum oxide, magnesium oxide, silicon dioxide, nickel oxide, cobalt oxide and copper oxide;
[0011] The inorganic filler includes talc and titanium dioxide.
[0012] Preferably, the lamellar structure filler includes one or more of talc, mica, MoS2, WSe2, WTe2, MoO3 and Fe3GeTe2.
[0013] Preferably, the diameter-to-thickness ratio of the lamellar structure filler is 30 to 80, D 50 The thickness of the filler is 5 to 25 μm, and the mass of the lamellar structure filler is 0.1 to 10% of the total mass of the color-changing layer.
[0014] Preferably, the color-changing agent includes one or more of 1,3-diphenyl-4-thenoyl-5-pyrazolone 4-phenylaminourea, 4-acylpyrazolone, tungsten trioxide, molybdenum trioxide, cupric chloride, vanadium dioxide and silver chloride, and the mass of the color-changing agent is 0.3 to 20% of the total mass of the color-changing layer.
[0015] Preferably, the mass of the infrared reflective particles is 0.5-20% of the total mass of the infrared reflective layer.
[0016] Preferably, the infrared reflective particles include D 90 The particles are 450-550nm, 580-650nm, 750-850nm and 900-1100nm respectively, and the D 90 The mass ratios of particles of 450-550 nm, 580-650 nm, 750-850 nm and 900-1100 nm are 4.5-5.5:2-4:0.5-1.5:0.5-1.5, respectively.
[0017] Preferably, the D of the talc is 50 is 5 to 25 μm, and the D 90 The thickness of the inorganic filler is 200-500 nm, and the mass of the inorganic filler is 0.5-20% of the total mass of the anti-ultraviolet layer.
[0018] Preferably, the matrix resins in the infrared reflecting layer, the color-changing layer and the UV protection layer are independently one or a combination of at least two of polyphenylene ether, polyvinylidene fluoride, polyethylene resin, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, polyisobutylene, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-octene copolymer and ethylene-vinyl acetate copolymer.
[0019] Preferably, the infrared reflection layer has a thickness of 5 to 50 μm, the color change layer has a thickness of 10 to 50 μm, and the anti-ultraviolet layer has a thickness of 5 to 50 μm.
[0020] The present invention also provides a method for preparing the color-changing film described in the above scheme, comprising the following steps: co-extruding, casting, cooling and shaping the raw materials used for the infrared reflection layer, the color-changing layer and the ultraviolet protection layer to obtain the color-changing film.
[0021] The present invention provides a color-changing film, comprising an infrared reflection layer, a color-changing layer and an anti-ultraviolet layer stacked in sequence; the infrared reflection layer comprises infrared reflection particles and a matrix resin; the color-changing layer comprises a color-changing agent, a lamellar structure filler and a matrix resin; the anti-ultraviolet layer comprises an inorganic filler and a matrix resin; the infrared reflection particles comprise one or more of titanium dioxide, aluminum oxide, magnesium oxide, silicon dioxide, nickel oxide, cobalt oxide and copper oxide; the inorganic filler comprises talcum powder and titanium dioxide. The present invention sets the color-changing layer at the position of the middle layer, relies on the upper and lower multilayer structures to prevent the migration of the color-changing agent, and introduces the lamellar structure filler into the color-changing layer to further prevent the migration of the color-changing agent, and also prevents the aging effect of external water vapor, oxygen and other factors on the color-changing agent, and will not affect the color-changing function of the color-changing agent. In summary, the color-changing agent in the color-changing film provided by the present invention is not easy to migrate and precipitate, and the color-changing stability is good, which is conducive to improving the durability of the color-changing film.
[0022] Furthermore, the present invention further improves the reflective performance of the infrared reflective layer by adding infrared reflective particles with different particle sizes into the infrared reflective layer.
[0023] The present invention also provides a method for preparing the color-changing film of the above scheme. The preparation method provided by the present invention has simple steps, is easy to operate, and is easy to carry out industrial production. DETAILED DESCRIPTION
[0024] The present invention provides a color-changing film, comprising an infrared reflection layer, a color-changing layer and an anti-ultraviolet layer which are stacked in sequence; the infrared reflection layer comprises infrared reflection particles and a matrix resin; the color-changing layer comprises a color-changing auxiliary agent, a lamellar structure filler and a matrix resin; the anti-ultraviolet layer comprises an inorganic filler and a matrix resin; the infrared reflection particles comprise one or more of titanium dioxide, aluminum oxide, magnesium oxide, silicon dioxide, nickel oxide, cobalt oxide and copper monoxide; the inorganic filler comprises talcum powder and titanium dioxide.
