A method for preparing star-shaped block structure polyether and polymer special surfactant

Through the preparation of star block structure polyethers and polymer special surfactants, the problems of poor emulsion uniformity and lack of lasting stability in the papermaking process of mineral oil defoaming agents are solved, and better appearance uniformity and high temperature are achieved Stability extends the stability of the emulsion.

CN116102729BActive Publication Date: 2024-11-26JINING NANTIAN AGRI CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211624655.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-11-26
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

The existing mineral oil defoaming agents have poor emulsion uniformity and lack of stability during papermaking, resulting in limited defoaming and fewer highly efficient special surfactants on the market.

Method used

Using the preparation method of star block structure polyether and polymer special surfactant, the ring-opening polymerization reaction of branched polyhydroxy starting agent and ethylene oxide and propylene oxide is combined with 12-hydroxystearic acid. The esterification reaction of polymers produces star polymer special surfactants with specific molecular weights and structures.

Benefits of technology

It significantly improves the appearance uniformity and high temperature stability of the mineral oil defoamer emulsion, allowing the emulsion to be stable at 55℃ for more than six months, solving the problem of limited stability of the mineral oil defoamer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure BDA0004003677110000011
    Figure BDA0004003677110000011
  • Figure BDA0004003677110000081
    Figure BDA0004003677110000081
Patent Text Reader

Abstract

The invention discloses a method for preparing a star-shaped block structure polyether and a polymer special surfactant, wherein a polyhydroxyl (hydroxyl number ≥ 3) initiator with a star structure is selected and ring-opening polymerization is performed with ethylene oxide (EO for short) and propylene oxide (PO for short) to prepare a five-segment block polyether, and then the block polyether is synthesized with a specific molecular weight 12-hydroxystearic acid self-polymer to prepare a star-shaped polymer special surfactant. The mineral oil defoamer emulsion formula of the polymer special surfactant obtained by the invention has long-lasting stability and uniform appearance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pulp and paper making, and in particular relates to a polymer special surfactant modification technology in a mineral oil defoamer in pulp and paper making. Background Art

[0002] Currently, mineral oil defoamers are widely used in the pulp and papermaking field. However, during the use of mineral oil defoamers, the emulsion may have poor appearance uniformity or short-term stability, resulting in limited defoaming effect in subsequent use and difficulty in achieving better results.

[0003] It has become a consensus in the field of pulp and paper making to add surfactants to mineral oil to improve the uniformity and stability of mineral oil defoamer emulsions. However, the existing surfactants on the market still have problems such as general use effects, difficulty in maintaining the long-term stability of mineral oil emulsions, or high surfactant prices. Therefore, in actual production, there are very few special surfactants that can be effectively used in industrial mineral oils to keep the emulsions more stable. Summary of the invention

[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing a star-shaped block structure polyether and a polymer special surfactant.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solution: a star-shaped block structure polyether having the following chemical structure:

[0006] R-(O-EO m -PO X -EO n -PO y -EO q -H) i or

[0007]

[0008] Wherein, R is the main chain structure of a polyhydroxy initiator having a hydroxyl number ≥ 3, i is the number of hydroxyl groups of the polyhydroxy initiator, E0 is ethylene oxide, P0 is propylene oxide, the degree of polymerization m=n=q, ranging from 1 to 4; the degree of polymerization x=y, ranging from 1 to 4; and (m+n+q)>(x+y);

[0009] Among them, a=b=c=1~3, w=z=2~5, the value is an integer, and (a+b+c)<(w+z).

[0010] As a preferred embodiment, the polyhydroxy initiator is glycerol, pentaerythritol, sorbitan, alkyl glycoside, cyclohexanehexol or triglycerol.

[0011] As a preferred embodiment, the molecular weight of the block structure polyether is in the range of 1200-3200.

[0012] As a preferred embodiment, the molar ratio of the polyhydroxy initiator to EO is 1:9-1:40, and the molar ratio of EO to PO is EO:PO≥3:2.

