Environmentally friendly composite coated paper and preparation method thereof

Through the combination of modified PLA coating layer and reinforced composite paper core, the problems of environmental pollution and poor high temperature resistance of existing coated paper are solved, efficient biodegradation and improvement of mechanical properties are achieved, and the production needs of environmentally friendly composite materials are met. , with significant economic and environmental benefits.

CN116100909BActive Publication Date: 2024-10-01SHANGHAI XINXIAO ENVIRONMENTAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210989246.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-17
Publication Date
2024-10-01
Estimated Expiration
2042-08-17

AI Technical Summary

Technical Problem

Existing PE and PP coated papers cause environmental pollution due to their non-degradability, are difficult to meet environmental protection requirements, and have poor high temperature resistance, making them unable to effectively solve the production needs of environmentally friendly composite materials.

Method used

Using modified PLA coating layer and reinforced composite paper core, through cross-linking modification of cyclodextrin, PLA, acid anhydride additives, phosphates and fillers, a composite system similar to CBM resin is formed, and added to the coating paper Corrugated paper layers and reinforcing ribs improve toughness and mechanical properties, while using degradable adhesives to simplify production.

Benefits of technology

It achieves efficient biodegradation of the modified PLA coating layer, enhances the mechanical properties and degradation performance of the composite paper core, and the degradation rate reaches more than 90%, which complies with green environmental protection standards, simplifies the production process, and has significant economic and environmental benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116100909B_ABST
    Figure CN116100909B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of environmentally friendly materials, and more specifically, it relates to an environmentally friendly composite coated paper and a preparation method thereof. The environmentally friendly composite coated paper comprises a reinforced composite paper core and a modified PLA coated layer arranged on both sides of the reinforced composite paper core; the raw material masterbatch of the modified PLA coated layer is prepared from the following raw materials in parts by weight: 40-60 parts of cyclodextrin, 100-150 parts of PLA, 0.3-0.5 parts of anhydride additives, 0.1-0.2 parts of coupling agents, 0.5-0.8 parts of phosphates, and 10-30 parts of fillers. The present application retains the excellent performance of the composite coated material through the composite modification of multiple components, while having the advantages of green environmental protection, which can effectively reduce the pollution and load brought to the environment, and thus has extremely high economic and environmental benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of environmentally friendly materials, and more specifically, to an environmentally friendly composite coated paper and a preparation method thereof. Background Art

[0002] Laminated paper refers to a composite material formed by coating and bonding plastic particles to the surface of paper through a casting method. Due to the characteristics of plastic particles, it generally has excellent waterproof and oil-proof properties and is widely used in the production of disposable paper cups, paper bowls, paper lunch boxes and other paper containers.

[0003] The typical representative of the coated paper in the related technology is PE coated paper, which has excellent waterproof and oil-proof properties and is easy to process and produce, but has poor high temperature resistance. Therefore, some companies also use PP coated paper or composite coated paper with a compound resin of the two.

[0004] However, success or failure is due to the non-natural degradation of plastic particles such as PE and PP, making such composite materials unable to meet the environmental protection requirements that people are meeting at this stage. After being discarded, they also bring great pollution and burden to the environment. Therefore, there is an urgent need to provide an environmentally friendly composite coated paper and a preparation method thereof. Summary of the invention

[0005] In order to retain the excellent performance of composite coated paper while having the advantages of being green and environmentally friendly, thereby reducing pollution and load on the environment, the present application specifically provides an environmentally friendly composite coated paper and a preparation method thereof.

[0006] In the first aspect, the present application provides an environmentally friendly composite coated paper, which adopts the following technical solution:

[0007] An environmentally friendly composite coated paper comprises a reinforced composite paper core and modified PLA coated layers arranged on both sides of the reinforced composite paper core; the raw material masterbatch of the modified PLA coated layer is prepared from the following raw materials in parts by weight: 40-60 parts of cyclodextrin, 100-150 parts of PLA, 0.3-0.5 parts of anhydride additives, 0.1-0.2 parts of coupling agents, 0.5-0.8 parts of phosphates, and 10-30 parts of fillers.

[0008] By adopting the above technical solution, the prepared modified PLA coating layer meets the definition of green environmental protection. Under the cross-linking modification of cyclodextrin, acid anhydride additives, phosphate and coupling agent, PLA forms a composite system similar to CBM resin, overcoming the original defects of brittleness and poor toughness.

[0009] When the above-mentioned environmentally friendly composite coated paper is discarded or landfilled, its modified PLA coating layer structure will be degraded first, and then cause the destruction of the surface to the internal structure of the reinforced composite paper core. The degradation rate can reach more than 90% in 3 months, and it mainly adopts biodegradation, so it has significant economic and environmental benefits.