[0025] Unless otherwise specified, the raw materials used in the present invention are all commercially available.
[0026] In the present invention, the infrared reflective layer includes infrared reflective particles and a matrix resin. In the present invention, the infrared reflective particles include one or more of titanium dioxide, aluminum oxide, magnesium oxide, silicon dioxide, nickel oxide, cobalt oxide and copper oxide, preferably a mixture of titanium dioxide, magnesium oxide, cobalt oxide, titanium dioxide, aluminum oxide, magnesium oxide and silicon dioxide, a mixture of titanium dioxide, aluminum oxide, cobalt oxide and nickel oxide, or a mixture of titanium dioxide, magnesium oxide, cobalt oxide and nickel oxide, more preferably a mixture of titanium dioxide, aluminum oxide, magnesium oxide and silicon dioxide, a mixture of titanium dioxide, aluminum oxide, cobalt oxide and nickel oxide, or a mixture of titanium dioxide, magnesium oxide, cobalt oxide and nickel oxide. In the present invention, the titanium dioxide is preferably rutile titanium dioxide. In the present invention, the mass of the infrared reflective particles is preferably 0.5 to 20% of the total mass of the infrared reflective layer, more preferably 3 to 15%, and further preferably 10 to 12%.
[0027] In the present invention, the infrared reflective particles preferably include D 90 The particles of 450-550nm, 580-650nm, 750-850nm and 900-1100nm are more preferably D 90 The particles are 480-520 nm, 600-620 nm, 780-820 nm and 950-1050 nm respectively, and further preferably include D 90 In the present invention, the D 90 The mass ratio of particles with a diameter of 450 to 550 nm, 580 to 650 nm, 750 to 85 nm and 900 to 1100 nm is preferably 4.5 to 5.5: 2 to 4: 0.5 to 1.5: 0.5 to 1.5, more preferably 4.7 to 5.2: 2.5 to 3.5: 0.7 to 1.2: 0.7 to 1.2, and further preferably 5: 3: 1: 1. In a specific embodiment of the present invention, the infrared reflective particles are D 90 500nm titanium dioxide, D 90 600nm aluminum oxide, D 90 800nm MgO and D 90 A mixture of 1000 nm silicon dioxide, wherein the mass ratio of titanium dioxide, aluminum oxide, magnesium oxide and silicon dioxide is preferably 5:3:1:1; or: D 90 500nm titanium dioxide, D 90 600nm aluminum oxide, D 90 800nm cobalt oxide and D 90 A mixture of 1000 nm nickel oxide, wherein the mass ratio of titanium dioxide, aluminum oxide, cobalt oxide and nickel oxide is preferably 5:3:1:1; or: D90 500nm titanium dioxide, D 90 600nm magnesium oxide, D 90 800nm cobalt oxide and D 90 The mixture is a 1000nm nickel oxide mixture, and the mass ratio of titanium dioxide, magnesium oxide, cobalt oxide and nickel oxide is preferably 5:3:1:1.
[0028] In the present invention, the color-changing layer includes a color-changing auxiliary agent, a lamellar structure filler and a matrix resin. In the present invention, the color-changing aid preferably includes one or more of 5-[N-(tert-butoxycarbonyl)amino]-1,3,3-triethyl-6'-nitroindole spiropyran, 3,3-dimethyl-N-ethyl-6'-nitrobenzospiropyran, 1,3-diphenyl-4-thenoyl-5-pyrazolone 4-phenylsemicarbazide, 4-acylpyrazolone, tungsten trioxide, molybdenum trioxide, copper chloride, vanadium dioxide and silver chloride, more preferably one or more of 5-[N-(tert-butoxycarbonyl)amino]-1,3,3-triethyl-6'-nitroindole spiropyran, 4-acylpyrazolone, vanadium dioxide and tungsten trioxide, and further preferably one or more of 5-[N-(tert-butoxycarbonyl)amino]-1,3,3-triethyl-6'-nitroindole spiropyran, 4-acylpyrazolone and vanadium dioxide. In the present invention, the mass of the color-changing auxiliary agent is preferably 0.3 to 20% of the total mass of the color-changing layer, more preferably 3 to 15%, and even more preferably 7 to 13%.