[0013] The present invention also provides a method for preparing a polymer special surfactant based on the block structure polyether, comprising the following steps:

[0014] Step S1, preparation of star-shaped block polyether: in a reactor, add an appropriate amount of polyhydroxy initiator, solvent and catalyst, stir uniformly at 20-100° C., introduce nitrogen to maintain an oxygen-free environment, and heat the system to 100-140° C., under nitrogen protection, add EO and PO to the system in 5 times for ring-opening polymerization, continue to react for 10-90 minutes after the addition of EO and PO, stop passing nitrogen, cool the system to below 100° C., add an appropriate amount of citric acid to adjust the pH of the system to neutral, and obtain a star-shaped block polyether product;

[0015] Step S2, preparation of 12-hydroxystearic acid self-polymer: 12-hydroxystearic acid and a catalyst are added to a reactor, and stirred and melted at 75-120° C. to form a uniform solution. Under nitrogen protection, the system is heated to 120-150° C., and a self-polymerization reaction occurs for 6-15 hours. The molecular weight range of the self-polymer is controlled according to the acid value of the measurement system. When the molecular weight of the self-polymer reaches the range of 2000-6000, nitrogen is stopped to obtain a brown-yellow opaque liquid of 12-hydroxystearic acid self-polymer;

[0016] Step S3, preparation of polymer special surfactant: in a reactor, add the 12-hydroxystearic acid self-polymer and the catalyst obtained in step S2, and stir and mix to form a uniform solution, heat to 120-150° C. under nitrogen protection, and add the star-shaped block polyether product obtained in step S1, react for 6-15 hours under stirring, and control the molecular weight of the reaction product to be in the range of 7000-39000 according to the acid value of the determination system, stop nitrogen discharge, and cool to obtain a solid product of a star-shaped polymer special surfactant.

[0017] As a preferred solution, steps S2 and S3 use the same catalyst, which is p-toluenesulfonic acid or phosphoric acid, and the amount of the catalyst added is 0.1-2% of the total weight of the reactants.

[0018] As a preferred embodiment, the catalyst in step S1 is KOH or NaOH, and the catalyst addition amount is 0.1-3% of the total weight of the reactants; the solvent is dimethyl sulfoxide, and the addition mass ratio of the polyhydroxy initiator to the solvent is 1:2-1:3.

[0019] As a preferred embodiment, the molar ratio of the star-shaped block polyether product to the 12-hydroxystearic acid self-polymer in step S3 is 1:3-1:20.

[0020] As a preferred embodiment, in step S1, the EO is added to the reaction system three times, and the PO is added to the reaction system twice, and EO and PO are added at alternating intervals.

[0021] As a preferred embodiment, in step S1, the EO is added to the reaction system twice, and the PO is added to the reaction system three times, and EO and PO are added at alternating intervals.

[0022] Beneficial effects: Compared with the prior art, the present invention has the following advantages:

[0023] 1. A polyhydroxyl (hydroxyl number ≥ 3) initiator with a branched (star-shaped) structure was selected, and ethylene oxide (EO) and propylene oxide (PO) were grafted under certain process conditions to carry out a ring-opening polymerization reaction to prepare a (star-shaped) block structure polyether. Compared with a linear hydroxyl-containing initiator, a polyhydroxyl (hydroxyl number ≥ 3) initiator with a branched structure has more grafting sites and can be connected to multiple EO and PO groups as needed to form a five-segment EO / PO segment with ABABA. At the same time, compared with the traditional three-segment ABA EO / PO segment, this type of block polyether structure has better stability and is also conducive to better graft copolymerization with the subsequent acid self-polymer.

[0024] 2. EO has good hydrophilicity and good foaming effect, while PO has relatively poor hydrophilicity. Therefore, in the design of the polyether block of the present invention, the inventor innovatively makes the amount of EO greater than the amount of PO, which plays a key role in the subsequent synthesis of the special surfactant of the star-shaped polymer and in the use of the mineral oil defoamer to make the emulsion have better appearance uniformity and stability. In addition, the inventor also found that the block polyether has better effect, especially when the molecular weight range is 1200-3200.