[0010] Preferably, the preparation process of the raw material masterbatch of the modified PLA coating layer is as follows:

[0011] a. Premix cyclodextrin, anhydride additives and phosphate, then add deionized water, wait for the phosphate to be hydrolyzed to a pH of 7.6-8.8, heat to 80-120°C and stir to obtain prefabricated cyclodextrin;

[0012] b. Then the prefabricated cyclodextrin, PLA, coupling agent and filler are dried and blended under vacuum conditions, and finally melt-extruded at 180-220° C. to obtain the raw material masterbatch of the modified PLA coating layer.

[0013] By adopting the above technical scheme, the raw material masterbatch of the modified PLA coating layer prepared by the above process has significant environmental benefits, and its own toughness and brittleness are significantly improved under the cross-linking and bonding effect of the prefabricated cyclodextrin; the reasons may be analyzed as follows: the cyclodextrin, acid anhydride additives and phosphates in the above ratio are heated in the alkaline environment generated after the hydrolysis of phosphate, which can effectively induce the grafting reaction of cyclodextrin and acid anhydride, thereby giving the modified PLA excellent biocompatibility, degradability and envelope structure in the process of blending the prefabricated cyclodextrin with PLA, coupling agent and filler.

[0014] Preferably, the anhydride auxiliary agent is composed of 2-octenyl succinic anhydride, maleic anhydride and dodecenyl succinic anhydride in a weight ratio of 1:(1-1.2):(0.3-0.5).

[0015] Preferably, the phosphate is selected from one or more of sodium hydrogen phosphate, sodium dihydrogen phosphate, sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate.

[0016] Preferably, the filler is 1-3 mm short-cut degradable plant fiber, selected from one or more of straw fiber, rice husk fiber, corn fiber and soybean fiber.

[0017] Preferably, the reinforced composite paper core comprises a first substrate layer, a second substrate layer and a corrugated paper layer bonded between the first substrate layer and the second substrate layer;

[0018] A plurality of connecting micropores are evenly formed on the surface of the corrugated paper layer, and reinforcing ribs are inserted into the connecting micropores along the length direction of the corrugated paper layer, and the reinforcing ribs are made of PLA material.

[0019] By adopting the above technical scheme, the corrugated paper layer arranged on the first substrate layer and the second substrate layer can significantly improve the toughness and mechanical properties of the composite coated paper through the corrugated structure of the corrugated paper layer and the synergistic effect of the reinforcing ribs and the connecting micropores, reduce the adverse effects of the wrinkle damage of the reinforced composite paper core on its coating layer or the whole, and facilitate the introduction of moisture and degrading microorganisms during degradation.

[0020] Preferably, a degradable adhesive is filled between the crests, troughs and reinforcing ribs of the corrugated paper layer.

[0021] Preferably, the degradable adhesive is preformed cyclodextrin, and the specific preparation steps are as follows:

[0022] First, cyclodextrin, anhydride additives and phosphate are premixed in a weight ratio of 1: (0.008-0.012): (0.01-0.02), and then deionized water is added. After the phosphate is hydrolyzed to a pH of 7.6-8.8, the temperature is raised to 80-120° C. and stirred to obtain prefabricated cyclodextrin.

[0023] By adopting the above technical solution, the degradable adhesive or prefabricated cyclodextrin filled between the crests, troughs and reinforcing ribs of the corrugated paper layer can not only glue the reinforced composite paper core into a hard whole and give it excellent mechanical properties, but also provide the most favorable decomposition environment for microorganisms during the degradation process, including organic matter, nitrogen and phosphorus nutrients, salinity, etc.

[0024] In a second aspect, the present application provides a method for preparing an environmentally friendly composite coated paper, using the following technical solution: A method for preparing an environmentally friendly composite coated paper, comprising the following steps:

[0025] Preparation of reinforced composite paper core;

[0026] Preparation of raw material masterbatch for modified PLA coating layer;

[0027] S1. Place the obtained raw material masterbatch of modified PLA coating layer into a coating machine, and use the coating machine to coat the reinforced composite paper core, with a coating amount of 10-12g / m 2 ;

[0028] S2, drying the reinforced composite paper core after coating, the drying temperature is 25-30° C., the drying time is 1-2 hours, and the environmentally friendly composite coated paper is obtained after drying.

[0029] Preferably, the preparation steps of the reinforced composite paper core are as follows:

[0030] Firstly, reinforcing ribs are correspondingly inserted into the connecting micropores of the corrugated paper layer, and then a degradable adhesive is applied to the joint surfaces of the first substrate layer, the second substrate layer and the corrugated paper layer, and then extrusion is performed to obtain a reinforced composite paper core.

[0031] The environmentally friendly composite coated paper prepared by adopting the above technical solution has uniform and stable performance, excellent mechanical properties, meets the requirements of green environmental protection, and the overall production is relatively simple, easy to industrialize and mass produce, and has extremely high economic and environmental benefits.