[0029] In the present invention, the lamellar structure filler preferably includes one or more of talc, mica, MoS2, WSe2, WTe2, MoO3 and Fe3GeTe2, more preferably one or more of talc, WSe2 and WTe2, further preferably talc, a mixture of talc and WTe2 or a mixture of talc and WSe2, more preferably a mixture of talc and WSe2. In the present invention, the diameter-to-thickness ratio of the lamellar structure filler is preferably 30 to 80, more preferably 30 to 50, and the D 50 Preferably, it is 5 to 25 μm, more preferably 10 to 15 μm, and further preferably 10 μm. In a specific embodiment of the present invention, the lamellar structure filler is preferably talcum powder, a mixture of talcum powder and WTe2, or a mixture of talcum powder and WSe2; when the lamellar structure filler is preferably talcum powder, the diameter-to-thickness ratio of the talcum powder is preferably 30, D 50 When the lamellar structure filler is preferably a mixture of talc and WTe2, the mass ratio of the talc and the WTe2 is preferably 3:2, the diameter-to-thickness ratio of the talc is preferably 50, D 50 Preferably, the thickness ratio of WTe2 is 30, D50 When the lamellar structure filler is preferably a mixture of talc and WSe2, the mass ratio of the talc and the WSe2 is preferably 1:1, the diameter-to-thickness ratio of the talc is preferably 80, D 50 Preferably, the thickness ratio of WSe2 is 50, D 50 Preferably, it is 25 μm. In the present invention, the mass of the lamellar structure filler is preferably 0.1 to 10% of the total mass of the color-changing layer, more preferably 3 to 8%, and even more preferably 5 to 6%.
[0030] In the present invention, the anti-ultraviolet layer comprises an inorganic filler and a matrix resin. In the present invention, the inorganic filler comprises talcum powder and titanium dioxide, and the titanium dioxide is preferably rutile titanium dioxide. In the present invention, the mass ratio of the talcum powder and titanium dioxide is any ratio. In the present invention, the D 50 Preferably, it is 5 to 25 μm, more preferably 8 to 15 μm, and even more preferably 10 to 12 μm. 90 It is preferably 200-500 nm, more preferably 250-350 nm, and even more preferably 300 nm. In the present invention, the mass of the inorganic filler is preferably 0.5-20% of the total mass of the UV protection layer, more preferably 7-15%, and even more preferably 10-12%.
[0031] In the present invention, the matrix resin in the infrared reflection layer, the color-changing layer and the anti-ultraviolet layer is independently preferably polyphenylene ether, polyvinylidene fluoride, polyethylene resin, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, polyisobutylene, ethylene-propylene copolymer, ethylene-butylene copolymer, ethylene-octene copolymer and ethylene-vinyl acetate copolymer, or a combination of at least two thereof, and more preferably polyphenylene ether, ethylene-butylene copolymer, polyethylene resin, ethylene-vinyl acetate copolymer and ethylene-octene copolymer, or a combination of at least two thereof. In a specific embodiment of the present invention, the matrix resin of the infrared reflection layer is preferably polyethylene, a mixture of ethylene-octene copolymer and polyethylene, a mixture of ethylene-octene copolymer, ethylene-propylene copolymer and polyphenylene ether, and the mass ratio of ethylene-octene copolymer and polyethylene in the mixture of ethylene-octene copolymer and polyethylene resin is preferably 50:40; the mass ratio of ethylene-octene copolymer, ethylene-propylene copolymer and polyphenylene ether in the mixture of ethylene-octene copolymer, ethylene-propylene copolymer and polyphenylene ether is preferably 5:30:5. The base resin of the color-changing layer is preferably a mixture of ethylene-butene copolymer and polyethylene or a mixture of ethylene-butene copolymer and ethylene-propylene copolymer. The mass ratio of ethylene-butene copolymer to polyethylene in the mixture of ethylene-butene copolymer and polyethylene is preferably 0.6:99 or 8:80, and the mass ratio of ethylene-butene copolymer to ethylene-propylene copolymer is preferably 10:60. The base resin of the anti-ultraviolet layer is preferably a mixture of ethylene-vinyl acetate copolymer and polyethylene, and the mass ratio of ethylene-vinyl acetate copolymer to polyethylene in the mixture of ethylene-vinyl acetate copolymer and polyethylene is preferably 0.5:99, 85:5 or 80:5.