[0025] 3. By controlling the process conditions, a 12-hydroxystearic acid self-polymer with a specific molecular weight range (2000-6000) was prepared. Compared with directly using low molecular weight 12-hydroxystearic acid to react with the above-mentioned polyether, the self-polymerized 12-hydroxystearic acid (i.e., the self-polymer) itself has a more stable structure, and the macromolecular substance with a specific molecular weight range formed is more conducive to obtaining a star-shaped polymer special surfactant with a lower acid value in the subsequent esterification reaction. At the same time, the self-polymer is helpful for the subsequent synthesis of a polymer special surfactant with a specific molecular weight range.

[0026] 4. The prepared star-shaped block structure polyether with a specific molecular weight range and a designed structure and 12-hydroxystearic acid self-polymer are subjected to an esterification reaction under certain process conditions to synthesize a polymer special surfactant with a specific molecular weight range (7000-39000, acid value 1-10 mgKOH / g). The polymer special surfactant with this specific molecular weight can make the mineral oil defoamer emulsion have better appearance uniformity and high temperature stability when used, and can be stably placed at 55°C for more than 6 months, solving the current problem of limited stability of mineral oil defoamer emulsion. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. After reading the present invention, modifications to various equivalent forms of the present invention by those skilled in the art all fall within the scope defined by the appended claims of the present application.

[0028] Comparison of Chinese and English names of substances:

[0029] Polyoxyethylene fatty acid LAE

[0030] PEG-2 diethylene glycol monolaurate

[0031] The polymer special surfactant of the present invention is used in a mineral oil type defoamer for papermaking, and the synthesis process of the polymer special surfactant mainly includes the following steps:

[0032] 1. Preparation of star-shaped block polyether (C):

[0033] An appropriate amount of a polyhydroxy (hydroxyl number ≥ 3) initiator with a branched (star-shaped) structure, a solvent, and a catalyst are placed in a reactor equipped with a thermometer, a stirring paddle, and a reflux condenser, and stirred uniformly at 20 to 100° C. After the system is repeatedly vacuumed and nitrogen-filled for several times, nitrogen is continuously introduced into the system to maintain an oxygen-free environment, and the system is slowly heated to 100 to 140° C.

[0034] EO and PO should be added in batches for reaction under nitrogen protection. 1 / 3 of the total amount of EO is added for the first time, 1 / 5 of the EO is slowly added first, and the reaction is stirred for 5 to 15 minutes, and then the remaining 4 / 5 of the EO is slowly introduced, and the system continues to carry out ring-opening polymerization for 10 to 45 minutes; 1 / 2 of PO is slowly added, and the reaction continues for 10 to 45 minutes; 1 / 3 of EO is slowly added for the second time, and the reaction continues for 10 to 45 minutes; the remaining 1 / 2 of PO is slowly added, and the reaction continues for 10-45 minutes; the remaining 1 / 3 of EO is slowly added for the third time, and the reaction continues for 10 to 90 minutes; then stop the nitrogen introduction, cool the system below 100°C, add an appropriate amount of citric acid to adjust the system pH to neutral discharge, and obtain star-shaped block polyether C (single segment structure: initiator RO-EOm-POx-EOn-POy-EOq-H).

[0035] In the above process, the branched polyhydroxy (hydroxyl number ≥ 3) initiator can be any one of glycerol, pentaerythritol, anhydrous sorbitol, alkyl glycoside, cyclohexane hexol, triglycerol and other similar structures; the solvent used in the reaction system is dimethyl sulfoxide, and the catalyst is KOH or NaOH, and the most preferred addition amount is 0.1-1.5%. It is important that the molar ratio of the initiator to the total amount of EO is preferably 1:9-1:40, and the molar ratio of the total amount of EO to the total amount of PO should be ≥3:2, that is, EO accounts for at least more than 60%, because EO has good hydrophilicity and good foaming effect, and PO has relatively poor hydrophilicity, so the amount of EO is greater than the amount of PO in the polyether block design, which also plays a key role in the subsequent synthesis of special surfactants of star-shaped polymers and in the use of mineral oil defoamers to make the emulsion have better appearance uniformity and stability.

[0036] Similarly, the above steps can be used to prepare a star-shaped segmented polyether C (the structure of a single hydroxyl-containing segment is: RO-POa-EOw-POb-EOz-POc-H) by changing the addition order to PO, EO, PO, EO and then PO in a certain proportion.