[0032] In summary, this application has the following beneficial effects:

[0033] 1. The modified PLA coating layer formed by blending and modifying components such as cyclodextrin, PLA, anhydride additives, coupling agents, phosphates and fillers in this application not only meets the definition of green environmental protection, but also forms a CBM resin-like system under the action of multi-component cross-linking modification, thereby effectively overcoming the defects of the original PLA, such as brittleness and poor toughness, and has extremely high economic and environmental benefits;

[0034] 2. The reinforced composite paper core with a specific structure in the present application can significantly improve the toughness and mechanical properties of the composite coated paper through the corrugated structure of the corrugated paper layer and the synergistic effect of the reinforcing ribs and the connecting micropores, thereby reducing the adverse effects of the reinforced composite paper core on its coated layer or the whole due to the wrinkle damage;

[0035] 3. The degradable adhesive filled between the reinforced composite paper cores in this application can not only give it excellent mechanical properties, but also provide the most favorable decomposition environment for microorganisms during the degradation process, including organic matter, nitrogen and phosphorus nutrition, salinity, etc. required by microorganisms;

[0036] 4. The preparation process in this application is relatively simple in overall production and easy to industrialize and scale up. At the same time, the obtained environmentally friendly composite coated paper has excellent mechanical properties and degradation properties, and has extremely high economic and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is an overall schematic diagram of the environmentally friendly composite coated paper in Examples 1-20 of the present application;

[0038] Figure 2 It is an overall schematic diagram of the environmentally friendly composite coated paper in Examples 21-26 of the present application;

[0039] Figure 3 yes Figure 2 Schematic diagram of the structure of the environmentally friendly composite coated paper with the degradable adhesive partly hidden.

[0040] Reference numerals: 1. reinforced composite paper core; 11. first substrate layer; 12. second substrate layer; 13. corrugated paper layer; 131. connecting micropores; 132. reinforcing ribs; 2. modified PLA coating layer. DETAILED DESCRIPTION

[0041] The following is combined with Figure 1-3 This application is described in further detail.

[0042] Preparation Example

[0043] Preparation Example 1-6

[0044] A raw material masterbatch for a modified PLA coating layer, the raw material components and their corresponding weights are shown in the following table (in kg), and are prepared by the following steps:

[0045] a. Premix cyclodextrin, anhydride additives and phosphate, then add deionized water, wait for the phosphate to be hydrolyzed to pH 7.6, heat to 120°C and stir to obtain prefabricated cyclodextrin;

[0046] The cyclodextrin is β-cyclodextrin; the acid anhydride auxiliary is 2-octenylsuccinic anhydride; the phosphate is composed of sodium hydrogen phosphate and sodium hexametaphosphate in a weight ratio of 1:0.2;

[0047] b. Then the prefabricated cyclodextrin, PLA, coupling agent and filler are dried and blended under vacuum conditions, and finally melt-extruded at 220° C. to obtain the raw material masterbatch of the modified PLA coating layer;

[0048] The coupling agent is titanate coupling agent TMC-201; the filler is corn fiber with a length of 3 mm.

[0049] Table: Components and weights of environmentally friendly composite coated paper in Preparation Examples 1-6 (kg)

[0050]

[0051] Preparation Example 7

[0052] A raw material masterbatch for a modified PLA coating layer, which is different from Preparation Example 1 in that it is prepared by the following steps: a. premixing cyclodextrin, anhydride additives and phosphate, adding deionized water, and heating to 120° C. for stirring after the phosphate is hydrolyzed to a pH of 8.2 to obtain prefabricated cyclodextrin;

[0053] b. Then the prefabricated cyclodextrin, PLA, coupling agent and filler are dried and blended under vacuum conditions, and finally melt-extruded at 220° C. to obtain the raw material masterbatch of the modified PLA coating layer.

[0054] Preparation Example 8

[0055] A raw material masterbatch for a modified PLA coating layer, which is different from Preparation Example 1 in that it is prepared by the following steps: a. premixing cyclodextrin, anhydride additives and phosphate, adding deionized water, and heating to 120° C. for stirring after the phosphate is hydrolyzed to a pH of 8.8 to obtain prefabricated cyclodextrin;

[0056] b. Then the prefabricated cyclodextrin, PLA, coupling agent and filler are dried and blended under vacuum conditions, and finally melt-extruded at 220° C. to obtain the raw material masterbatch of the modified PLA coating layer.

[0057] Preparation Example 9

[0058] A raw material masterbatch for a modified PLA coating layer, which is different from Preparation Example 1 in that it is prepared by the following steps: a. premixing cyclodextrin, anhydride additives and phosphate, adding deionized water, and heating to 100° C. for stirring after the phosphate is hydrolyzed to a pH of 7.6 to obtain prefabricated cyclodextrin;

[0059] b. Then the prefabricated cyclodextrin, PLA, coupling agent and filler are dried and blended under vacuum conditions, and finally melt-extruded at 220° C. to obtain the raw material masterbatch of the modified PLA coating layer.