[0032] In the present invention, the thickness of the infrared reflection layer is preferably 5 to 50 μm, more preferably 10 to 35 μm, and further preferably 20 to 25 μm; the thickness of the color-changing layer is preferably 10 to 50 μm, more preferably 15 to 40 μm, and further preferably 25 to 35 μm; the thickness of the anti-ultraviolet layer is preferably 5 to 50 μm, more preferably 20 to 45 μm, and further preferably 30 to 40 μm.
[0033] The present invention also provides a method for preparing the color-changing film described in the above scheme, comprising the following steps: co-extruding, casting, cooling and shaping the raw materials used for the infrared reflection layer, the color-changing layer and the ultraviolet protection layer to obtain the color-changing film.
[0034] In the present invention, the three-layer coextrusion and casting are preferably carried out in a three-layer coextrusion casting machine, and the melting temperature of the three-layer coextrusion is preferably 160-280°C, more preferably 180-240°C, and further preferably 200-220°C.
[0035] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.
[0036] Example 1
[0037] The raw materials of infrared reflection layer are: 5 parts D 90 500nm titanium dioxide, 3 parts D 90 600nm aluminum oxide, 1 part D 90 800nm magnesium oxide, 1 part D 90 1000nm silicon dioxide, 190 parts polyethylene;
[0038] The raw materials of the color-changing layer are: 0.3 parts of 5-[N-(tert-butyloxycarbonyl)amino]-1,3,3-triethyl-6'-nitroindolinol spiropyran, 0.1 parts of diameter-to-thickness ratio 30, particle size D 50 5 μm talc, 0.6 parts of ethylene-butene copolymer, 99 parts of polyethylene;
[0039] The raw materials of the UV protection layer are: 0.2 parts of D 50 5μm talc, 0.3 parts D 90 It is 200nm titanium dioxide, 0.5 parts of ethylene-vinyl acetate copolymer, and 99 parts of polyethylene;
[0040] In a three-layer co-extrusion casting machine, the raw materials of the infrared reflection layer, the color-changing layer and the anti-ultraviolet layer are respectively put into the A\B\C extruder hopper, and melt-extruded at a temperature of 160°C. After being discharged from the film head of the casting machine, the materials are cooled, shaped, pulled, and finally rolled up to obtain a color-changing film. The thicknesses of the infrared reflection layer, the color-changing layer, and the anti-ultraviolet layer in the color-changing film are 5μm, 10μm, and 5μm, respectively.
[0041] Example 2
[0042] The raw materials of infrared reflection layer are: 5 parts D 90 500nm titanium dioxide, 3 parts D 90 600nm aluminum oxide, 1 part D 90 800nm cobalt oxide, 1 part D 90 1000nm nickel oxide, 50 parts of ethylene-octene copolymer, 40 parts of polyethylene;
[0043] The raw materials of the color-changing layer are: 5 parts of 4-acylpyrazolone, 2 parts of vanadium dioxide, 3 parts of 50 10μm talcum powder, 2 parts diameter-to-thickness ratio 30, particle size D 50 5 μm WTe2, 8 parts of ethylene-butene copolymer, 80 parts of polyethylene resin;
[0044] The raw materials of the UV protection layer are: 5 parts of D50 10 μm talc powder, 5 parts D 90 300nm titanium dioxide, 85 parts of ethylene-vinyl acetate copolymer, 5 parts of polyethylene;
[0045] In a three-layer co-extrusion casting machine, the raw materials of the infrared reflection layer, the color-changing layer and the anti-ultraviolet layer are respectively put into the A\B\C extruder hopper, and melt-extruded at a temperature of 200°C. After being discharged from the film head of the casting machine, the materials are cooled, shaped, pulled, and finally rolled up to obtain a color-changing film. The thicknesses of the infrared reflection layer, the color-changing layer, and the anti-ultraviolet layer in the color-changing film are 25μm, 25μm, and 35μm, respectively.