[0037] 2. Preparation of 12-hydroxystearic acid self-polymer (H) with a specific molecular weight range:

[0038] Add appropriate amount of 12-hydroxystearic acid and catalyst to a four-necked flask equipped with a thermometer and a stirring paddle, melt in an oil bath at 75-120°C, stir until the solution is uniform, and introduce nitrogen into the system at the same time. After the air in the system is evacuated and stabilized (take a sample to measure the acid value before the reaction), heat the system to 120-150°C, and react at the specified temperature for 6-15h. During the process, test the acid value of the system at regular intervals (to obtain a self-polymer that meets the molecular weight range requirements), terminate the reaction until it meets the requirements, stop introducing nitrogen, cool and discharge the material, and obtain a brown-yellow impermeable liquid, i.e., 12-hydroxystearic acid self-polymer H.

[0039] 3. Preparation of star polymer specialty surfactant (S)

[0040] Put an appropriate amount of the 12-hydroxystearic acid self-polymer (i.e. H) obtained by the above 2 reactions and a catalyst into a four-mouth reactor equipped with a stirring paddle and a thermometer, and stir at 85°C and 200rpm until the solution is uniform. Nitrogen is introduced into the system, and after the air in the system is evacuated stably, the temperature is raised to 120-150°C; an appropriate amount of block polyether (i.e. C) is introduced into the reactor and stirred until it is uniform; the above materials are reacted at a constant temperature for 6-15h, and the acid value of the system is tested at regular intervals during the process until the reaction is terminated when it meets the requirements, the nitrogen introduction is stopped, and the temperature is lowered to discharge the material. The sample is a block solid at room temperature, i.e., the star polymer special surfactant S.

[0041] Embodiment 1:

[0042] 1. Preparation of star-shaped block polyether:

[0043] 1 mol of anhydrous sorbitol, 330 g of dimethyl sulfoxide, and 0.6% KOH catalyst were placed in a reactor equipped with a thermometer, a stirring blade, and a reflux condenser, and stirred uniformly at 90° C. After the system was repeatedly vacuumed and nitrogen-filled for several times, nitrogen was continuously introduced into the system to maintain an oxygen-free environment, and the system was slowly heated to 110° C.;

[0044] Under nitrogen protection, 26 mol and 17 mol of EO and PO should be added in batches for reaction. 1 / 3 of the total amount of EO is added for the first time, and 1 / 5 of the EO is slowly added first, stirring and reacting for 10 minutes, and then the remaining 4 / 5 of the EO is slowly introduced, and the system continues to carry out ring-opening polymerization for 30 minutes; 1 / 2 of PO is slowly added, and the reaction continues for 30 minutes; 1 / 3 of EO is slowly added for the second time, and the reaction continues for 30 minutes; the remaining 1 / 2 of PO is slowly added, and the reaction continues for 30 minutes; the remaining 1 / 3 of EO is slowly added for the third time, and the reaction continues for 60 minutes; then stop nitrogen introduction, cool the system below 100°C, add appropriate amount of citric acid to adjust the system pH to neutral, and obtain star-shaped block polyether C1 (wherein the EO / PO structure in a single hydroxyl segment: initiator-EO 2 -PO 2 -EO 2 -PO 2 -EO 2 ). After testing: the molecular weight of the star-shaped block polyether C1 obtained in this example is 2193.

[0045] 2. Preparation of 12-hydroxystearic acid self-polymer with specific molecular weight range:

[0046] 300 g of 12-hydroxystearic acid and 0.5% of p-toluenesulfonic acid were added to a four-necked flask equipped with a thermometer and a stirring paddle. After melting in a 90°C oil bath, stirring was started until the solution was uniform. Nitrogen was introduced into the system at the same time. After the air in the system was evacuated stably (sampling was performed to measure the acid value before the reaction), the system was heated to 145°C and subjected to self-polymerization reaction at the specified temperature for 8 hours. During the process, the acid value of the system was tested at regular intervals until the reaction was terminated when it met the requirements. The nitrogen introduction was stopped, the temperature was lowered and the material was discharged to obtain a brown-yellow impermeable liquid, i.e., 12-hydroxystearic acid self-polymer H1, with a measured molecular weight of 3614.