[0060] Preparation Example 10

[0061] A raw material masterbatch for a modified PLA coating layer, which is different from Preparation Example 1 in that it is prepared by the following steps: a. premixing cyclodextrin, anhydride additives and phosphate, adding deionized water, and heating to 80° C. for stirring after the phosphate is hydrolyzed to a pH of 7.6 to obtain prefabricated cyclodextrin;

[0062] b. Then the prefabricated cyclodextrin, PLA, coupling agent and filler are dried and blended under vacuum conditions, and finally melt-extruded at 220° C. to obtain the raw material masterbatch of the modified PLA coating layer.

[0063] Preparation Example 11

[0064] A raw material masterbatch for a modified PLA coating layer, which differs from Preparation Example 1 in that the anhydride additive is composed of 2-octenyl succinic anhydride, maleic anhydride and dodecenyl succinic anhydride in a weight ratio of 1:0.8:0.6.

[0065] Preparation Example 12

[0066] A raw material masterbatch for a modified PLA coating layer, which differs from Preparation Example 1 in that the anhydride additive is composed of 2-octenyl succinic anhydride, maleic anhydride and dodecenyl succinic anhydride in a weight ratio of 1:1:0.3.

[0067] Preparation Example 13

[0068] A raw material masterbatch for a modified PLA coating layer, which differs from Preparation Example 1 in that the anhydride additive is composed of 2-octenyl succinic anhydride, maleic anhydride and dodecenyl succinic anhydride in a weight ratio of 1:1.1:0.4.

[0069] Preparation Example 14

[0070] A raw material masterbatch for a modified PLA coating layer, which differs from Preparation Example 1 in that the anhydride additive is composed of 2-octenyl succinic anhydride, maleic anhydride and dodecenyl succinic anhydride in a weight ratio of 1:1.2:0.5.

[0071] Preparation Example 15

[0072] A raw material masterbatch for a modified PLA coating layer, which is different from Preparation Example 1 in that the phosphate is composed of sodium hydrogen phosphate and sodium dihydrogen phosphate in a weight ratio of 1:0.3.

[0073] Preparation Example 16

[0074] A raw material masterbatch for a modified PLA coating layer is different from that in Preparation Example 1 in that the phosphate is composed of sodium hydrogen phosphate, sodium dihydrogen phosphate and sodium hexametaphosphate in a weight ratio of 1:0.3:0.2.

[0075] Preparation Example 17

[0076] A raw material masterbatch for a modified PLA coating layer is different from that in Preparation Example 1 in that the phosphate is composed of sodium hydrogen phosphate, sodium dihydrogen phosphate and sodium pyrophosphate in a weight ratio of 1:0.3:0.5.

[0077] Preparation Example 18

[0078] A raw material masterbatch for a modified PLA coating layer, which is different from Preparation Example 1 in that the filler is corn fiber with an average length of 1 mm.

[0079] Preparation Example 19

[0080] A raw material masterbatch for a modified PLA coating layer, which differs from Preparation Example 1 in that the filler is soybean fiber with an average length of 3 mm.

[0081] Preparation Example 20

[0082] A raw material masterbatch of a modified PLA coating layer is different from that of Preparation Example 1 in that the filler is composed of corn fiber with an average length of 1 mm and soybean fiber with an average length of 3 mm in a weight ratio of 1:1.8.

[0083] Preparation Example 21

[0084] A reinforced composite paper core, see Figure 2-3 , comprising a first substrate layer 11 and a second substrate layer 12 with a thickness of 1 mm, and a corrugated paper layer 13 with a thickness of 0.5 mm and a wave height of 3 mm bonded between the first substrate layer 11 and the second substrate layer 12;

[0085] The surface of the corrugated paper layer 13 is uniformly provided with a plurality of connecting micropores 131 along its width direction, the connecting micropores have a pore diameter of 1 mm and a density of 2 / cm, and reinforcing ribs 132 made of PLA with a diameter of 1 mm are inserted into the connecting micropores 131 along the length direction of the corrugated paper layer 13;

[0086] The crests, troughs and reinforcing ribs 132 of the corrugated paper layer 13 are filled with a degradable adhesive, and the degradable adhesive is cyclodextrin;

[0087] And it is prepared by the following preparation steps;

[0088] First, the reinforcing ribs 132 are correspondingly inserted into the connecting micropores 131 of the corrugated paper layer 13, and then a degradable adhesive is applied to the joint surfaces of the first substrate layer 11, the second substrate layer 12 and the corrugated paper layer 13, and then extruded and composited to obtain the reinforced composite paper core 1.

[0089] Preparation Example 22

[0090] A reinforced composite paper core, which is different from Preparation Example 21 in that the opening density of the pore size of the connecting micropores 132 is 5 / cm.

[0091] Preparation Example 23

[0092] A reinforced composite paper core, which is different from Preparation Example 21 in that the hole diameter of the connecting micropores 132 is 2 mm, the opening density is 2 / cm, and the diameter of the reinforcing ribs 132 is 2 mm.