[0046] Example 3
[0047] The raw materials of infrared reflection layer are: 5 parts D 90 500nm titanium dioxide, 3 parts D 90 600nm magnesium oxide, 1 part D 90 800nm cobalt oxide, 1 part D 90 1000nm nickel oxide, 5 parts of ethylene-octene copolymer, 30 parts of ethylene-propylene copolymer, 5 parts of polyphenylene ether;
[0048] The raw materials of the color-changing layer are: 10 parts of 5-[N-(tert-butyloxyformyl)amino]-1,3,3-triethyl-6'-nitroindolinyl spiropyran, 9 parts of tungsten trioxide, 1 part of vanadium dioxide, 5 parts of diameter-to-thickness ratio of 80, particle size D 50 25μm talcum powder, 5 parts diameter-to-thickness ratio of 50, particle size D 50 25 μm WSe2, 10 parts of ethylene-butene copolymer, 60 parts of ethylene-propylene copolymer;
[0049] The raw materials of the UV protection layer are: 15 parts of D 50 25 μm talc powder, 5 parts D 90 500nm titanium dioxide, 80 parts of ethylene-vinyl acetate copolymer, 5 parts of polyethylene resin;
[0050] In a three-layer co-extrusion casting machine, the raw materials of the infrared reflection layer, the color-changing layer and the anti-ultraviolet layer are respectively put into the A\B\C extruder hopper, and melt-extruded at a temperature of 280°C. After being discharged from the film head of the casting machine, the materials are cooled, shaped, and pulled, and finally rolled up to obtain a color-changing film. The thickness of the infrared reflection layer, the color-changing layer, and the anti-ultraviolet layer in the color-changing film are 50μm, 50μm, and 50μm, respectively.
[0051] Comparative Example 1
[0052] Raw materials of color-changing film: 10 parts of 5-[N-(tert-butyloxycarbonyl)amino]-1,3,3-triethyl-6'-nitroindolinyl spiropyran, 9 parts of tungsten trioxide, 1 part of vanadium dioxide, 20 parts of ethylene-butene copolymer, 60 parts of ethylene-butene copolymer;
[0053] In the casting machine, the raw materials are put into the extruder hopper and melt-extruded at a temperature of 280°C. After being discharged from the film head of the casting machine, the materials are cooled, shaped, pulled, and finally rolled up to obtain a color-changing film with a thickness of 150 μm.
[0054] Comparative Example 2
[0055] Raw materials of color-changing film: 5 parts of 4-acylpyrazolone, 2 parts of vanadium dioxide, 13 parts of ethylene-butene copolymer, 80 parts of polyethylene resin;
[0056] In the casting machine, the raw materials are put into the extruder hopper and melt-extruded at a temperature of 280°C. After being discharged from the film head of the casting machine, the materials are cooled, shaped, pulled, and finally rolled up to obtain a 150um color-changing film.
[0057] Comparative Example 3
[0058] The raw materials of infrared reflection layer are: 5 parts D 90 500nm titanium dioxide, 3 parts D 90 600nm aluminum oxide, 1 part D 90 800nm cobalt oxide, 1 part D 90 1000nm nickel oxide, 50 parts of ethylene-octene copolymer, 40 parts of polyethylene;
[0059] The raw materials of the color-changing layer are: 5 parts of 4-acylpyrazolone, 2 parts of vanadium dioxide, 13 parts of ethylene-butene copolymer, and 80 parts of polyethylene resin;
[0060] The raw materials of the UV protection layer are: 5 parts of D 50 10 μm talc powder, 5 parts D 90 300 μm titanium dioxide, 85 parts of ethylene-vinyl acetate copolymer, 5 parts of polyethylene;
[0061] In a three-layer co-extrusion casting machine, the raw materials of the infrared reflection layer, the color-changing layer and the anti-ultraviolet layer are respectively put into the A\B\C extruder hopper, and melt-extruded at a temperature of 200°C. After being discharged from the film head of the casting machine, the materials are cooled, shaped, pulled, and finally rolled up to obtain a color-changing film. The thicknesses of the infrared reflection layer, the color-changing layer, and the anti-ultraviolet layer in the color-changing film are 25μm, 25μm, and 35μm, respectively.
[0062] The color-changing films obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were tested for tensile properties, infrared reflectivity, photobleaching properties, and 24h boiling water migration. Among them, the tensile property test refers to GB / T13022-1991 Plastic Film Tensile Property Test Method, the infrared reflectivity refers to ASTM F1252-2010 Standard Test Method for Measuring Light Reflectivity of Transparent Materials, and the photobleaching experimental conditions are: in an ultraviolet aging box, 10mw / square centimeter, the main wavelength is 360nm ultraviolet lamp continuous irradiation, regular removal to observe the color change effect of the color-changing film, when the color change characteristics disappear, record the illumination time. 24h boiling water migration experimental conditions: the color-changing film is placed in boiling water for 24h, and then the migration of the color-changing auxiliary agent in the color-changing film to the surface is observed. The performance test results of the color-changing films obtained in Examples 1 to 3 and Comparative Examples 1 to 2 are shown in Table 1.