[0047] 3. Preparation of star polymer specialty surfactants

[0048] 10 mol of 12-hydroxystearic acid self-polymer H1 and 0.5% of p-toluenesulfonic acid were added to a four-mouth reactor equipped with a stirring paddle and a thermometer, and stirred at 85°C and 200 rpm until the solution was uniform. Nitrogen was introduced into the system, and after the air in the system was evacuated stably, the temperature was raised to 145°C; 1 mol of the above-mentioned block polyether was added to the reactor and stirred until it was uniform; the above-mentioned materials were reacted at a constant temperature for 12 hours, and the acid value of the system was tested at regular intervals during the process until the reaction was terminated when it met the requirements, the nitrogen introduction was stopped, the temperature was lowered and the material was discharged. The sample was a block solid at room temperature, that is, the star polymer special surfactant S1.

[0049] Embodiment 2:

[0050] 1. Preparation of star-shaped block polyether:

[0051] 1 mol of anhydrous sorbitol, 330 g of dimethyl sulfoxide, and 0.6% KOH catalyst were placed in a reactor equipped with a thermometer, a stirring blade, and a reflux condenser, and stirred uniformly at 90° C. After the system was repeatedly vacuumed and nitrogen-filled for several times, nitrogen was continuously introduced into the system to maintain an oxygen-free environment, and the system was slowly heated to 110° C.;

[0052] Under nitrogen protection, 25 mol of EO and 13 mol of PO should be added in batches for reaction. 1 / 3 of the total amount of PO is added for the first time, and 1 / 5 of the PO is slowly added first, stirring and reacting for 10 minutes, and then the remaining 4 / 5 of the PO is slowly introduced, and the system continues to carry out ring-opening polymerization for 30 minutes; 1 / 2 of EO is slowly added, and the reaction continues for 30 minutes; 1 / 3 of PO is slowly added for the second time, and the reaction continues for 30 minutes; the remaining 1 / 2 of EO is slowly added, and the reaction continues for 30 minutes; the remaining 1 / 3 of PO is slowly added for the third time, and the reaction continues for 60 minutes; then stop the nitrogen introduction, cool the system below 100°C, add an appropriate amount of citric acid to adjust the system pH to neutral, and obtain the star-shaped block polyether C2 (wherein the EO / PO structure in a single hydroxyl segment: initiator-PO 1 -EO3 -PO 1 -EO 3 -PO 1 ). After testing: the molecular weight of the star-shaped block polyether C2 obtained in this example is 1930.

[0053] 2. Preparation of 12-hydroxystearic acid self-polymer with specific molecular weight range:

[0054] In a four-necked flask equipped with a thermometer and a stirring paddle, 300 g of 12-hydroxystearic acid and 0.5% of p-toluenesulfonic acid were added, and after melting in a 90°C oil bath, stirring was started until the solution was uniform. At the same time, nitrogen was introduced into the system. After the air in the system was evacuated stably (sampling was performed to measure the acid value before the reaction), the system was heated to 145°C and subjected to self-polymerization reaction at the specified temperature for 8 hours. During the process, the acid value of the system was tested at regular intervals until the reaction was terminated when it met the requirements. The nitrogen introduction was stopped, the temperature was lowered and the material was discharged to obtain a brown-yellow impermeable liquid, i.e., 12-hydroxystearic acid self-polymer H2, with a measured molecular weight of 3614.

[0055] 3. Preparation of star polymer specialty surfactants

[0056] 10 mol of 12-hydroxystearic acid self-polymer H1 and 0.5% of p-toluenesulfonic acid were added to a four-mouth reactor equipped with a stirring paddle and a thermometer, and stirred at 85°C and 200 rpm until the solution was uniform. Nitrogen was introduced into the system, and after the air in the system was evacuated steadily, the temperature was raised to 145°C; 1 mol of the above-mentioned block polyether was added to the reactor and stirred until it was uniform; the above-mentioned materials were reacted at a constant temperature for 12 hours, and the acid value of the system was tested at regular intervals during the process until the reaction was terminated when it met the requirements, the nitrogen introduction was stopped, the temperature was lowered and the material was discharged. The sample was a block solid at room temperature, that is, the star polymer special surfactant S2.