[0093] Preparation Example 24

[0094] A reinforced composite paper core, which is different from Preparation Example 21 in that the degradable adhesive is prefabricated cyclodextrin, and the specific preparation steps are as follows:

[0095] First, cyclodextrin, anhydride additives and phosphate are premixed in a weight ratio of 1:0.006:0.024, and then deionized water is added. After the phosphate is hydrolyzed to a pH of 8.2, the temperature is raised to 120° C. and stirred to obtain prefabricated cyclodextrin.

[0096] Preparation Example 25

[0097] A reinforced composite paper core, which is different from Preparation Example 21 in that the degradable adhesive is prefabricated cyclodextrin, and the specific preparation steps are as follows:

[0098] First, cyclodextrin, anhydride additives and phosphate are premixed in a weight ratio of 1:0.008:0.01, and then deionized water is added. After the phosphate is hydrolyzed to a pH of 8.2, the temperature is raised to 120° C. and stirred to obtain prefabricated cyclodextrin.

[0099] Preparation Example 26

[0100] A reinforced composite paper core, which is different from Preparation Example 21 in that the degradable adhesive is prefabricated cyclodextrin, and the specific preparation steps are as follows:

[0101] First, cyclodextrin, anhydride additives and phosphate are premixed in a weight ratio of 1:0.12:0.02, and then deionized water is added. After the phosphate is hydrolyzed to a pH of 8.2, the temperature is raised to 120° C. and stirred to obtain prefabricated cyclodextrin.

[0102] Performance testing

[0103] The composite coated paper prepared in each embodiment and comparative example was selected as the test object, and three groups of each sample were set in parallel, and then the mechanical properties and degradation properties were tested respectively, and the final test results were averaged and recorded. The specific test steps and test standards are as follows:

[0104] 1) Mechanical properties: The environmentally friendly composite coated paper is characterized by its tensile strength (KN.m) and tear strength (mN). Please refer to GB / T12914-2018 "Determination of tensile strength of paper and paperboard - Constant tension method (20 mm / min)" and GB / T 455-2002 "Determination of tear strength of paper and paperboard";

[0105] 2) Degradation performance: The sample is landfilled in the soil for a degradation test. The specific test steps and test standards refer to GB / T39951-2021 "Evaluation Method for Degradation Performance of Disposable Paper Products". After a fixed number of days of 45d and 90d, the residual weight is recorded and the weight loss rate is calculated.

[0106] Example

[0107] Examples 1-6

[0108] An environmentally friendly composite coated paper, the usage of the raw material masterbatch of the modified PLA coating layer is shown in the following table, and is prepared by the following steps:

[0109] S1. Place the obtained raw material masterbatch of modified PLA coating layer into a coating machine, and use the coating machine to coat the reinforced composite paper core. The coating amount is 10g / m 2 ;

[0110] S2, drying the reinforced composite paper core after coating, the drying temperature is 30° C., the drying time is 2 h, and the environmentally friendly composite coated paper is obtained after drying;

[0111] Among them, the reinforced composite paper core is Figure 1, including a first substrate layer 11 and a second substrate layer 12 with a thickness of 1 mm, and a corrugated paper layer 13 with a thickness of 0.5 mm and a wave height of 3 mm bonded between the first substrate layer 11 and the second substrate layer 12, and the degradable adhesive used for bonding is cyclodextrin.

[0112] Table: Comparison table of usage of raw material masterbatch of modified PLA coating layer in Examples 1-6

[0113] Group Raw material masterbatch for modified PLA coating layer Example 1 Prepared from Preparation Example 1 Example 2 Prepared from Preparation Example 2 Example 3 Prepared from Preparation Example 3 Example 4 Prepared by Preparation Example 4 Example 5 Prepared from Preparation Example 5 Example 6 Prepared from Preparation Example 6

[0114] Comparative Example 1

[0115] A composite coated paper, which is different from Example 1 in that the raw material matrix of the coated layer is prepared from the following raw materials in parts by weight: 150 kg of PLA resin, 0.5 kg of KY1010 antioxidant, and 30 kg of calcium carbonate with a particle size of 0.3 um.

[0116] The composite coated papers prepared in the above Examples 1-6 and Comparative Example 1 were selected, and their mechanical properties and degradation properties were tested according to the above measurement steps and measurement standards. The average values ​​of the test results were recorded in the following table.

[0117] Table: Performance test results of Examples 1-6 and Comparative Example 1

[0118]

[0119]

[0120] As can be seen from the above table, the environmentally friendly composite coated papers prepared in Examples 1-6 all have excellent mechanical properties, with a tensile strength of up to 4.21-4.24 KN.m and a tear strength of up to 462-468 mN, which are 8.5-9.3% and 12.4-13.9% higher than those of Comparative Example 1 using a PLA coating layer, respectively.

[0121] The obtained environmentally friendly composite coated paper also has excellent environmental benefits and degradation ability. Its weight loss rate at 45 days is 41.2-44.2%, and its weight loss rate at 90 days is as high as 91.2-92.5%. The degradation rate is efficient and relatively thorough, which is still improved to varying degrees compared with comparative example 1.