[0063] Table 1 Performance test results of the color-changing films obtained in Examples 1 to 3 and Comparative Examples 1 to 2
[0064]
[0065] As can be seen from Table 1, the mechanical properties of the color-changing films obtained in Examples 1 to 3 are similar to those of the color-changing films obtained in Comparative Examples 1 to 3. Due to the addition of the infrared reflection layer, the infrared reflectivity of the color-changing films obtained in Examples 1 to 3 is higher than that of the color-changing films obtained in Comparative Examples 1 to 3. At the same time, since a filler with a lamellar structure is added to the color-changing layer and other protective layers are provided on both sides of the color-changing layer, the migration of the color-changing agent can be prevented, and the aging effect of external factors such as water vapor and oxygen on the color-changing agent can be prevented, so that the light bleaching resistance of the color-changing film obtained in Examples 1 to 3 and the migration resistance of the color-changing agent are improved, and the color-changing performance stability of the color-changing film is improved, which is beneficial to improving the durability of the color-changing film.
[0066] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A color-changing film, It is characterized in that It includes an infrared reflection layer, a color-changing layer and an anti-ultraviolet layer which are stacked in sequence; The infrared reflective layer comprises infrared reflective particles and a matrix resin; The color-changing layer includes a color-changing auxiliary agent, a lamellar structure filler and a base resin; The anti-ultraviolet layer comprises an inorganic filler and a base resin; The infrared reflective particles include one or more of titanium dioxide, aluminum oxide, magnesium oxide, silicon dioxide, nickel oxide, cobalt oxide and copper oxide; the mass of the infrared reflective particles is 0.5 to 20% of the total mass of the infrared reflective layer; The color-changing agent includes one or more of 1,3-diphenyl-4-thenoyl-5-pyrazolone 4-phenyl semicarbazide, 4-acylpyrazolone, tungsten trioxide, molybdenum trioxide, copper chloride, vanadium dioxide and silver chloride, and the mass of the color-changing agent is 0.3-20% of the total mass of the color-changing layer; The inorganic filler comprises talcum powder and titanium dioxide; the mass of the inorganic filler is 0.5 to 20% of the total mass of the anti-ultraviolet layer; The lamellar structure filler includes talc, mica, MoS 2 ,WSe 2 、WTe 2 、MoO 3 and Fe 3 Get 2 One or more of the following; the mass of the lamellar structure filler is 0.1 to 10% of the total mass of the color-changing layer; The matrix resins in the infrared reflection layer, the color-changing layer and the UV protection layer are independently one or a combination of at least two of polyphenylene ether, polyvinylidene fluoride, polyethylene resin, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, polyisobutylene, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-octene copolymer and ethylene-vinyl acetate copolymer.
2. The color-changing film according to claim 1, It is characterized in that The diameter-to-thickness ratio of the lamellar structure filler is 30-80, D 50 5~25μm.
3. The color-changing film according to claim 1, It is characterized in that The infrared reflective particles include D 90 The particles are 450-550nm, 580-650nm, 750-850nm and 900-1100nm respectively, and the D 90 The mass ratios of particles of 450-550 nm, 580-650 nm, 750-850 nm and 900-1100 nm are 4.5-5.5:2-4:0.5-1.5:0.5-1.5, respectively.
4. The color-changing film according to claim 1, It is characterized in that The D of the talc 50 is 5 to 25 μm, and the D 90 It is 200~500nm.
5. The color-changing film according to claim 1, It is characterized in that The infrared reflection layer has a thickness of 5 to 50 μm, the color change layer has a thickness of 10 to 50 μm, and the anti-ultraviolet layer has a thickness of 5 to 50 μm.
6. A method for preparing the color-changing film according to any one of claims 1 to 5, It is characterized in that The following steps are involved: The raw materials used for the infrared reflection layer, the color-changing layer and the anti-ultraviolet layer are subjected to three-layer co-extrusion, casting, cooling and shaping to obtain the color-changing film.