[0057] Embodiment 3-15:

[0058] In Examples 3-15, the preparation process of the (star-shaped) polymer specialty surfactant is different from that of Example 1 in that the initiator, the addition ratio and batch order of ethylene oxide EO and propylene oxide PO, the molecular weight of the block polyether, or the molecular weight of the 12-hydroxystearic acid self-polymer are different, and the rest of the contents are the same. In each embodiment, each reactant and the addition amount are shown in Table 1, and the basic product indicators of the obtained surfactant product are shown in Tables 2 and 3.

[0059] Table 1: Amount of reactants added and reaction time in each example

[0060]

[0061] Table 2: Block polyether structures and molecular weights obtained in each example

[0062]

[0063] Table 3 shows the product indicators of special surfactants obtained in various examples

[0064]

[0065]

[0066] The special surfactant S prepared in Examples 1-15 was used to prepare a mineral oil emulsion according to the following method: appropriate amounts of 15# white oil, hydrophobic silica, D10, special surfactant S and water were added in sequence to a four-necked flask equipped with a thermometer and a stirring paddle, and the mixture was emulsified and stirred at 80-150°C for 10-90 minutes to obtain a mineral oil emulsion M, and the stability of the mineral oil emulsion was evaluated. The formula of each component in the mineral oil emulsion is as follows:

[0067]

[0068] Then, the performance of the mineral oil emulsion was tested, as shown in Table 4:

[0069] Table 4: Properties and product indicators of mineral oil emulsions prepared in various examples

[0070]

[0071] Performance characterization:

[0072] The characteristic surfactant products obtained in each embodiment were subjected to performance characterization tests, and the characterization test methods are as follows:

[0073] (1) Characterization of synthetic special surfactants

[0074] Appearance: Observe and record the appearance of the samples with naked eyes at room temperature.

[0075] Acid value test method: refer to Appendix A of "Food Additive Polyglycerol Fatty Acid Esters", prepare equal volumes of isopropanol and toluene mixed solvent, 1% phenolphthalein isopropanol solution, 0.1mol / L potassium hydroxide standard titration solution; take 50mL of isopropanol-toluene solvent in a conical flask, and add 2mL of 1% phenolphthalein isopropanol solution; titrate with 0.1mol / L potassium hydroxide standard solution until the solution turns light pink, accurately weigh 0.3-0.5g of the sample, record it as W, dissolve it in the mixed solvent, heat it if necessary, shake it vigorously, and titrate it with 0.1mol / L potassium hydroxide standard solution. The solution turns pink, which is the end point. Record the volume of potassium hydroxide standard solution consumed during titration, record it as V. The acid value X1 calculation formula is:

[0076]

[0077] Esterification rate test method: Calculate the esterification rate according to the change in the acid value of the system before and after the reaction. The calculation formula is as follows:

[0078] Esterification rate = (acid value of the system before reaction - acid value of the system after reaction) / acid value of the system before reaction × 100% Molecular weight test method: Agilent 1260 GPC was used to test the molecular weight of the sample.

[0079] (2) Characterization of the application performance of surfactants in mineral oil emulsions

[0080] Stability test: Take an appropriate amount of the prepared mineral oil emulsion and use the Landiscan TOWER stabilizer to test the stability of the mineral oil emulsion at a high temperature of 55°C.

[0081] It can be seen from the above embodiments and comparative examples that the star-shaped five-segment block polyether C with a specific molecular weight synthesized from an initiator with a branched structure (number of hydroxyl groups ≥ 3) and EO and PO, and the 12-hydroxystearic acid self-polymer H with a specific molecular weight can help to generate a special surfactant S with a certain molecular weight; compared with other linear structure initiators, 12-hydroxystearic acid self-polymers with molecular weights not within the range, and a single surfactant, the above-mentioned special surfactant S that meets the requirements has a more uniform appearance and more lasting high temperature stability in the mineral oil emulsion.