[0122] It can be seen that the prepared modified PLA coating layer meets the definition of green environmental protection. Under the cross-linking modification of cyclodextrin, acid anhydride additives, phosphate and coupling agent, PLA forms a composite system similar to CBM resin, overcoming the original defects of brittleness and poor toughness.

[0123] When the above-mentioned environmentally friendly composite coated paper is discarded or landfilled, its modified PLA coating layer structure will be preferentially degraded, and then cause the destruction of the surface to the internal structure of the reinforced composite paper core, and the degradation rate can reach more than 90% in 3 months, and mainly adopts biodegradation, so it has significant economic and environmental benefits. The specific theoretical basis can be found in Examples 1-6.

[0124] Examples 7-10

[0125] An environmentally friendly composite coated paper, which is different from Example 1 in that the usage of the raw material masterbatch of the modified PLA coating layer is different, as shown in the following table:

[0126] Table: Comparison table of usage of raw material masterbatch of modified PLA coating layer in Examples 7-10

[0127]

[0128]

[0129] Comparative Example 2

[0130] A composite coated paper, which is different from Example 1 in that the raw material masterbatch of the modified PLA coating layer is prepared in the following steps:

[0131] First, cyclodextrin, anhydride additives and phosphates are heated to 120°C and mixed, and then PLA, coupling agent and filler are added in sequence, dried and blended under vacuum conditions, and finally melt-extruded at 220°C to obtain the raw material masterbatch of the modified PLA coating layer.

[0132] The composite coated papers prepared in the above Examples 7-10 and Comparative Example 2 were selected, and their mechanical properties and degradation properties were tested according to the above measurement steps and measurement standards. The average values ​​of the test results were recorded in the following table.

[0133] Table: Performance test results of Examples 7-10 and Comparative Example 2

[0134]

[0135] It can be seen from the above table that the environmentally friendly composite coated paper prepared in Examples 1, 7-10 has excellent mechanical properties, with a tensile strength of up to 4.20-4.22 KN.m and a tear strength of up to 460-465 mN, which are respectively increased by 4.5-5.0% and 6.7-7.9% compared with Comparative Example 2;

[0136] The obtained environmentally friendly composite coated paper also has excellent environmental benefits and degradation ability. Its weight loss rate at 45 days is 42.5-43.6%, and its weight loss rate at 90 days is as high as 90.8-92.2%. The degradation rate is efficient and relatively thorough, which is improved to varying degrees compared with comparative example 2.

[0137] It can be seen that the raw material masterbatch of the modified PLA coating layer prepared by the above specific process has significant environmental benefits. At the same time, its own toughness and brittleness are significantly improved under the cross-linking and bonding effect of the prefabricated cyclodextrin, while the comparative example 2 which is only simply mixed obviously does not achieve the expected effect;

[0138] The reasons may be as follows: the above-mentioned proportion of cyclodextrin, anhydride additives and phosphate, when heated in the alkaline environment produced by the hydrolysis of phosphate, can effectively initiate the grafting reaction of cyclodextrin and anhydride, thereby giving the modified PLA excellent biocompatibility, degradability and inclusion structure in the process of blending the prefabricated cyclodextrin with PLA, coupling agent and filler.

[0139] Examples 11-14

[0140] An environmentally friendly composite coated paper, which is different from Example 1 in that the usage of the raw material masterbatch of the modified PLA coating layer is different, as shown in the following table:

[0141] Table: Comparison table of usage of raw material masterbatch of modified PLA coating layer in Examples 11-14

[0142] Group Raw material masterbatch for modified PLA coating layer Embodiment 11 Prepared from Preparation Example 11 Example 12 Prepared from Preparation Example 12 Example 13 Prepared from Preparation Example 13 Embodiment 14 Prepared from Preparation Example 14

[0143] The composite coated papers prepared in the above Examples 11-14 were selected, and their mechanical properties and degradation properties were tested according to the above measurement steps and measurement standards. The average values ​​of the test results were recorded in the following table.

[0144] Table: Performance test results of Examples 11-14

[0145]

[0146] As can be seen from the above table, the environmentally friendly composite coated papers prepared in Examples 11-14 all have excellent mechanical properties, with a tensile strength of up to 4.22-4.26 KN.m and a tear strength of up to 463-473 mN. It can be seen that the multi-component anhydride additives have a certain compounding effect;

[0147] The obtained environmentally friendly composite coated paper also has excellent environmental benefits and degradation ability. Its weight loss rate at 45 days is 43.1-43.8%, and its weight loss rate at 90 days is as high as 91.5-92.5%. The degradation rate is efficient and relatively thorough, which is further improved compared with Example 1 using only 2-octenyl succinic anhydride.

[0148] Examples 15-17

[0149] An environmentally friendly composite coated paper, which is different from Example 1 in that the usage of the raw material masterbatch of the modified PLA coating layer is different, as shown in the following table:

[0150] Table: Comparison table of usage of raw material masterbatch of modified PLA coating layer in Examples 15-17

[0151] Group Raw material masterbatch for modified PLA coating layer Embodiment 15 Prepared from Preparation Example 15 Example 16 Prepared from Preparation Example 16 Embodiment 17 Prepared from Preparation Example 17

[0152] Comparative Example 3

[0153] A composite coated paper, which is different from Example 1 in that the raw materials for preparing the raw material masterbatch of the modified PLA coating layer do not contain phosphate.

[0154] The composite coated papers prepared in the above Examples 15-17 and Comparative Example 3 were selected, and their mechanical properties and degradation properties were tested according to the above measurement steps and measurement standards. The average values ​​of the test results were recorded in the following table.

[0155] Table: Performance test results of Examples 15-17 and Comparative Example 3

[0156]

[0157] As can be seen from the above table, the environmentally friendly composite coated papers prepared in Examples 1, 15-17 all have excellent mechanical properties, with a tensile strength of up to 4.21-4.23 KN.m and a tear strength of up to 462-465 mN, which are 6.3-6.8% and 9.5-10.2% higher than those of Comparative Example 3 without phosphate, respectively;

[0158] The obtained environmentally friendly composite coated paper also has excellent environmental benefits and degradation ability. Its weight loss rate at 45 days is 42.9-43.2%, and its weight loss rate at 90 days is as high as 91.2-91.8%. The degradation rate is efficient and relatively thorough. Compared with comparative example 3, its degradation rate is further improved.

[0159] In addition, it can be seen from the data of Examples 15-17 that phosphates have a certain compounding effect, but the more types the better. The most preferred is the compounding of sodium hydrogen phosphate and sodium dihydrogen phosphate. The compounding of other phosphates will have a certain impact on the final modification due to the change of their groups.

[0160] Examples 18-20

[0161] An environmentally friendly composite coated paper, which is different from Example 1 in that the usage of the raw material masterbatch of the modified PLA coating layer is different, as shown in the following table:

[0162] Table: Comparison table of usage of raw material masterbatch of modified PLA coating layer in Examples 18-20

[0163] Group Raw material masterbatch for modified PLA coating layer Embodiment 18 Prepared from Preparation Example 18 Embodiment 19 Prepared from Preparation Example 19 Embodiment 20 Prepared from Preparation Example 20

[0164] The composite coated papers prepared in the above Examples 18-20 were selected, and their mechanical properties and degradation properties were tested according to the above measurement steps and measurement standards. The average values ​​of the test results were recorded in the following table.

[0165] Table: Performance test results of Examples 18-20

[0166]

[0167] It can be seen from the above table that the environmentally friendly composite coated paper prepared in Examples 1 and 18-20 has excellent mechanical properties, with a tensile strength of up to 4.21-4.22 KN.m and a tear strength of up to 461-465 mN. The long-diameter soybean fiber and its composite fiber have a better effect on enhancing the mechanical properties.

[0168] The obtained environmentally friendly composite coated paper also has excellent environmental benefits and degradation capabilities. Its 45d weight loss rate is 42.9-43.2%, and its 90d weight loss rate is as high as 91.1-91.2%. The degradation rate is efficient and relatively thorough. The degradation performance of short-diameter corn fiber or its composite fiber is better.

[0169] Examples 21-26

[0170] An environmentally friendly composite coated paper, which is different from Example 1 in that the usage of its reinforced composite paper core is different, as shown in the following table:

[0171] Table: Comparison table of usage of reinforced composite paper core in Examples 21-26

[0172] Group Reinforced composite paper core Embodiment 21 Prepared from Preparation Example 21 Embodiment 22 Prepared from Preparation Example 22 Embodiment 23 Prepared from Preparation Example 23 Embodiment 24 Prepared from Preparation Example 24 Embodiment 25 Prepared from Preparation Example 25 Embodiment 26 Prepared from Preparation Example 26

[0173] The composite coated papers prepared in the above Examples 21-26 were selected, and their mechanical properties and degradation properties were tested according to the above measurement steps and measurement standards. The average values ​​of the test results were recorded in the following table.

[0174] Table: Performance test results of Examples 21-26

[0175]

[0176] It can be seen from the above table that the environmentally friendly composite coated papers prepared in Examples 21-26 all have excellent mechanical properties, with a tensile strength of up to 4.65-4.73 KN.m and a tear strength of up to 488-496 mN, which are respectively increased by 10.5-12.4% and 5.6-7.4% compared with Example 1;

[0177] The obtained environmentally friendly composite coated paper also has excellent environmental benefits and degradation ability. Its weight loss rate at 45 days is 43.6-44.5%, and its weight loss rate at 90 days is as high as 92.1-94.0%. The degradation rate is efficient and relatively thorough, which is improved to varying degrees compared with Example 1.