Claims

1. A star-shaped block structure polyether, characterized in that It has the following chemical structure: or , Wherein, R is the main chain structure of a polyhydroxy initiator having a hydroxyl number ≥ 3, i is the number of hydroxyl groups of the polyhydroxy initiator, EO is ethylene oxide, PO is propylene oxide, the degree of polymerization m=n=q, ranging from 1 to 4; the degree of polymerization x=y, ranging from 1 to 4; and (m+n+q)>(x+y); Wherein, a=b=c=1-3, w=z=2-5, the values ​​are integers, and (a+b+c)<(w+z); the molecular weight range of the block structure polyether is 1200-3200.

2. The star-shaped block structure polyether according to claim 1, characterized in that: The polyhydroxy initiator is glycerol, pentaerythritol, sorbitan, alkyl glycoside, cyclohexanehexol or triglycerol.

3. The star-shaped block structure polyether according to claim 1, characterized in that: The molar ratio of the polyhydroxy initiator to EO is 1:9-1:40, and the molar ratio of EO to PO is EO:PO≥3:

2.

4. A method for preparing a polymer special surfactant based on any one of the block structure polyethers according to claims 1 to 3, characterized in that The following steps are involved: Step S1, preparation of star-shaped block polyether: in a reactor, add an appropriate amount of polyhydroxy initiator, solvent and catalyst, stir uniformly at 20-100° C., introduce nitrogen to maintain an oxygen-free environment, and heat the system to 100-140° C., under nitrogen protection, add EO and PO to the system in 5 times for ring-opening polymerization, continue to react for 10-90 minutes after the addition of EO and PO, stop passing nitrogen, cool the system to below 100° C., add an appropriate amount of citric acid to adjust the pH of the system to neutral, and obtain a star-shaped block polyether product; Step S2, preparation of 12-hydroxystearic acid self-polymer: 12-hydroxystearic acid and a catalyst are added to a reactor, and stirred and melted at 75-120° C. to form a uniform solution, and the system is heated to 120-150° C. under nitrogen protection, and a self-polymerization reaction occurs for 6-15 hours, and the molecular weight range of the self-polymer is controlled according to the acid value of the measurement system. When the molecular weight of the self-polymer reaches the range of 2000-6000, nitrogen is stopped to obtain a brown-yellow opaque liquid of 12-hydroxystearic acid self-polymer; Step S3, preparation of polymer special surfactant: in a reactor, add the 12-hydroxystearic acid self-polymer and the catalyst obtained in step S2, and stir and mix to form a uniform solution, heat to 120-150° C. under nitrogen protection, and add the star-shaped block polyether product obtained in step S1, react for 6-15 hours under stirring, and control the molecular weight of the reaction product to be in the range of 7000-39000 according to the acid value of the determination system, stop nitrogen discharge, and cool to obtain a solid product of a star-shaped polymer special surfactant.

5. The method for preparing the polymer special surfactant of the block structure polyether according to claim 4, characterized in that: Steps S2 and S3 use the same catalyst, which is p-toluenesulfonic acid or phosphoric acid, and the amount of the catalyst added is 0.1-2% of the total weight of the reactants.

6. The method for preparing the polymer special surfactant of the block structure polyether according to claim 4, characterized in that: In step S1, the catalyst is KOH or NaOH, and the amount of catalyst added is 0.1-3% of the total weight of the reactants; the solvent is dimethyl sulfoxide, and the mass ratio of the polyhydroxy initiator to the solvent is 1:2-1:

3.

7. The method for preparing the polymer special surfactant of the block structure polyether according to claim 4, characterized in that: The molar ratio of the star-shaped block polyether product to the 12-hydroxystearic acid self-polymer in step S3 is 1:3-1:

20.

8. The method for preparing the polymer special surfactant of the block structure polyether according to claim 4, characterized in that: In step S1, the EO is added to the reaction system three times, and the PO is added to the reaction system twice, and EO and PO are added alternately.

9. The method for preparing the polymer special surfactant of block structure polyether according to claim 4, characterized in that: In step S1, the EO is added to the reaction system twice, and the PO is added to the reaction system three times, and EO and PO are added alternately.