[0178] It can be seen that the corrugated paper layer arranged on the first substrate layer and the second substrate layer can significantly improve the toughness and mechanical properties of the composite coated paper through the corrugated structure of the corrugated paper layer and the synergistic effect of the reinforcing ribs and the connecting micropores, reduce the adverse effects of the wrinkle damage of the reinforced composite paper core on its coating layer or the whole, and facilitate the introduction of moisture and degrading microorganisms during degradation;

[0179] It can also be seen from Examples 24-26 that the degradable adhesive or preformed cyclodextrin filled between the crests, troughs and reinforcing ribs of the corrugated paper layer can not only glue the reinforced composite paper core into a hard whole and give it excellent mechanical properties, but also provide the most favorable decomposition environment for microorganisms during the degradation process, including organic matter, nitrogen and phosphorus nutrients, salinity, etc.

[0180] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An environmentally friendly composite coated paper, It is characterized in that It comprises a reinforced composite paper core (1) and modified PLA coating layers (2) arranged on both sides of the reinforced composite paper core (1); The raw material masterbatch of the modified PLA coating layer (2) is prepared from the following raw materials in parts by weight: 40-60 parts of cyclodextrin, 100-150 parts of PLA, 0.3-0.5 parts of anhydride additives, 0.1-0.2 parts of coupling agents, 0.5-0.8 parts of phosphates, and 10-30 parts of fillers; The preparation process of the raw material masterbatch of the modified PLA coating layer (2) is as follows: a. Premix cyclodextrin, anhydride additives and phosphate, then add deionized water, wait for the phosphate to be hydrolyzed to a pH of 7.6-8.8, heat to 80-120°C and stir to obtain prefabricated cyclodextrin; b. Then, the prefabricated cyclodextrin, PLA, coupling agent and filler are dried and blended under vacuum conditions, and finally melt-extruded at 180-220° C. to obtain the raw material masterbatch of the modified PLA coating layer (2).

2. The environmentally friendly composite coated paper according to claim 1, It is characterized in that The acid anhydride auxiliary agent is composed of 2-octenyl succinic anhydride, maleic anhydride and dodecenyl succinic anhydride in a weight ratio of 1:(1-1.2):(0.3-0.5).

3. The environmentally friendly composite coated paper according to claim 1, It is characterized in that The phosphate is selected from one or more of sodium hydrogen phosphate, sodium dihydrogen phosphate, sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate.

4. The environmentally friendly composite coated paper according to claim 1, It is characterized in that The filler is 1-3 mm short-cut degradable plant fiber, selected from one or more of straw fiber, rice husk fiber, corn fiber and soybean fiber.

5. The environmentally friendly composite coated paper according to claim 1, It is characterized in that The reinforced composite paper core comprises a first substrate layer (11), a second substrate layer (12), and a corrugated paper layer (13) bonded between the first substrate layer (11) and the second substrate layer (12); A plurality of connecting micropores (131) are evenly formed on the surface of the corrugated paper layer (13), and reinforcing ribs (132) are inserted into the connecting micropores (131) along the length direction of the corrugated paper layer (13), wherein the reinforcing ribs (132) are made of PLA material.

6. The environmentally friendly composite coated paper according to claim 5, It is characterized in that A degradable adhesive is filled between the wave crests, wave troughs and reinforcing ribs (132) of the corrugated paper layer (13).

7. The environmentally friendly composite coated paper according to claim 6, It is characterized in that The degradable adhesive is preformed cyclodextrin, and the specific preparation steps are as follows: First, cyclodextrin, anhydride additives and phosphate are premixed in a weight ratio of 1: (0.008-0.012): (0.01-0.02), and then deionized water is added. After the phosphate is hydrolyzed to a pH of 7.6-8.8, the temperature is raised to 80-120° C. and stirred to obtain prefabricated cyclodextrin.

8. The method for preparing the environmentally friendly composite coated paper according to any one of claims 1 to 7, It is characterized in that The following steps are involved: Preparation of reinforced composite paper core (1); Preparation of raw material masterbatch for modified PLA coating layer (2); S1. Place the obtained raw material masterbatch of the modified PLA coating layer (2) into a coating machine, and use the coating machine to coat the reinforced composite paper core (1) with a coating amount of 10-12 g / m 2 ; S2, drying the reinforced composite paper core (1) after coating, with the drying temperature being 25-30° C. and the drying time being 1-2 h. After drying, the environmentally friendly composite coated paper is obtained.

9. The method for preparing the environmentally friendly composite coated paper according to claim 8, It is characterized in that The steps for preparing the reinforced composite paper core (1) are as follows; First, reinforcing ribs (132) are correspondingly inserted into the connecting micropores (131) of the corrugated paper layer (13), and then a degradable adhesive is applied to the joint surfaces of the first substrate layer (11), the second substrate layer (12) and the corrugated paper layer (13), and then extrusion composite is performed to obtain a reinforced composite paper core (1).